Visible-light-responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material and preparation method thereof
By combining Bi2MoO6 and g-C3N4 on the kaolin support, Bi2MoO6/g-C3N4/kaolin composite photocatalytic material is formed, which solves the problem of low activity of existing photocatalytic materials under visible light, and achieves efficient pollutant degradation. It is suitable for Water and air purification, simple process and low cost.
Patent Information
- Application Number
- CN202410922548.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
AI Technical Summary
The existing photocatalytic materials have low photocatalytic activity under visible light, and the preparation process is cumbersome and costly, with a narrow application range, making it difficult to effectively degrade organic pollutants in water and air.
Using kaolin as a support, melamine, Bi(NO3)3·5H2O, Na2MoO4·2H2O as precursors, combined with solid-phase sintering method and solvent-thermal method, Bi2MoO6/g-C3N4/kaolin composite photocatalytic material was prepared, and Bi2MoO6 was modified using Bi2MoO6. g-C3N4/kaolin composite material forms heterostructures to improve photocatalytic properties.
It significantly improves the specific surface area and reactive sites of the composite material, enhances the photocatalytic degradation performance of visible light, reduces the preparation cost and operational complexity, and is suitable for wastewater treatment and air purification.
Smart Images

Figure CN118892856A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of non-metallic mineral materials and environmental engineering, and in particular to a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material and a preparation method thereof. Background Art
[0002] With the advancement of the national "dual carbon" strategy, new requirements have been put forward for the green transformation of building materials, water pollution control and air purification. At present, the main methods for water pollution control are physical adsorption, chemical method, biological method and photocatalysis. The physical adsorption method is simple to operate, efficient and low in cost, but the adsorption materials are often saturated and selective, and cannot completely eliminate pollutants, and may also cause secondary pollution. The chemical method has high treatment cost and treatment efficiency, but it is easy to react with other substances to produce secondary pollution. The biological method has high requirements for environmental conditions and experimental equipment, and the treatment time is long. In contrast, the photocatalytic method is simple to operate, has high degradation efficiency, and will not produce secondary pollution when treating organic pollutants, thus meeting the needs of green and efficient technology development. With the in-depth research in the field of photocatalysis, the degradation of organic pollutants under visible light has become a research focus. Under sunlight irradiation, the synthesized g-C3N4 / kaolin binary composite material showed a good degradation effect on organic pollutants, but the photocatalytic activity in the visible light range was still very low. As a narrow-gap semiconductor material, Bi2MoO6 has the characteristics of large specific surface area, non-toxicity, chemical stability, low price and adjustable electronic structure. It is a visible light responsive photocatalyst with good application prospects. However, due to its weak built-in electric field and high recombination rate of electron-hole pairs, the photocatalytic activity of Bi2MoO6 is severely limited.
[0003] The patent application with application number 202010533764.2 discloses a g-C3N4-Bi2WO6 heterojunction photocatalytic hydrogen production material and its preparation method. Although a Z-type heterojunction is formed in the composite photocatalyst to achieve high-efficiency photocatalytic hydrogen production performance, the preparation process is cumbersome and the production cost is high. The catalyst only responds under simulated sunlight and has a narrow range of application. Summary of the invention
[0004] In order to solve the above problems, the present invention proposes a method of synthesizing a g-C3N4 / kaolin composite material using kaolin as a carrier and melamine as a precursor, and constructing a heterostructure by adding a bismuth-based narrow bandgap semiconductor Bi2MoO6, thereby modifying the g-C3N4 / kaolin composite material to prepare a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material;
[0005] The technical solution of the present invention is: a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material, wherein the composite photocatalytic material is a kaolin sheet layer surface loaded with nano g-C3N4 and Bi2MoO6 particles, the average particle size of the Bi2MoO6 particles is 1-1.5μm, the nano g-C3N4 is a nano sheet, the average size of the nano g-C3N4 is 2-5um, the mass ratio of kaolin to Bi2MoO6 in the composite photocatalytic material is 0.4-1.2:1, and the mass ratio of kaolin to nano g-C3N4 is 3:1.5-2.
[0006] Furthermore, the kaolin is intercalated-exfoliated kaolin,
[0007] The preparation method of the intercalation-stripping kaolin is:
[0008] Step A: 3-5 g of kaolin and 3-5 g of urea are mixed, 30-50 mL of deionized water is added, and centrifugation is performed at 40-60° C. and a speed of 10000-13000 rpm for 10-15 min to form a suspension;
[0009] Step B: The suspension obtained in step A is filtered, washed, and then dried at 80° C. to obtain a white product;
[0010] Step C: add 20-40 mL of deionized water to the white product obtained in step B, and perform ultrasonic treatment at 50-70° C. for 6-10 min. During the ultrasonic treatment, blow nitrogen into the mixed solution for 5-6 min to obtain a mixed solution;
[0011] Step D: filtering and washing the mixed solution obtained in step C, and then drying it at 80° C. to obtain intercalation-stripping kaolin;
[0012] Description: Preparing kaolin into intercalation-stripping kaolin can be more conducive to the loading of Bi2MoO6 / g-C3N4, thereby improving the composite photocatalytic effect of the product; under the action of ultrasound, the surface of the intercalation-stripping kaolin becomes more active, and under the synergistic effect of nitrogen blowing, more pores can be woven in the intercalation-stripping kaolin, and the surface has more loading points, which is beneficial to the subsequent loading of Bi2MoO6 particles and g-C3N4, thereby increasing the loading amount of the intercalation-stripping kaolin and enhancing the overall performance of the composite material.
[0013] Furthermore, the ultrasonic frequency in step C is 30-50 KHz, and the ultrasonic power density is 0.2-0.25 W / cm 2 ;
[0014] Note: Too high ultrasonic frequency and power density will shatter the product into pieces, which is not conducive to the loading of the catalyst.
[0015] A method for preparing a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material, using kaolin as a carrier, melamine, Bi(NO3)3·5H2O and Na2MoO4·2H2O as precursors, and loading nano g-C3N4 and Bi2MoO6 on the surface of kaolin sheets by solid phase sintering and solvothermal method, comprising the following steps:
[0016] S1. Mix kaolin flakes and melamine in a mass ratio of 3:4 and grind in a mortar for 30 to 60 minutes;
[0017] S2, calcining the mixture obtained in step S1 at a heating rate of 2.5-5°C / min, and keeping the temperature at 525-575°C for 3.9-4.1h, and grinding the obtained product after the end of the heat preservation to obtain a kaolin-loaded g-C3N4 composite photocatalytic material;
[0018] S3, dissolve 0.8-1.0 g Bi(NO3)3·5H2O and 0.23-0.25 g Na2MoO4·2H2O respectively in 10-20 mL ethylene glycol, and stir to form solution A and solution B;
[0019] S4, then add 30-60 mL of anhydrous ethanol to solution A, and continue stirring for 20-40 min to obtain solution C, then take 0.3-0.9 g of kaolin-loaded g-C3N4 composite photocatalytic material in step S2 and add it to solution C, continue stirring for 20-40 min to obtain solution D, and finally add solution B to solution D, and stir for 20-40 min to mix;
[0020] S5, transferring the suspension obtained in step S4 to a high pressure reactor, maintaining the reaction temperature at 150-180° C. for 6-12 hours;
[0021] S6, filtering the product obtained in step S5 and washing it with deionized water and anhydrous ethanol for 2 to 4 times respectively, drying the obtained product in an oven at 55 to 65° C. for 10 to 12 hours, and grinding to obtain the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material;
[0022] Description: The present invention uses kaolin as a carrier to solve the agglomeration problem of pure g-C3N4 and improve the adsorption capacity and photocatalytic performance of the composite material; then Bi2MoO6 is used to modify the g-C3N4 / kaolin composite material, which further improves the specific surface area of the nanocomposite material and increases a large number of reaction active sites, which is beneficial to the efficient photocatalytic reaction.
[0023] Further, in step S4, the amount of kaolin-loaded g-C3N4 composite photocatalytic material added is 0.5 g;
[0024] Note: The photocatalytic performance of the product under the above addition amount is better.
[0025] Further, in step S6, the Bi2MoO6 / g-C3N4 / kaolin composite material is ground to a specific surface area of 37 to 49 m 2 / g, pore size distribution is in the range of 2 to 20 nm;
[0026] Note: The photocatalytic material has better performance under the above parameters.
[0027] Furthermore, in step S4, solution C is subjected to mineralization treatment.
[0028] The mineralization treatment method comprises: preparing a reducing mineralizer according to a mass ratio of solution C to reducing mineralizer of 1:0.5-0.8, then dropping the reducing mineralizer dropwise into a reactor containing solution C, stirring continuously for 20-40 minutes during the dropping process, generating product A, washing the surface of product A with deionized water, air, and carbon dioxide for 4-6 times respectively, finally sealing the reactor and placing it in a microwave hydrothermal reactor for reaction for 25-30 minutes, and obtaining a mineralized solution C; wherein the temperature of the microwave hydrothermal reactor is set to 230-250° C., and the power is set to 100-150W;
[0029] Description: After the bismuth nitrate solution is subjected to mineralization treatment and then reacted with sodium molybdate, the bismuth oxide generated after the mineralization treatment has higher chemical stability, which can help it to react better with sodium molybdate and then be firmly loaded on the surface of kaolin. At the same time, on the surface of kaolin with carbon nitride, the stable loading state can reduce the loss of catalyst during the reaction process, thereby improving the catalytic efficiency and the life of the catalyst. In particular, after the mineralization treatment, there is still a trace amount of δ-Bi2O3, which has a cubic fluorite ore structure, and some oxygen ion positions are vacant in its lattice, so it has very high oxygen ion conductivity. And from the perspective of chemical bonding, hydrogen bonds or other types of chemical bonding may be formed between the oxygen ions of δ-Bi2O3 in the bismuth nitrate solution after the mineralization treatment and the hydroxyl or oxygen-containing groups in the kaolin, thereby enhancing the loading effect of bismuth ions.
[0030] Furthermore, the reducing mineralizer comprises, by mass percentage, 40-45% of sodium hydroxide, 5-10% of ammonium chloride, 5-7% of sodium polyacrylate and the balance of water;
[0031] Description: Sodium polyacrylate can improve the dispersibility of kaolin, thus facilitating the loading of bismuth molybdate and carbon nitride on the surface of kaolin; the addition of ammonium chloride can expand kaolin, and when applied to molybdate solution, it can improve the conductivity of the solution, which helps the extraction efficiency of molybdenum, thereby promoting the formation of bismuth molybdate to further improve the loading effect; in addition, ammonium chloride itself can also be used as a chemical bulking agent, which can produce gas through thermal decomposition to achieve the expansion effect of the material, thereby expanding kaolin and further promoting the loading effect of bismuth molybdate and carbon nitride on the surface of kaolin.
[0032] Further, the filling ratio of the microwave hydrothermal reactor is controlled to be 55-65%;
[0033] Note: At the above filling degree, the reactor has good mixing effect and heat transfer performance, and the reaction pressure is relatively low, which helps to maintain the safety and stability of the reaction.
[0034] The beneficial effects of the present invention are:
[0035] (1) The material of the present invention utilizes the visible light response and excellent specific surface area characteristics of Bi2MoO6, and modifies the g-C3N4 / kaolin composite material to increase the specific surface area of the Bi2MoO6 / g-C3N4 / kaolin composite material, so that the composite material has a strong visible light photocatalytic degradation performance for pollutants, thereby solving the problems of high electron-hole pair recombination rate and low photocatalytic degradation ability of the g-C3N4 / kaolin composite material under visible light.
[0036] (2) The present invention uses kaolin as a carrier to solve the agglomeration problem of pure g-C3N4 and improve the adsorption capacity and photocatalytic performance of the composite material; then Bi2MoO6 is used to modify the g-C3N4 / kaolin composite material, which further improves the specific surface area of the nanocomposite material and increases a large number of reaction active sites, which is conducive to the efficient photocatalytic reaction; and the required raw materials are low in price, the preparation process is simple, and the reaction conditions are mild, which has great application value in the fields of wastewater treatment and air purification.
[0037] (3) The present invention performs a mineralization treatment on the bismuth nitrate solution before reacting it with sodium molybdate, which helps it to react better with sodium molybdate and then be firmly loaded on the surface of kaolin. At the same time, on the surface of kaolin with carbon nitride, the stable loading state can reduce the loss of the catalyst during the reaction, thereby improving the catalytic efficiency and the life of the catalyst. The bismuth nitrate solution after the mineralization treatment has δ-Bi2O3 with a cubic fluorite ore structure, and some oxygen ion positions are vacant in its lattice, so it has very high oxygen ion conductivity. This structure can promote its interaction with oxygen-containing groups on the surface of kaolin. From the perspective of chemical bonding, the oxygen ions in the trace δ-Bi2O3 in the bismuth nitrate solution after the mineralization treatment can also form hydrogen bonds or other types of chemical bonds with hydroxyl groups or oxygen-containing groups in kaolin, thereby enhancing the loading effect of bismuth. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 XRD patterns of kaolin, g-C3N4, Bi2MoO6, g-C3N4 / kaolin, Bi2MoO6 / kaolin, Bi2MoO6 / g-C3N4 and Bi2MoO6 / g-C3N4 / kaolin in different mass ratios in the present invention;
[0039] Figure 2 SEM images of kaolin, intercalation-exfoliation kaolin, g-C3N4, Bi2MoO6, g-C3N4 / kaolin and Bi2MoO6 / g-C3N4 / kaolin in the present invention;
[0040] Figure 3 TEM images of g-C3N4 / kaolin and Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic materials;
[0041] Figure 4 The N2 adsorption-desorption isotherms and pore size distribution diagrams of kaolin, g-C3N4, Bi2MoO6, and Bi2MoO6 / g-C3N4 / kaolin in the present invention;
[0042] Figure 5 These are the PL spectra of g-C3N4, Bi2MoO6, and Bi2MoO6 / g-C3N4 / kaolin in the present invention. DETAILED DESCRIPTION
[0043] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.
[0044] Embodiment 1: A visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material, wherein the composite photocatalytic material is a kaolin sheet layer with nano g-C3N4 and Bi2MoO6 particles loaded on the surface, wherein the average particle size of the Bi2MoO6 particles is 1.3 μm, the nano g-C3N4 is a nano sheet, and the average size of the nano g-C3N4 is 3.5 μm. In the composite photocatalytic material, the mass ratio of kaolin to Bi2MoO6 is 0.8:1, and the mass ratio of kaolin to nano g-C3N4 is 3:1.8;
[0045] Kaolin is intercalated-stripped kaolin,
[0046] The preparation method of intercalation-stripping kaolin is:
[0047] Step A: 4 g of kaolin and 4 g of urea were mixed, 40 mL of deionized water was added, and the mixture was centrifuged and stirred at 50° C. and 11500 rpm for 13 min to form a suspension;
[0048] Step B: The suspension obtained in step A is filtered, washed, and then dried at 80° C. to obtain a white product;
[0049] Step C: add 30 mL of deionized water to the white product obtained in step B, and perform ultrasonic treatment at 60° C. for 8 min. During the ultrasonic treatment, blow nitrogen into the mixed solution for 5 min to obtain a mixed solution;
[0050] Step D: The mixed solution obtained in step C is filtered, washed, and then dried at 80° C. to obtain intercalation-stripping kaolin.
[0051] The ultrasonic frequency in step C is 40KHz and the ultrasonic power density is 0.23W / cm 2 ;
[0052] A method for preparing a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material, using kaolin as a carrier, melamine, Bi(NO3)3·5H2O and Na2MoO4·2H2O as precursors, and loading nano g-C3N4 and Bi2MoO6 on the surface of kaolin sheets by solid phase sintering and solvothermal method, comprising the following steps:
[0053] S1. Mix kaolin flakes and melamine in a mass ratio of 3:4 and grind in a mortar for 45 minutes;
[0054] S2, calcining the mixture obtained in step S1 at a heating rate of 3.5°C / min, and keeping the temperature at 550°C for 4 hours. After the temperature is kept, grinding the obtained product to obtain a kaolin-loaded g-C3N4 composite photocatalytic material;
[0055] S3, dissolve 0.9 g Bi(NO3)3·5H2O and 0.24 g Na2MoO4·2H2O in 15 mL ethylene glycol respectively, and stir to form solution A and solution B;
[0056] S4, then add 40mL of anhydrous ethanol to solution A, and continue stirring for 30min to obtain solution C, then take 0.6g of kaolin-loaded g-C3N4 composite photocatalytic material in step S2 and add it to solution C, continue stirring for 30min to obtain solution D, and finally add solution B to solution D, stir for 30min to mix; the amount of kaolin-loaded g-C3N4 composite photocatalytic material added is 0.5g;
[0057] S5, transferring the suspension obtained in step S4 to a high pressure reactor, and maintaining the reaction at 160° C. for 8 h;
[0058] S6. The product obtained in step S5 is filtered and washed three times with deionized water and anhydrous ethanol respectively, and the obtained product is dried in an oven at 60° C. for 12 h, and the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material is obtained after grinding; wherein the specific surface area of the Bi2MoO6 / g-C3N4 / kaolin composite material after grinding is 43 m 2 / g, pore size distribution is in the range of 9-17nm;
[0059] In step S4, solution C is subjected to mineralization treatment.
[0060] The mineralization treatment method is as follows: prepare a reducing mineralizer according to a mass ratio of solution C to reducing mineralizer of 1:0.7, then drop the reducing mineralizer into a reactor containing solution C, continuously stir for 30 minutes during the dropping process, generate product A, wash it with deionized water, air, and carbon dioxide for 5 times respectively, finally seal the reactor and place it in a microwave hydrothermal reactor for reaction for 28 minutes, and obtain the mineralized solution C; wherein, the temperature of the microwave hydrothermal reactor is set to 240°C and the power is set to 125W; the filling ratio of the microwave hydrothermal reactor is controlled to be 60%; wherein, the microwave hydrothermal reactor is an existing product;
[0061] The reducing mineralizer comprises, by weight percentage, 43% of sodium hydroxide, 8% of ammonium chloride, 6% of sodium polyacrylate and the balance of water.
[0062] Example 2: Different from Example 1, the preparation method of intercalation-stripping kaolin is:
[0063] Step A: 3 g of kaolin and 3 g of urea were mixed, 30 mL of deionized water was added, and the mixture was centrifuged and stirred at 10000 rpm for 10 min at 40° C. to form a suspension;
[0064] Step B: The suspension obtained in step A is filtered, washed, and then dried at 80° C. to obtain a white product;
[0065] Step C: add 20 mL of deionized water to the white product obtained in step B, and perform ultrasonic treatment at 50° C. for 10 min. During the ultrasonic treatment, blow nitrogen into the mixed solution for 5 min to obtain a mixed solution;
[0066] Step D: The mixed solution obtained in step C is filtered, washed, and then dried at 80° C. to obtain intercalation-stripping kaolin.
[0067] The ultrasonic frequency in step C is 30KHz and the ultrasonic power density is 0.2W / cm 2 .
[0068] Example 3: Different from Example 1, the preparation method of intercalation-stripping kaolin is:
[0069] Step A: 5 g of kaolin and 5 g of urea were mixed, 50 mL of deionized water was added, and the mixture was centrifuged and stirred at 60° C. and 13,000 rpm for 15 min to form a suspension;
[0070] Step B: The suspension obtained in step A is filtered, washed, and then dried at 80° C. to obtain a white product;
[0071] Step C: add 40 mL of deionized water to the white product obtained in step B, and perform ultrasonic treatment at 70° C. for 6 min. During the ultrasonic treatment, blow nitrogen into the mixed solution for 6 min to obtain a mixed solution;
[0072] Step D: The mixed solution obtained in step C is filtered, washed, and then dried at 80° C. to obtain intercalation-stripping kaolin.
[0073] The ultrasonic frequency in step C is 50KHz and the ultrasonic power density is 0.25W / cm 2 .
[0074] Embodiment 4: Different from Embodiment 1,
[0075] S1. Mix kaolin flakes and melamine in a mass ratio of 3:4 and grind in a mortar for 30 minutes;
[0076] S2, calcining the mixture obtained in step S1 at a heating rate of 2.5°C / min, and keeping the temperature at 550°C for 4.1h. After the temperature is kept, grinding the obtained product to obtain a kaolin-loaded g-C3N4 composite photocatalytic material;
[0077] S3, dissolve 0.8g Bi(NO3)3·5H2O and 0.23g Na2MoO4·2H2O in 10mL ethylene glycol respectively, and stir to form solution A and solution B;
[0078] S4, then add 30mL of anhydrous ethanol to solution A, and continue stirring for 20min to obtain solution C, then take 0.3g of kaolin-loaded g-C3N4 composite photocatalytic material in step S2 and add it to solution C, continue stirring for 20min to obtain solution D, and finally add solution B to solution D, stir for 20min to mix; the amount of kaolin-loaded g-C3N4 composite photocatalytic material added is 0.3g;
[0079] S5, transferring the suspension obtained in step S4 to a high pressure reactor, and maintaining the reaction at 150° C. for 6 hours;
[0080] S6. The product obtained in step S5 is filtered and washed twice with deionized water and anhydrous ethanol respectively, and the obtained product is dried in an oven at 60° C. for 12 h, and the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material is obtained after grinding; wherein the specific surface area of the Bi2MoO6 / g-C3N4 / kaolin composite material after grinding is 37 m 2 / g, and the pore size distribution is in the range of 2-8nm.
[0081] Embodiment 5: Different from Embodiment 1,
[0082] S1. Mix kaolin flakes and melamine in a mass ratio of 3:4 and grind in a mortar for 60 minutes;
[0083] S2, calcining the mixture obtained in step S1 at a heating rate of 5°C / min, and keeping the temperature at 550°C for 4 hours. After the temperature is kept, grinding the obtained product to obtain a kaolin-loaded g-C3N4 composite photocatalytic material;
[0084] S3, dissolve 1.0 g Bi(NO3)3·5H2O and 0.25 g Na2MoO4·2H2O in 20 mL ethylene glycol respectively, and stir to form solution A and solution B;
[0085] S4, then add 50mL of anhydrous ethanol to solution A, and continue stirring for 40min to obtain solution C, then take 0.9g of kaolin-loaded g-C3N4 composite photocatalytic material in step S2 and add it to solution C, continue stirring for 40min to obtain solution D, and finally add solution B to solution D, stir for 40min to mix; the amount of kaolin-loaded g-C3N4 composite photocatalytic material added is 0.7g;
[0086] S5, transferring the suspension obtained in step S4 to a high pressure reactor, and maintaining the reaction at 170° C. for 10 h;
[0087] S6. The product obtained in step S5 was filtered and washed with deionized water and anhydrous ethanol for 4 times respectively, and the obtained product was dried in an oven at 60° C. for 12 h, and the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material was obtained after grinding; wherein the specific surface area of the Bi2MoO6 / g-C3N4 / kaolin composite material after grinding was 49 m 2 / g, and the pore size distribution is in the range of 15-20nm.
[0088] Example 6: Different from Example 1, the mineralization treatment method is as follows: a reducing mineralizer is prepared according to a mass ratio of solution C to reducing mineralizer of 1:0.5, and then the reducing mineralizer is added dropwise to a reactor containing solution C, and stirring is continued for 20 minutes during the dropping process to generate product A, which is washed with deionized water, air, and carbon dioxide for 4 times in sequence, and finally the reactor is sealed and placed in a microwave hydrothermal reactor for reaction for 25 minutes to obtain a mineralized solution C; wherein the microwave hydrothermal reaction temperature is set to 230°C and the power is set to 100W; and the filling ratio of the microwave hydrothermal reactor is controlled to be 55%;
[0089] The reducing mineralizer comprises, by weight percentage, 40% of sodium hydroxide, 5% of ammonium chloride, 5% of sodium polyacrylate and the balance of water.
[0090] Example 7: Different from Example 1, the mineralization treatment method is as follows: a reducing mineralizer is prepared according to a mass ratio of solution C to reducing mineralizer of 1:0.8, and then the reducing mineralizer is added dropwise to a reactor containing solution C, and stirring is continued for 40 minutes during the dropping process to generate product A, which is washed with deionized water, air, and carbon dioxide for 6 times in sequence, and finally the reactor is sealed and placed in a microwave hydrothermal reactor for reaction for 30 minutes to obtain a mineralized solution C; wherein the temperature of the microwave hydrothermal reactor is set to 250°C and the power is set to 150W; and the filling ratio of the microwave hydrothermal reactor is controlled to be 65%;
[0091] The reducing mineralizer comprises, by weight percentage, 45% of sodium hydroxide, 10% of ammonium chloride, 7% of sodium polyacrylate and the balance of water.
[0092] Experimental example: XRD test
[0093] XRD analysis was performed on kaolin, g-C3N4, Bi2MoO6, g-C3N4 / kaolin, Bi2MoO6 / kaolin, Bi2MoO6 / g-C3N4 and composite photocatalysts with different mass ratios of Bi2MoO6 / g-C3N4 / kaolin. Figure 1 As shown, the characteristic diffraction peak of Bi2MoO6 can be clearly seen in the XRD spectrum of the Bi2MoO6 / g-C3N4 / kaolin ternary composite material, proving that the ternary composite photocatalyst was successfully prepared.
[0094] SEM Testing
[0095] SEM analysis was performed on kaolin, intercalated-exfoliated kaolin, g-C3N4, Bi2MoO6, g-C3N4 / kaolin and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts. Figure 2 As shown in (a) and (b), pure kaolin is stacked in a book shape, and the kaolin aggregates after intercalation and stripping are significantly reduced, and the number of thin kaolin flakes increases. Figure 2 As shown in (c), the morphology of pure g-C3N4 presents a lamellar stacking morphology with larger particle size. Figure 2 As shown in (d), the morphology of pure Bi2MoO6 is a microsphere or flower-like structure with a diameter of 1 to 1.5 μm, and the aggregate is composed of nano-spherical particles and nano-sheets. Figure 2 As shown in (e), in the g-C3N4 / kaolin composite material, the agglomeration of g-C3N4 can be significantly improved, and the g-C3N4 nanoparticles can be well dispersed on the kaolin sheet. Figure 2 As shown in (f), the Bi2MoO6 / g-C3N4 / kaolin composite material is in the form of particle stacking, and many Bi2MoO6 fragments are loaded on the surface.
[0096] TEM test
[0097] TEM analysis was performed on the g-C3N4 / kaolin and Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic materials. Figure 3 As shown in (a), in the g-C3N4 / kaolin binary composite material, kaolin and g-C3N4 are tightly bound together, which increases the specific surface area of the material and provides more active sites for photocatalytic reactions. Figure 3 As shown in (b), in the Bi2MoO6 / g-C3N4 / kaolin ternary composite material, kaolin, g-C3N4 nanosheets and Bi2MoO6 nanosheets formed a heterojunction structure through coupling, further confirming the formation of the ternary composite material structure.
[0098] BET Test
[0099] BET analysis was performed on kaolin, g-C3N4, Bi2MoO6 and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts. Figure 4As shown in (a) and (b), compared with pure g-C3N4 and kaolin, the number of mesopores in the Bi2MoO6 / g-C3N4 / kaolin composite material is increased, and its pore size distribution is in the range of 2-20nm, which is beneficial to promote the adsorption and diffusion of the target reactants.
[0100] PL test
[0101] PL analysis was performed on g-C3N4, Bi2MoO6 and Bi2MoO6 / g-C3N4 / kaolin composite photocatalysts. Figure 5 As shown, the fluorescence intensity of the Bi2MoO6 / g-C3N4 / kaolin composite material is low, indicating that the introduction of kaolin and the formation of Bi2MoO6 / g-C3N4 heterojunction can effectively improve the separation efficiency of electron-hole pairs.
[0102] The properties and parameters of the final products in Examples 1 to 7 were tested and calculated according to the following method. The results are listed in Table 1.
[0103] Determination of photocatalytic degradation performance of tetracycline wastewater: Tetracycline is widely used and used in the largest amount, and is one of the main antibiotic pollutants. Therefore, tetracycline was selected as the target liquid phase pollutant to test the degradation performance of the sample on antibiotic wastewater. The smaller the absorbance of tetracycline under specific conditions, the better the photocatalytic degradation performance of the composite material. In this specific embodiment, the concentration of the tetracycline solution used is 30 mg / L, and 50 mL of tetracycline solution is taken each time and mixed with 0.04 g of the product, and ultrasonically dispersed for 5 minutes. After 1 hour of dark reaction, turn on the 500W xenon lamp for photocatalytic reaction, take samples at regular intervals, extract 3 mL of solution each time, filter out the catalyst with a 0.22 μm filter membrane, and use an ultraviolet spectrophotometer to accurately measure the absorbance C of the tetracycline solution at a wavelength of 355 nm. Then the removal rate of the tetracycline solution is calculated as follows: Removal rate = (C0-C t ) / C0×100%, where C0 is the absorbance of the initial tetracycline solution, C t is the absorbance value of the tetracycline solution when the reaction is complete.
[0104] Adsorption of formaldehyde gas - Determination of photocatalytic degradation performance: Formaldehyde is a volatile organic pollutant widely present in the air, which greatly reduces the indoor air quality and causes irreversible damage to human health. Therefore, formaldehyde is used as the target gas phase pollutant to further evaluate the visible light photocatalytic performance of the material. The formaldehyde reaction device is mainly composed of a 0.125L reaction box, a light source, a heating device, a fan, an injection port, a sampling pump, a formaldehyde detector and a CO2 detector. The light source is 3 LED lamps with a power of 8W. The lifting platform is located directly below the light source. The glass dish coated with the sample is placed on the lifting platform, and the distance between the sample and the light source is 15cm by adjusting the lifting platform. The main function of the heating device and the fan is to facilitate the dispersion and uniformity of formaldehyde. In this specific embodiment, the initial concentration of the formaldehyde gas used is about 1.54ppm. 750mg of catalyst is evenly applied to the glass dish and placed in the reaction box after drying. After dark adsorption for 60min, turn on the light to carry out the photocatalytic reaction process. Use formaldehyde detector and CO2 concentration detector to detect real-time formaldehyde concentration and CO2 concentration, and record data regularly. The formaldehyde removal rate calculation formula is: Removal rate = (C0-C t ) / C0×100%, where C0 is the initial formaldehyde concentration (ppm), and Ct is the formaldehyde concentration (ppm) when the reaction is completed.
[0105] Table 1 Performance and parameters of the final products of kaolin, g-C3N4, Bi2MoO6 and Examples 1 to 7 and Comparative Examples 1 to 3
[0106]
[0107] The difference between Control Example 1 and Example 1 is that no nitrogen blowing operation is performed during the preparation of intercalation-exfoliation kaolin.
[0108] The difference between Control Example 2 and Example 1 is that Solution C is not subjected to mineralization treatment.
[0109] The difference between Comparative Example 3 and Example 1 is that the reducing mineralizer does not contain ammonium chloride.
[0110] Conclusion: From the data in Table 1, it can be seen that the catalytic performance of the composite photocatalytic material obtained in Control Example 1 without nitrogen blowing is slightly reduced. Under the combined action of nitrogen blowing and ultrasonic treatment, the surface of kaolin becomes more active and porous, which is beneficial to the loading of Bi2MoO6 particles and g-C3N4, and is beneficial to increasing the loading amount of intercalated-stripped kaolin and enhancing the overall performance of the composite material. In addition, nitrogen blowing and ultrasonic treatment may help to improve the interfacial bonding ability of intercalated-stripped kaolin and promote the interfacial bonding ability between Bi2MoO6 particles, g-C3N4 and kaolin. force, good interface bonding can reduce the internal resistance between materials, improve the charge transfer efficiency, and thus enhance the photocatalytic performance of the composite material; in control example 2, if the bismuth nitrate solution is not mineralized, the catalytic performance of the composite photocatalytic material will be affected. This is because the present invention mineralizes the bismuth nitrate solution and then reacts with sodium molybdate, which helps it to react better with sodium molybdate and then firmly load it on the kaolin surface. At the same time, on the kaolin surface where carbon nitride is present, the stable loading state can reduce the loss of the catalyst during the reaction, thereby improving the catalytic efficiency and the life of the catalyst. In addition, the bismuth nitrate solution after mineralization has a small amount of delta-Bi2O3 containing a cubic fluorite ore structure, and some oxygen ion positions in its lattice are vacant, so it has very high oxygen ion conductivity. This structure can promote its interaction with oxygen-containing groups on the surface of kaolin, thereby improving the composite photocatalytic effect. In addition, the composite material prepared in the present application has a strong visible light photocatalytic degradation performance for pollutants, which solves the problem that the g-C3N4 / kaolin composite material has a high electron-hole pair recombination rate and a low photocatalytic degradation ability under visible light. The control example 3 does not contain chlorine The addition of ammonium chloride will lead to a weakening of the catalytic performance of the composite photocatalytic material. The main reason is that the addition of ammonium chloride can expand the kaolin, and when applied to molybdate solution, it can increase the conductivity of the solution, which is helpful for the extraction efficiency of molybdenum, thereby promoting the formation of bismuth molybdate to further improve the loading effect; in addition, ammonium chloride itself can also be used as a chemical swelling agent, which can produce gas through thermal decomposition to achieve the expansion effect of the material, thereby expanding the kaolin and further promoting the loading effect of bismuth molybdate and carbon nitride on the surface of kaolin. Therefore, the present application has significant progress compared with the prior art.
Claims
1. A visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material, characterized in that: The composite photocatalytic material is prepared by loading nano g-C3N4 and Bi2MoO6 particles on the surface of a kaolin sheet, wherein the average particle size of the Bi2MoO6 particles is 1 to 1.5 μm, the nano g-C3N4 is a nano sheet, and the average size of the nano g-C3N4 is 2 to 5 μm. In the composite photocatalytic material, the mass ratio of kaolin to Bi2MoO6 is 0.4 to 1.2:1, and the mass ratio of kaolin to nano g-C3N4 is 3:1.5 to 2.
2. A visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material as claimed in claim 1, characterized in that: The kaolin is intercalated-exfoliated kaolin, The preparation method of the intercalation-stripping kaolin is: Step A: 3-5 g of kaolin and 3-5 g of urea are mixed, 30-50 mL of deionized water is added, and centrifugation is performed at 40-60° C. and a speed of 10000-13000 rpm for 10-15 min to form a suspension; Step B: The suspension obtained in step A is filtered, washed, and then dried at 80° C. to obtain a white product; Step C: add 20-40 mL of deionized water to the white product obtained in step B, and perform ultrasonic treatment at 50-70° C. for 6-10 min. During the ultrasonic treatment, blow nitrogen into the mixed solution for 5-6 min to obtain a mixed solution; Step D: The mixed solution obtained in step C is filtered, washed, and then dried at 80° C. to obtain intercalation-exfoliation kaolin.
3. A visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material as claimed in claim 2, characterized in that: The ultrasonic frequency in step C is 30-50 KHz, and the ultrasonic power density is 0.2-0.25 W / cm 2 .
4. A method for preparing a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material according to any one of claims 1 to 3, characterized in that: Using kaolin as a carrier, melamine, Bi(NO3)3·5H2O and Na2MoO4·2H2O as precursors, nano g-C3N4 and Bi2MoO6 are loaded on the surface of kaolin sheets by solid phase sintering method and solvothermal method, including the following steps: S1. Mix kaolin flakes and melamine in a mass ratio of 3:4 and grind in a mortar for 30 to 60 minutes; S2, calcining the mixture obtained in step S1 at a heating rate of 2.5-5°C / min, and keeping the temperature at 525-575°C for 3.9-4.1h, and grinding the obtained product after the end of the heat preservation to obtain a kaolin-loaded g-C3N4 composite photocatalytic material; S3, dissolve 0.8-1.0 g Bi(NO3)3·5H2O and 0.23-0.25 g Na2MoO4·2H2O respectively in 10-20 mL ethylene glycol, and stir to form solution A and solution B; S4, then add 30-60 mL of anhydrous ethanol to solution A, and continue stirring for 20-40 min to obtain solution C, then take 0.3-0.9 g of kaolin-loaded g-C3N4 composite photocatalytic material in step S2 and add it to solution C, continue stirring for 20-40 min to obtain solution D, and finally add solution B to solution D, and stir for 20-40 min to mix; S5, transferring the suspension obtained in step S4 to a high pressure reactor, maintaining the reaction temperature at 150-180° C. for 6-12 hours; S6. Filter the product obtained in step S5 and wash it with deionized water and anhydrous ethanol for 2 to 4 times respectively, dry the obtained product in an oven at 55-65°C for 10 to 12 hours, and grind it to obtain the Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material.
5. The method for preparing a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material according to claim 4, characterized in that: In step S4, the added amount of kaolin-loaded g-C3N4 composite photocatalytic material is 0.5 g.
6. The method for preparing a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material according to claim 4, characterized in that: In step S6, the Bi2MoO6 / g-C3N4 / kaolin composite material is ground to a specific surface area of 37 to 49 m 2 / g, and the pore size distribution is in the range of 2 to 20 nm.
7. The method for preparing a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material according to claim 4, characterized in that: In step S4, solution C is subjected to mineralization treatment. The mineralization treatment method comprises: preparing a reducing mineralizer according to a mass ratio of solution C to reducing mineralizer of 1:0.5-0.8, then dropping the reducing mineralizer dropwise into a reactor containing solution C, continuously stirring for 20-40 minutes during the dropping process, generating product A, washing the surface of product A with deionized water, air and carbon dioxide for 4-6 times respectively, finally sealing the reactor and placing it in a microwave hydrothermal reactor for reaction for 25-30 minutes, and obtaining a mineralized solution C; wherein the temperature of the microwave hydrothermal reactor is set to 230-250°C and the power is set to 100-150W.
8. The method for preparing a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material according to claim 7, characterized in that: The reducing mineralizer comprises, by weight percentage, 40-45% of sodium hydroxide, 5-10% of ammonium chloride, 5-7% of sodium polyacrylate and the balance of water.
9. The method for preparing a visible light responsive Bi2MoO6 / g-C3N4 / kaolin composite photocatalytic material according to claim 7, characterized in that: The filling ratio of the microwave hydrothermal reactor is controlled to be 55-65%.
Citation Information
Patent Citations
Preparation method of ultrafine silane surface grafted kaolinite powder body
CN103864084A
Attapulgite / graphite phase carbon nitride composite material and preparation method thereof
CN104588063A
Method for preparing bismuth sulfide / montmorillonite composite material by hydrothermal method
CN104891514A
Preparation method and application of bismuth molybdate / graphite-phase carbon nitride composite catalyst
CN106076389A
g-C3N4 / kaolinite composite photocatalyst and preparation method thereof
CN106111174A