Preparation method and application of 3D printing copper-nickel alloy electrode

The preparation of copper-nickel alloy electrodes through 3D printing technology solves the problem of poor stability of nanostructured catalysts in extreme environments, achieves efficient ammonia recovery and energy consumption reduction, and is suitable for high-concentration nitrate wastewater treatment.

CN118893211APending Publication Date: 2024-11-05TSINGHUA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410921527.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing nanostructured catalysts are susceptible to extreme environments, resulting in limited ammonia recycling applications in high-concentration nitrate wastewater, and 3D printing technology has not been fully explored in this field.

Method used

Copper-nickel alloy electrodes are prepared by 3D printing technology, and a metal amorphous surface is formed by mechanical ball milling and laser printing. Combined with appropriate process parameters such as mass ratio, particle size, ball milling time and laser parameters, an excellent conductivity and porous structure is prepared. copper-nickel alloy electrode.

Benefits of technology

It achieves efficient and stable ammonia yield and Faraday efficiency in the process of electrocatalytic nitrate reduction and synthesis of ammonia. The electrode remains stable under large current conditions and reduces energy consumption. It is suitable for the treatment of high-concentration nitrate wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893211A_ABST
    Figure CN118893211A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a 3D printing copper-nickel alloy electrode, and the preparation method comprises the following steps: 1) mixing: carrying out mechanical ball milling on micron spherical copper powder and micron spherical nickel powder to obtain copper-nickel composite powder; (2) 3D printing is conducted, specifically, 3D laser printing is conducted on the copper-nickel composite powder obtained in the step (1), and a 3D printed copper-nickel alloy electrode is obtained; wherein the mass ratio of the micron spherical copper powder to the micron spherical nickel powder is 1: (0.5-2), and an amorphous layer is arranged on the surface of the copper-nickel alloy electrode. The preparation method disclosed by the invention has the outstanding advantages of simple preparation, controllable structure and the like, not only provides a thought for researching a nitrate reduction synthesis ammonia green energy system, but also provides reference significance for designing a novel nitrate reduction synthesis ammonia electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of preparing ammonia by electrocatalytic nitrate reduction and 3D printed copper-nickel alloy electrodes, and specifically relates to a preparation method of a 3D printed copper-nickel alloy electrode and an application thereof in preparing ammonia by electrocatalytic nitrate reduction. Background Art

[0002] Excessive discharge of nitrates will lead to eutrophication of water bodies, seriously affecting aquatic ecosystems and even endangering human health. Low-concentration nitrate wastewater is usually removed by biological denitrification technology, while high-concentration nitrate industrial wastewater, due to its complex water quality, is usually evaporated and crystallized before being landfilled. However, nitrates buried underground are at risk of leaking into groundwater. Electrocatalytic reduction of nitrate nitrogen is a promising method for recovering ammonia from high-concentration nitrate wastewater. The principle is to transfer eight electrons and multiple protons (NO3 - +6H2O+8e - →NH3+9OH - ), reducing nitrate to ammonia.

[0003] At present, significant progress has been made in the design and preparation of catalysts, and the selectivity and Faraday efficiency of nitrate reduction have been significantly improved. For example, copper-based nanocatalysts are widely used in nitrate reduction processes due to their high active surface area. In addition, the introduction of other metals (such as iron, cobalt, nickel, ruthenium, etc.) into the catalyst can further improve the activity and selectivity of the catalyst (see Reference 1, Reference 2, Reference 3, Reference 4 and Reference 5). However, nanostructured catalysts are susceptible to extreme environments due to their low Young's modulus and the complexity of the actual industrial wastewater components, which seriously hinders their practical application and industrial promotion.

[0004] In recent years, 3D printing technology, as an emerging material and device preparation technology, has attracted much attention due to its potential applications in electronics, aviation, medicine, new energy and other fields. Advances in technologies such as 3D printing technology (also known as "additive manufacturing" technology) have revolutionized material manufacturing technology, with rapid prototyping capabilities and flexibility in design and printing. This innovative technology has the potential to provide structures with a variety of geometries, better rigidity, adjustable porosity and size, thereby alleviating multiple limitations associated with traditional manufacturing technologies. In addition, the design can be modified using computer-aided design (CAD) software and is relatively simple. The nanostructures of these 3D-printed catalyst structures at micron resolution can induce pores and increase specific surface area, providing nano features, which are beneficial to improving catalytic activity. At the same time, the catalyst structures based on 3D printing can be designed into different geometric forms, which can increase the opportunity to manufacture active catalyst structures for nitrate reduction to synthesize ammonia.

[0005] Based on this, the copper-nickel alloy electrode with a metallic amorphous surface prepared by 3D printing technology in the present invention is used in the electrocatalytic reduction of nitrate to synthesize ammonia. There is no relevant report in this regard at present.

[0006] References:

[0007] Reference 1: CN116536698A

[0008] Reference 2: CN115465923A

[0009] Reference 3: CN116892037A

[0010] Reference 4: CN115074757A

[0011] Reference 5: CN117626347A Summary of the invention

[0012] Problem that the invention aims to solve

[0013] The technical problem solved by the present invention is to provide a preparation method and application of a 3D printed copper-nickel alloy electrode. The method successfully prepares a metal electrode through 3D laser printing technology. Copper and nickel form an alloy in the metal electrode, and the surface of the prepared copper-nickel alloy electrode has a metallic amorphous (glassy) surface layer.

[0014] Furthermore, the present invention also provides an application of the copper-nickel alloy electrode in electrocatalytic nitrate reduction to synthesize ammonia, in which the copper-nickel alloy electrode exhibits excellent ammonia yield, Faraday efficiency and stability.

[0015] Solutions for solving problems

[0016] The present invention believes that the above technical problems can be solved by implementing the following technical solutions:

[0017] [1]. The present invention provides a method for preparing a 3D printed copper-nickel alloy electrode, which comprises the following steps:

[0018] 1) Mixing step: mechanically milling the micron spherical copper powder and the micron spherical nickel powder to obtain a copper-nickel composite powder;

[0019] 2) 3D printing step: performing 3D laser printing on the copper-nickel composite powder obtained in step 1) to obtain a 3D printed copper-nickel alloy electrode;

[0020] Wherein, the mass ratio of the micron spherical copper powder to the micron spherical nickel powder is 1:(0.5-2),

[0021] The copper-nickel alloy electrode has an amorphous layer on its surface.

[0022] [2]. The preparation method according to [1], wherein in step 1),

[0023] The average particle size of the micron spherical copper powder is 15 to 53 μm;

[0024] The average particle size of the micron spherical nickel powder is 15 to 53 μm.

[0025] [3]. The preparation method according to [1] or [2], wherein in step 1),

[0026] The mass ratio of the micron spherical copper powder to the micron spherical nickel powder is 1:(0.8-1.2).

[0027] [4]. The preparation method according to any one of [1] to [3], wherein in step 1),

[0028] The rotation speed of the mechanical ball mill is 100 to 300 rpm, and the time of the mechanical ball mill is 1 to 3 hours.

[0029] [5]. The preparation method according to any one of [1] to [4], wherein in step 2),

[0030] The laser power is 200-400W, the scanning speed is 600-900mm / s, the powder layer thickness is 25-35μm, and the protective gas flow rate is 15-25L / min.

[0031] [6] The preparation method according to [5], wherein the protective gas is argon.

[0032] [7]. The preparation method according to any one of [1] to [6], wherein the preparation method further comprises the steps of separation and cleaning.

[0033] [8] The preparation method according to any one of [1] to [7], wherein the thickness of the amorphous layer is 1 to 10 nm.

[0034] [9]. The method according to any one of [1] to [8], wherein the resistivity of the copper-nickel alloy electrode is no more than 5.0×10 -5 Ω·cm.

[0035]

[10] . Application of a 3D printed copper-nickel alloy electrode prepared by the preparation method described in any one of [1] to [9] in electrocatalytic nitrate reduction to synthesize ammonia.

[0036] Effects of the Invention

[0037] 1) The 3D printed copper-nickel alloy electrode provided by the present invention has good electrical conductivity, and the resistivity does not exceed 5.0×10 -5 Ω·cm, which is beneficial to reduce the generation of Joule heat under high current conditions and improve energy utilization; at the same time, it has a large number of hierarchical porous structures, which provide more active sites for the nitrate reduction ammonia synthesis catalyst, greatly increase the contact area with the solution, and reduce energy consumption.

[0038] 2) The 3D printed copper-nickel alloy electrode provided by the present invention has good catalytic activity and can reach 100 mA / cm at -0.1 V compared with the standard hydrogen electrode. 2 The current density is -0.5V, and the yield of NH3-N is 0.94mmolh -1 cm -2 , the Faradaic efficiency of NH3 is >93%.

[0039] 3) The 3D printed copper-nickel alloy electrode provided by the present invention has excellent stability and an amorphous layer on the surface, which enables it to withstand 200 mA / cm 2 The reaction was carried out stably for more than 1000 h at an industrial current density of 1.38 W, and there was no significant change in the XRD and SEM images before and after the reaction.

[0040] 4) The 3D printed copper-nickel alloy electrode provided by the present invention can be applied to actual industrial nitrate wastewater, and high-purity ammonium chloride can be recovered from electroplating wastewater and photovoltaic wastewater with high nitrate concentration. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the XRD spectrum of the copper-nickel alloy electrode (MPCN) prepared in Example 1.

[0042] Figure 2 This is the TEM image of the copper-nickel alloy electrode prepared in Example 1.

[0043] Figure 3 The diagram is a Faraday efficiency diagram of the copper-nickel alloy electrode (MPCN) prepared in Example 1, the copper electrode (Cu) prepared in Comparative Example 3, and the nickel electrode (Ni) prepared in Comparative Example 4 at different potentials.

[0044] Figure 4 1 and 2 are linear sweep voltammetry (LSV) curves of the copper-nickel alloy electrodes prepared in Example 1, Comparative Example 1 and Comparative Example 2.

[0045] Figure 5 This is a long-term operation diagram of the copper-nickel alloy electrode prepared in Example 1.

[0046] Figure 6 The nitrate nitrogen removal rate and ammonia nitrogen selectivity of the copper-nickel alloy electrode prepared in Example 1 in treating actual photovoltaic wastewater. DETAILED DESCRIPTION

[0047] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. In order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details.

[0048] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0049] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0050] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0051] In this specification, "amorphous layer" and "surface layer having a metallic amorphous state (glassy state)" have the same meaning, and both refer to a metal or alloy solid without a three-dimensional periodic arrangement of atoms.

[0052] In the present invention, a numerical range expressed using "above" or "below" means a numerical range including the number.

[0053] In the present invention, the use of "optional" or "optionally" indicates that certain substances, components, execution steps, applied conditions and other factors are used or not used.

[0054] In the present invention, unless otherwise specified, the "normal temperature" used generally refers to a temperature of 23±2°C.

[0055] In the present invention, unless otherwise stated, "%" used herein means weight or mass percentage.

[0056] In this specification, the term "about" or "substantially" or "essentially" may mean that a value includes the standard deviation of the error of the device or method used to determine the value. The numerical ranges and parameters used to define the present invention are all approximate values, and the relevant values ​​in the specific embodiments have been presented as accurately as possible. However, any numerical value essentially inevitably contains the standard deviation caused by the aforementioned testing device or method. Therefore, unless otherwise explicitly stated, it should be understood that all ranges, quantities, values ​​and percentages used in the present invention are modified by "about". Here, "about" generally means that the standard deviation of the actual value and the theoretical model or theoretical data is within 3%, preferably 2%, and more preferably 1%.

[0057] In the present invention, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0058] <First aspect>

[0059] A first aspect of the present invention provides a method for preparing a 3D printed copper-nickel alloy electrode, comprising the following steps:

[0060] 1) Mixing step: mechanically milling the micron spherical copper powder and the micron spherical nickel powder to obtain a copper-nickel composite powder;

[0061] 2) 3D printing step: The copper-nickel composite powder obtained in step 1) is subjected to 3D laser printing to obtain a 3D printed copper-nickel alloy electrode.

[0062] Each step is described in detail below.

[0063] Step 1): Mixing step

[0064] In step 1), firstly, micron spherical copper powder and micron spherical nickel powder are put into a ball mill for mechanical ball milling to obtain copper-nickel composite powder.

[0065] In the present invention, the average particle size of the micron spherical copper powder is 15 to 53 μm, preferably 15 to 50 μm, for example, it can be 18 μm, 20 μm, 23 μm, 25 μm, 28 μm, 30 μm, 33 μm, 35 μm, 38 μm, 40 μm, 43 μm, 45 μm, 48 μm, 49 μm, etc.; the average particle size of the micron spherical nickel powder is 15 to 53 μm, preferably 15 to 50 μm, for example, it can be 18 μm, 20 μm, 23 μm, 25 μm, 28 μm, 30 μm, 33 μm, 34 μm, 35 μm, 38 μm, 40 μm, 43 μm, 45 μm, 48 μm, 49 μm, etc. The present invention controls the average particle size of micron spherical copper powder and nickel powder within the above range to maintain excellent powder fluidity during 3D printing powder feeding, which is beneficial to improving the forming quality of the prepared alloy and improving its comprehensive mechanical properties.

[0066] In a specific embodiment of the present invention, the mass ratio of the micron spherical copper powder to the micron spherical nickel powder is 1:(0.5-2), preferably 1:(0.8-1.2), for example, 1:0.6, 1:0.7, 1:0.9, 1:1, 1:1.1, 1.3:1, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, etc. The present invention controls the amount of micron spherical copper powder and micron spherical nickel powder within the above range to regulate the morphology, quantity and distribution of the copper phase and the nickel phase in the prepared alloy, which is beneficial to maintaining its good plastic elongation while improving the room temperature and high temperature strength, and achieving the best matching effect of alloy strength and toughness.

[0067] In a specific embodiment of the present invention, the rotation speed of the mechanical ball mill is 100-300 rpm, preferably 150-250 rpm, and more preferably 200 rpm.

[0068] In a specific embodiment of the present invention, the time of the mechanical ball milling is 1 to 3 hours, preferably 1.5 to 2.5 hours, and more preferably 2 hours.

[0069] The present invention controls the rotation speed and time of mechanical ball milling within the above range, so as to facilitate better and more uniform dispersion of micron spherical copper powder and micron spherical nickel powder, and is beneficial to improving the comprehensive performance of the copper-nickel alloy electrode prepared subsequently.

[0070] Step 2): 3D printing steps

[0071] In step 2), the copper-nickel composite powder obtained in step 1) is subjected to 3D laser printing to obtain a 3D printed copper-nickel alloy electrode.

[0072] In a specific embodiment of the present invention, the device used for 3D printing is a 3D laser printer, preferably a laser directed energy deposition laser.

[0073] In a specific embodiment of the present invention, the process parameters of the 3D laser printer include: laser power of 200-400 W, for example, 230 W, 250 W, 300 W, 350 W, 380 W, etc.; scanning speed of 600-900 mm / s, for example, 650 mm / s, 700 mm / s, 750 mm / s, 800 mm / s, 850 mm / s, 900 mm / s, etc.; powder layer thickness of 25-35 μm, for example, 26 μm, 28 μm, 30 μm, 32 μm, 34 μm, etc.; protective argon gas flow rate of 15-25 L / min, for example, 16 L / min, 18 L / min, 20 L / min, 22 L / min, 24 L / min, etc. The present invention controls the process parameters of the 3D laser printer within the above range, so as to obtain a near-equiaxed crystal structure without cracks and holes and with finer grains through appropriate laser heat input, thereby greatly improving the strength and toughness of the alloy at room temperature and high temperature.

[0074] Other Steps

[0075] The method for preparing the 3D printed copper-nickel alloy electrode of the present invention may optionally include a separation step and a cleaning step in addition to the above-mentioned mixing step and 3D printing step.

[0076] For the separation step, wire cutting can be used to separate the 3D printed copper-nickel alloy electrode from the substrate.

[0077] For the cleaning step, typically, acetone, deionized water, hydrochloric acid, and deionized water can be used in sequence to clean the prepared 3D printed copper-nickel alloy electrode to remove impurities on the electrode surface. In a preferred embodiment of the present invention, the concentration of the hydrochloric acid is 1 to 6 mol / L, for example, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 5.5 mol / L, etc.; the cleaning time is 5 to 20 min, for example, 7 min, 9 min, 12 min, 15 min, 17 min, 19 min, etc.

[0078] <Second Aspect>

[0079] In a second aspect of the present invention, a 3D printed copper-nickel alloy electrode prepared according to the preparation method described in the first aspect of the present invention is provided.

[0080] In a specific embodiment of the present invention, the 3D printed copper-nickel alloy electrode of the present invention has an amorphous layer on its surface (ie, a surface layer of metal amorphous (glassy) state).

[0081] In a preferred embodiment of the present invention, the thickness of the amorphous layer is 1 to 10 nm, for example, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, etc.

[0082] In a preferred embodiment of the present invention, the resistivity of the copper-nickel alloy electrode is no more than 5.0×10 -5 Ω·cm, for example, can be 4.9×10 -5 Ω·cm、4.8×10 -5 Ω·cm、4.7×10 -5 Ω·cm、4.6×10 -5 Ω·cm、4.5×10 -5 Ω·cm、4.3×10 -5 Ω·cm、4.0×10 -5 Ω·cm、3.5×10 -5 Ω·cm, etc. or less.

[0083] <Third Aspect>

[0084] In the third aspect of the present invention, there is provided the use of the 3D printed copper-nickel alloy electrode according to the second aspect of the present invention in the electrocatalytic nitrate reduction synthesis of ammonia.

[0085] In a specific embodiment of the present invention, the 3D printed copper-nickel alloy electrode is used as the cathode and the IrO2-Ta2O5 / Ti electrode is used as the anode, and an electrocatalytic reduction method is used to convert nitrate ions in the wastewater into ammonia, and further generate ammonium salts, thereby realizing nitrogen recovery.

[0086] Example

[0087] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0088] Embodiment 1:

[0089] A method for preparing a 3D printed copper-nickel alloy electrode comprises the following steps:

[0090] 1) Spherical copper powder with an average particle size of 34 μm and spherical nickel powder with an average particle size of 34 μm were weighed, mixed in a mass ratio of 1:1, put into a ball mill, and mechanically ball milled at a rotation speed of 200 rpm for 2 h to obtain a copper-nickel composite powder.

[0091] 2) The copper-nickel composite powder obtained in step 1) is placed in a laser 3D printer for printing to obtain a 3D printed copper-nickel alloy electrode. The electrode structure is three-dimensionally modeled using magics software, and the process parameters of the laser 3D printer include: laser power of 400W, scanning speed of 900mm / s, powder layer thickness of 30μm, and protective argon gas flow rate of 20L / min.

[0092] 3) Remove the powder around the electrode and separate the 3D printed copper-nickel alloy electrode from the substrate using wire cutting.

[0093] 4) Use acetone, deionized water, 3 mol / L hydrochloric acid, and deionized water to clean the 3D printed copper-nickel alloy electrode in sequence for 5 minutes to remove surface impurities.

[0094] The copper-nickel alloy electrode prepared in this example is denoted as Cu 50 Ni 50 (or MPCN).

[0095] Comparative Example 1:

[0096] A method for preparing a 3D printed copper-nickel alloy electrode comprises the following steps:

[0097] 1) Spherical copper powder with an average particle size of 34 μm and spherical nickel powder with an average particle size of 34 μm were weighed, mixed in a mass ratio of 9:1, put into a ball mill, and mechanically ball milled at a rotation speed of 200 rpm for 2 h to obtain a copper-nickel composite powder.

[0098] 2) The copper-nickel composite powder obtained in step 1) is placed in a laser 3D printer for printing to obtain a 3D printed copper-nickel alloy electrode. The electrode structure is three-dimensionally modeled using magics software, and the process parameters of the laser 3D printer include: laser power of 400W, scanning speed of 900mm / s, powder layer thickness of 30μm, and protective argon gas flow rate of 20L / min.

[0099] 3) Remove the powder around the electrode and separate the 3D printed copper-nickel alloy electrode from the substrate using wire cutting.

[0100] 4) Use acetone, deionized water, 3 mol / L hydrochloric acid, and deionized water to clean the 3D printed copper-nickel alloy electrode in sequence for 5 minutes to remove surface impurities.

[0101] The copper-nickel alloy electrode prepared in this comparative example is denoted as Cu 90 Ni 10 .

[0102] Comparative Example 2:

[0103] A method for preparing a 3D printed copper-nickel alloy electrode comprises the following steps:

[0104] 1) Spherical copper powder with an average particle size of 34 μm and spherical nickel powder with an average particle size of 34 μm were weighed, mixed in a mass ratio of 7:3, put into a ball mill, and mechanically ball milled at a rotation speed of 200 rpm for 2 h to obtain a copper-nickel composite powder.

[0105] 2) The copper-nickel composite powder obtained in step 1) is placed in a laser 3D printer for printing to obtain a 3D printed copper-nickel alloy electrode. The electrode structure is three-dimensionally modeled using magics software, and the process parameters of the laser 3D printer include: laser power of 400W, scanning speed of 900mm / s, powder layer thickness of 30μm, and protective argon gas flow rate of 20L / min.

[0106] 3) Remove the powder around the electrode and separate the 3D printed copper-nickel alloy electrode from the substrate using wire cutting.

[0107] 4) Use acetone, deionized water, 3 mol / L hydrochloric acid, and deionized water to clean the 3D printed copper-nickel alloy electrode in sequence for 5 minutes to remove surface impurities.

[0108] The copper-nickel alloy electrode prepared in this comparative example is denoted as Cu 70 Ni 30 .

[0109] Comparative Example 3:

[0110] A 3D printed pure copper electrode was prepared according to the method of Example 1. The difference from Example 1 is that micron spherical copper powder is directly used as a raw material for 3D printing without adding micron spherical nickel powder.

[0111] Comparative Example 4:

[0112] A 3D printed pure nickel electrode was prepared according to the method of Example 1. The difference from Example 1 is that micron spherical nickel powder is directly used as a raw material for 3D printing without adding micron spherical copper powder.

[0113] In order to clarify the composition elements and surface microstructure of 3D printed copper-nickel alloy electrodes, XRD and TEM tests were performed on them. Figure 1 As shown in the figure, by comparing the XRD spectra of the copper-nickel alloy electrode, copper electrode and nickel electrode, the diffraction peak of the copper-nickel alloy electrode is located between the diffraction peaks of copper and nickel, indicating the formation of copper-nickel alloy. Figure 2 As shown, there is an amorphous layer with a thickness of 1 to 5 nm on the surface of the electrode. The surface amorphous layer will protect the inside of the electrode and make it have excellent stability.

[0114] The 3D printed copper-nickel alloy electrode in Example 1 of the present invention has good electrical conductivity, and the resistivity is 4.7×10 -5 Ω·cm, which is beneficial to reduce the generation of Joule heat under high current conditions and improve energy utilization; at the same time, it has a large number of hierarchical porous structures, which provide more active sites for the nitrate reduction ammonia synthesis catalyst, greatly increase the contact area with the solution, and reduce energy consumption.

[0115] Performance Testing

[0116] 1) Electrochemical nitrate reduction test

[0117] The electrochemical test was carried out in a conventional three-electrode H-type electrolytic cell controlled by an electrochemical workstation Autolab PGSTAT204. The anode chamber and cathode chamber were separated by a proton exchange membrane (Nafion 117), and the electrolyte was a 1M KOH solution containing 0.1M KNO3. The volume of the electrolyte in the anode and cathode chambers was 30mL each. 3D-printed copper-nickel alloy electrodes, copper electrodes, and nickel electrodes were used as working electrodes, respectively, with a working electrode area of ​​1cm 2 Commercial Ag / AgCl (saturated KCl solution) and platinum wire were used as the reference electrode and counter electrode, respectively.

[0118] like Figure 3 As shown in the figure, the nitrate reduction effect of the copper-nickel alloy electrode is better than that of the copper electrode and the nickel electrode. At a potential of -0.5 V vs. RHE, the Faradaic efficiency (FE) of NH3 NH3 ) reached 93%, and the NH3 yield was 0.94 mmol h -1 cm -2 .

[0119] In addition, if Figure 4 As shown in the figure, the copper-nickel alloy electrode of Example 1 of the present invention has good catalytic activity, and is superior to the copper-nickel alloy electrodes of Comparative Examples 1 and 2. Compared with the standard hydrogen electrode, it can reach 100 mA / cm under -0.1 V. 2 of current density.

[0120] 2) Stability test

[0121] At a current density of 200 mA / cm 2 In constant current mode, stability experiments were carried out in a homemade penetration reactor, e.g. Figure 5 As shown, the copper-nickel alloy electrode in Example 1 of the present invention can be used for 1000 hours without obvious change in voltage fluctuation, indicating that the electrode remains stable within 1000 hours.

[0122] 3) Actual high-concentration nitrate industrial wastewater resource treatment experiment

[0123] In a self-made membrane-free penetrating reactor, actual photovoltaic wastewater was used for actual wastewater treatment experiments. Before the experiment, F in the water was removed by pretreatment. - The concentration of nitrate in the wastewater is 1.5 M. The copper-nickel alloy electrode (about 20 mm in diameter) and the IrO2-Ta2O5 / Ti electrode (about 20 mm in diameter) in Example 1 of the present invention are used as the cathode and the anode, respectively. In order to treat the actual wastewater as a resource, a peristaltic pump is used to pump 100 mL of wastewater into the electrochemical reactor, and the water flows through the electrodes. A DC power supply is used to apply 200 mA / cm 2 After a certain period of time, 100 μL of solution was taken at 0, 2, 4, 6, and 12 hours to analyze the concentration of nitrate nitrogen and ammonia nitrogen. Figure 6 As shown, the nitric nitrogen removal rate can exceed 80% within 12 hours, and the selectivity of ammonia nitrogen is close to 100% in 12 hours; then, the ammonia is blown into 0.3M hydrochloric acid for absorption by air stripping, and white crystals are obtained after evaporation and crystallization. XRD characterization shows that the white crystals are high-purity NH4Cl.

[0124] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.

[0125] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for preparing a 3D printed copper-nickel alloy electrode, characterized in that: The following steps are involved: 1) Mixing step: mechanically milling the micron spherical copper powder and the micron spherical nickel powder to obtain a copper-nickel composite powder; 2) 3D printing step: performing 3D laser printing on the copper-nickel composite powder obtained in step 1) to obtain a 3D printed copper-nickel alloy electrode; Wherein, the mass ratio of the micron spherical copper powder to the micron spherical nickel powder is 1:(0.5-2), The copper-nickel alloy electrode has an amorphous layer on its surface.

2. The preparation method according to claim 1, characterized in that: In step 1), The average particle size of the micron spherical copper powder is 15 to 53 μm; The average particle size of the micron spherical nickel powder is 15 to 53 μm.

3. The preparation method according to claim 1 or 2, characterized in that: In step 1), The mass ratio of the micron spherical copper powder to the micron spherical nickel powder is 1:(0.8-1.2).

4. The preparation method according to any one of claims 1 to 3, characterized in that In step 1), The rotation speed of the mechanical ball mill is 100 to 300 rpm, and the time of the mechanical ball mill is 1 to 3 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In step 2), The laser power is 200-400W, the scanning speed is 600-900mm / s, the powder layer thickness is 25-35μm, and the protective gas flow rate is 15-25L / min.

6. The preparation method according to claim 5, characterized in that: The protective gas is argon.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The preparation method also includes the steps of separation and cleaning.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The thickness of the amorphous layer is 1-10 nm.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The resistivity of the copper-nickel alloy electrode is no more than 5.0×10 -5 Ω·cm.

10. Application of the 3D printed copper-nickel alloy electrode prepared by the preparation method according to any one of claims 1 to 9 in electrocatalytic nitrate reduction to synthesize ammonia.