Preparation method and application of papermaking black liquid-based hard carbon negative electrode
Through the preparation method of paper-making black liquid-based hard carbon negative electrode, porous heteroatom doping is achieved by using organic matter and metal salt in paper-making black liquid, solving the problems of instability in the preparation process of hard carbon negative electrode materials, and improving sodium ion batteries energy density and reduce battery costs.
Patent Information
- Application Number
- CN202410922624.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The existing hard carbon negative electrode materials have complex preparation processes, resulting in unstable performance and poor batch performance, and the low energy density of sodium ion batteries, which limits its application prospects.
The preparation method of papermaking black liquid-based hard carbon negative electrode is adopted. Through drying, crushing, calcining, pickling, alkali washing and tempering steps, porous heteroatom doping is achieved by using organic matter and metal salt in papermaking black liquid to enhance the hard carbon negative electrode. performance.
It realizes the preparation of hard carbon negative electrode materials with excellent performance, improves the energy density and reduces battery cost of sodium ion batteries, solves the problem of papermaking black liquid pollution, and realizes high-value utilization.
Smart Images

Figure CN118894515A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a preparation method and application of a papermaking black liquor-based hard carbon negative electrode. Background Art
[0002] Lithium-ion batteries are currently the first choice for commercial batteries, but the scarcity of lithium resources and high prices have limited the development of lithium-ion batteries. Sodium-ion batteries have become a research hotspot in recent years due to their low cost and abundant sodium reserves. However, sodium-ion batteries have a low energy density and are one of the preferred options in the future energy storage field. They have broad application prospects in the utilization of renewable energy sources such as wind power, solar energy, and tides that are restricted by geography and time. They also have potential application prospects in grid peak regulation and energy storage power stations. In summary, the development of high-performance sodium-ion batteries is of great significance to the development of the future energy storage field.
[0003] The rapid development of sodium-ion batteries has increased the demand for hard carbon negative electrodes, and it is necessary to develop hard carbon negative electrode materials with excellent performance. At present, hard carbon negative electrode precursor materials mainly include biomass-based, polymer-based, resin-based and coal-based carbon materials. These materials need to go through complex steps such as crushing, ball milling, and calcination to obtain hard carbon negative electrode powder. At the same time, in order to improve performance, they also need to go through modification steps such as pore formation and heteroatom doping, which increases the complexity of the preparation process of the hard carbon negative electrode, and the uniformity and batch quality of the product are poor. Therefore, the development of a more stable precursor and a simple preparation method is of great significance for the preparation of hard carbon negative electrodes. Summary of the invention
[0004] In view of the complex preparation process of biomass hard carbon precursors, the present invention provides a preparation method and application of a papermaking black liquor-based hard carbon negative electrode. By utilizing components such as organic matter, alkaline substances, and nitrogen, sulfur, and phosphorus substances contained in the papermaking black liquor, the controllable preparation of a porous heteroatom-doped hard carbon negative electrode is achieved, and a sodium ion battery hard carbon negative electrode material with excellent performance is obtained, thereby solving the pollution problem of papermaking black liquor and realizing its high-value utilization.
[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0006] In one aspect, the present invention provides a method for preparing a papermaking black liquor-based hard carbon negative electrode, the method comprising the following steps:
[0007] (1) drying and crushing the papermaking black liquor to obtain papermaking black liquor powder;
[0008] (2) calcining the papermaking black liquor powder at high temperature to obtain black liquor carbon powder;
[0009] (3) The black liquor carbon powder is acid-washed and alkaline-washed to remove impurities, and then washed with water until neutral;
[0010] (4) The black liquor carbon powder after impurities removal is subjected to high temperature tempering to obtain hard carbon powder.
[0011] Preferably, in step (1), the drying temperature is 80-150° C. and the drying time is 5-15 h.
[0012] Preferably, in step (2), the calcination temperature is 800-1600° C., and the calcination time is 2-20 h.
[0013] Preferably, in step (3), the acid used in the pickling is one of sulfuric acid, hydrochloric acid, and nitric acid, or a combination of the two, and the alkali used in the alkali washing is one of sodium hydroxide and potassium hydroxide.
[0014] Preferably, in step (4), the tempering temperature is 600-1000° C., and the tempering time is 2-10 h.
[0015] Preferably, the particle size of the hard carbon powder is 0.5-100 μm.
[0016] Another aspect of the present invention provides an application of the hard carbon negative electrode prepared by the above preparation method in a sodium ion battery.
[0017] The beneficial effects of the present invention are:
[0018] The present invention discloses a preparation method and application of a papermaking black liquor-based hard carbon negative electrode. The papermaking black liquor is dried and crushed to obtain black liquor powder, and then calcined, pickled, alkali washed, tempered and other steps are performed to convert the papermaking black liquor into a sodium ion battery hard carbon negative electrode with high value. On the one hand, organic matter such as cellulose, lignin, hemicellulose and the like present in the papermaking black liquor can be used as a carbon source, and hard carbon powder can be obtained after high-temperature calcination. On the other hand, metal salts such as sodium, potassium, and iron in the papermaking black liquor can be evenly distributed in the black liquor carbon as a pore-forming agent during calcination, effectively improving the porosity of the black liquor porous carbon, providing abundant sodium storage sites for sodium ions, and heteroatom doping can effectively improve the conductivity and improve the capacity of the hard carbon negative electrode. The invention can effectively solve the pollution problem of papermaking black liquor, while realizing the high-value utilization of papermaking black liquor and reducing battery costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a scanning electron microscope image of the sample prepared in Comparative Example 1;
[0020] Figure 2 This is a sample cycle efficiency diagram obtained in Comparative Example 1;
[0021] Figure 3 This is a scanning electron microscope image of the sample prepared in Example 1;
[0022] Figure 4 This is a sample cycle efficiency diagram obtained in Example 1;
[0023] Figure 5 This is a scanning electron microscope image of the sample prepared in Example 2;
[0024] Figure 6 This is a sample cycle efficiency diagram obtained in Example 2;
[0025] Figure 7 This is a scanning electron microscope image of the sample obtained in Example 3;
[0026] Figure 8 This is the sample cycle efficiency diagram obtained in Example 3. DETAILED DESCRIPTION
[0027] The present invention is described in detail below through specific embodiments.
[0028] Unless otherwise specified, the materials used in the embodiments of the present invention can be obtained through commercial channels or prepared according to conventional methods well known to those skilled in the art.
[0029] Comparative Example 1
[0030] (1) crushing dried coconut shells using a crusher to obtain coconut shell fine powder;
[0031] (2) calcining the coconut shell fine powder in a tubular furnace at 900° C. in a nitrogen atmosphere for 10 h to obtain coconut shell carbon powder;
[0032] (3) washing the obtained coconut shell carbon powder with hydrochloric acid, centrifuging, washing with sodium hydroxide, centrifuging, and washing with deionized water until the pH value is 7;
[0033] (4) The treated coconut shell carbon powder was calcined at 800°C for 5 h in a tube furnace and ball milled to obtain hard carbon powder.
[0034] like Figure 1 As shown, the hard carbon powder prepared in Comparative Example 1 is irregular in shape, with a particle size distribution mainly concentrated in the range of 50-300 μm and a specific surface area of 20 m 2 / g, pore size distribution is 500nm-1μm. Figure 2 As shown, the first coulombic efficiency is 68%, the first capacity is 250 mAh / g, and it decays to 150 mAh / g after 300 times.
[0035] Example 1
[0036] (1) drying the papermaking black liquor in a forced air oven at 80° C. for 15 h, crushing and grinding the obtained solid product after drying to obtain black liquor powder;
[0037] (2) calcining the black liquor powder in a tubular furnace at 900° C. in a nitrogen atmosphere for 10 h to obtain black liquor carbon powder;
[0038] (3) washing the obtained black liquor carbon powder with hydrochloric acid, centrifuging, washing with sodium hydroxide, centrifuging, washing with deionized water to pH=7, and drying;
[0039] (4) The treated black liquor carbon powder was calcined at 800° C. for 5 h in a tube furnace and ball milled to obtain hard carbon powder.
[0040] like Figure 3 As shown, the hard carbon powder prepared in Example 1 is irregular in shape, with a particle size distribution mainly concentrated in the range of 10-100 μm and a specific surface area of 500 m 2 / g, pore size distribution is 2-10nm. Figure 4 As shown, the first coulombic efficiency is 86% and the capacity is stable at 300mAh / g.
[0041] Example 2
[0042] (1) drying the papermaking black liquor in a blast oven at 100° C. for 10 h, crushing and grinding the obtained solid product after drying to obtain black liquor powder;
[0043] (2) calcining the black liquor powder in a tubular furnace at 1200° C. in a nitrogen atmosphere for 10 h to obtain black liquor carbon powder;
[0044] (3) washing the obtained black liquor carbon powder with sulfuric acid, filtering, washing with potassium hydroxide, filtering, washing with deionized water to pH=7, and drying;
[0045] (4) The treated black liquor carbon powder was calcined at 800° C. for 15 h in a tube furnace and ball milled to obtain hard carbon powder.
[0046] like Figure 5 As shown in the figure, the prepared hard carbon powder is irregular in shape, with a particle size distribution mainly concentrated in the range of 10-80 μm and a specific surface area of 350 m 2 / g, pore size distribution is 5-15nm. Figure 6 As shown, the first coulombic efficiency is 85% and the capacity is stable at 330 mAh / g.
[0047] Example 3
[0048] (1) drying the papermaking black liquor in a forced air oven at 120° C. for 5 h, crushing and grinding the obtained solid product after drying to obtain black liquor powder;
[0049] (2) calcining the black liquor powder in a tubular furnace at 1600° C. in a nitrogen atmosphere for 10 h to obtain black liquor carbon powder;
[0050] (3) washing the obtained black liquor carbon powder with nitric acid, filtering, washing with sodium hydroxide, filtering, washing with deionized water to pH=7, and drying;
[0051] (4) The treated black liquor carbon powder was calcined at 800° C. for 5 h in a tube furnace and ball milled to obtain hard carbon powder.
[0052] like Figure 7 As shown in the figure, the prepared hard carbon powder is irregular in shape, with a particle size distribution mainly concentrated in the range of 10-50 μm and a specific surface area of 150 m 2 / g, pore size distribution is 10-20nm. Figure 8 As shown, the first coulombic efficiency is 90% and the capacity is stable at 300mAh / g.
[0053] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the implementation methods. The protection scope of the present invention shall be subject to the scope defined by the claims. Other different forms of changes or modifications may be made based on the above description. Obvious changes or modifications derived therefrom are still within the protection scope of the present invention.
Claims
1. A method for preparing a papermaking black liquor-based hard carbon negative electrode, characterized in that: The method comprises the following steps: (1) drying and crushing the papermaking black liquor to obtain papermaking black liquor powder; (2) calcining the papermaking black liquor powder at high temperature to obtain black liquor carbon powder; (3) The black liquor carbon powder is acid-washed and alkaline-washed to remove impurities, and then washed with water until neutral; (4) The black liquor carbon powder after impurities removal is subjected to high temperature tempering to obtain hard carbon powder.
2. The method for preparing a papermaking black liquor-based hard carbon negative electrode according to claim 1, characterized in that: In step (1), the drying temperature is 80-150° C. and the time is 5-15 hours.
3. The method for preparing a papermaking black liquor-based hard carbon negative electrode according to claim 1, characterized in that: In step (2), the calcination temperature is 800-1600° C., and the calcination time is 2-20 hours.
4. The method for preparing a papermaking black liquor-based hard carbon negative electrode according to claim 1, characterized in that: In step (3), the acid used in the pickling is one or a combination of sulfuric acid, hydrochloric acid, and nitric acid, and the alkali used in the alkali washing is one of sodium hydroxide and potassium hydroxide.
5. The method for preparing a papermaking black liquor-based hard carbon negative electrode according to claim 1, characterized in that: In step (4), the tempering temperature is 600-1000° C. and the tempering time is 2-10 h.
6. The method for preparing a papermaking black liquor-based hard carbon negative electrode according to claim 1, characterized in that: The particle size of the hard carbon powder is 0.5-100 μm.
7. Use of a hard carbon negative electrode prepared by the preparation method according to any one of claims 1 to 6 in a sodium ion battery.
Citation Information
Patent Citations
Active carbon of produced by concentration carbonization papermaking pulping black liquor
CN101045535A
Porous carbon material, and preparation method and application thereof
CN106185920A
Preparation method for papermaking black liquid-transferred porous carbon negative electrode material for sodium ion battery
CN107452960A
Sulfur-doped porous carbon, method for preparing sulfur-doped porous carbon from eucalyptus black liquor and application
CN111977647A
Preparation method and application of hard carbon negative electrode material
CN116081599A
Cited By
Preparation method of bio-based spherical porous carbon, preparation method of bio-based spherical silicon-carbon negative electrode material and battery
CN119750575A