Hard carbon material, negative plate, preparation method of negative plate and sodium ion battery
By modifying lignin and nitrogen doping modification, combined with the pre-sodium agent Na3PO4 sintering treatment, nitrogen-modified pre-sodium porous hard carbon material was prepared, which solved the specific capacity and efficiency of hard carbon material in sodium ion batteries. The problem of low achieves high capacity and high first-time Coulomb efficiency sodium storage performance.
Patent Information
- Application Number
- CN202410951105.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-05
AI Technical Summary
The specific capacity and first-time Coulomb efficiency of existing hard carbon materials in sodium ion batteries are low, which cannot meet commercial needs. Moreover, the layer spacing of biomass-based hard carbons is small and the active sites are few, resulting in unfavorable storage of sodium ion intercalation.
By modifying lignin, combining melamine and polyvinyl alcohol for hydrothermal reaction, introducing nitrogen doping modification, and sintering with presodium agent Na3PO4, nitrogen-modified presodium porous hard carbon material is prepared, and the nitrogen-modified presodium-modified porous hard carbon material is added. Layer spacing and pore structure improve sodium ion transport.
It significantly improves the specific capacity of hard charcoal materials and the first-time Coulomb efficiency, improves the charging and discharging performance and cycle life of sodium ion batteries, and meets the high first-term efficiency and high energy density requirements of sodium ion batteries.
Smart Images

Figure CN118894518A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of batteries, and in particular relates to a hard carbon material, a negative electrode sheet and a preparation method thereof, and a sodium ion battery. Background Art
[0002] At present, sodium-ion batteries have become the most promising candidate to replace lithium-ion batteries due to their abundant sodium resources and low cost. The development and optimization of high-performance electrode materials for sodium-ion batteries is the key to the development of sodium-ion batteries. Among them, hard carbon negative electrode materials with larger interlayer spacing have become the most likely materials for commercialization. Hard carbon precursors mainly include polymer resins, biomass, and carbohydrates.
[0003] The preparation process of polymer resin-based and carbohydrate-based hard carbon is lengthy and complicated, and the preparation cost is relatively high, which does not meet the low-cost requirements of sodium-ion batteries; biomass has become the most promising material for commercialization due to its cheap price and easy availability. However, the specific capacity and first coulombic efficiency of biomass-based hard carbon are relatively low.
[0004] Lignin is a renewable amorphous aromatized polymer that is low in price and environmentally friendly. Its sodium storage active sites and pore structure are conducive to the storage of sodium ions. However, the interlayer spacing (d 002 ) is too small to be conducive to sodium ion intercalation storage, and has fewer reversible active sites and more open pores, which results in a low specific capacity of hard carbon. However, in order to increase the specific capacity of hard carbon materials, after the hard carbon materials are modified by heteroatom doping, the introduced active functional groups / active sites are very likely to undergo more side reactions with the electrolyte, resulting in a decrease in the first coulombic efficiency of hard carbon, which cannot meet the requirements of high first efficiency of commercial sodium ion batteries. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a hard carbon material, a negative electrode sheet and a preparation method thereof, and a sodium ion battery.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a hard carbon material comprises the following steps: 1) modifying lignin to obtain modified lignin; 2) subjecting the modified lignin to a hydrothermal reaction with melamine and polyvinyl alcohol to obtain a nitrogen-doped lignin-based carbon material; 3) mixing the lignin-based carbon material with a pre-sodium agent and subjecting the mixture to a sintering treatment to finally obtain a nitrogen-modified pre-sodium porous hard carbon material.
[0008] The specific steps of step 1) are: dissolving lignin in an alkaline solution, stirring at 20-50° C. for 2-5 hours to obtain modified lignin; the lignin after alkaline treatment can produce more free chemical bonds, which is beneficial to the subsequent cross-linking grafting reaction with melamine to obtain a lignin-melamine-polyvinyl alcohol composite, which is beneficial to increasing the nitrogen doping rate of the carbon-based material, and at the same time, it is beneficial to inhibit the decomposition loss of nitrogen elements during subsequent high-temperature sintering.
[0009] Preferably, the lignin includes one or more of lignin with a p-hydroxyphenylpropane structure, lignin with a guaiacylphenylpropane structure, and lignin with a syringylphenylpropane structure.
[0010] Preferably, the alkaline solution includes one or more of sodium hydroxide, sodium bicarbonate, and ammonium bicarbonate;
[0011] Preferably, the concentration of the alkaline solution is 1-10 mol / L;
[0012] Preferably, the mass ratio of the lignin in the alkaline solution is 5-40%.
[0013] In step 2), the hydrothermal reaction temperature is 90-150° C., and the reaction time is 2-8 hours. Preferably, after the hydrothermal reaction, the nitrogen-doped lignin-based carbon material is washed with ethanol and deionized water and then dried.
[0014] In step 2), the mass ratio of modified lignin: melamine: polyvinyl alcohol is (10-20): (1-10): (0.5-2); preferably, the mass ratio of modified lignin: melamine: polyvinyl alcohol is 15: (1.5-4): 1, more preferably 15: (2.8-3.2): 1;
[0015] Melamine can introduce a large number of nitrogen-containing functional groups into the lignin hard carbon structure, which is beneficial to increase the interlayer spacing, increase the sodium storage active sites and defect sites, and at the same time improve the ionic and electronic conductivity of lignin-based hard carbon materials.
[0016] In step 3), the pre-sodium agent is Na3PO4; preferably, the amount of the pre-sodium agent added relative to the lignin-based carbon material is 4-20wt%; more preferably 7.5wt%.
[0017] During the sintering process of the pre-sodium agent Na3PO4 with nitrogen-doped modified lignin-based carbon materials, the phosphate and carbon functional groups decompose together to produce gas and then volatilize, resulting in the production of corresponding micro / mesoporous structures in the hard carbon structure. The introduced pore structure can serve as a transmission channel, which is beneficial to the transmission and diffusion of sodium ions, thereby improving the rate performance of lignin-based hard carbon materials.
[0018] The sintering process in step 3) includes a pre-carbonization process and a high-temperature carbonization process;
[0019] Preferably, the pre-carbonization step is: heating to 300-600°C, heating rate 0.5-3°C / min, and holding time 1-3h.
[0020] Preferably, the high temperature carbonization process: heating to 900-1800°C, heating rate 1-5°C / min, holding time 2-5h;
[0021] Preferably, the inert atmosphere includes one or more of nitrogen, argon, and a hydrogen-argon mixture.
[0022] The present invention also includes a negative electrode sheet, comprising the hard carbon material obtained by the preparation method, a binder, and a conductive agent.
[0023] The binder is one or more of PVDF, SBR, CMC and PTFE;
[0024] The conductive agent is one or more of conductive carbon black, conductive graphite, carbon nanotubes, carbon nanofibers, and graphene.
[0025] The present invention also includes a method for preparing the negative electrode sheet, comprising the following steps: mixing hard carbon material, a binder, a conductive agent and water to obtain a negative electrode active slurry, coating the negative electrode current collector, preferably copper foil, and drying the mixture.
[0026] The present invention also includes a sodium ion battery, comprising the negative electrode sheet.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The technical solution of the present application provides a hard carbon material, a negative electrode sheet and a preparation method thereof, and a sodium ion battery to meet the practical application requirements of electrode materials. The hard carbon material selects lignin as a carbon precursor, melamine as a nitrogen source modifier, and adds Na3PO4 as a pre-sodium agent and activator, and polyvinyl alcohol as a cross-linking agent and activator, and finally obtains a nitrogen-modified pre-sodium porous hard carbon material.
[0029] The nitrogen-doped lignin-based hard carbon material has a larger graphite-like interlayer spacing, which is conducive to the rapid intercalation and storage of more sodium ions, significantly improving the platform capacity; the irreversible active sites in the pre-sodium treated hard carbon are reduced, which significantly improves the first efficiency of the hard carbon material, thus helping to improve the first efficiency, energy density and cycle life of the full battery; the porous structure introduced due to decomposition during the sintering process of the pre-sodium agent and lignin can provide more transmission channels, which is conducive to the rapid diffusion and transmission of sodium ions within the hard carbon material; polyvinyl alcohol will decompose during carbonization at a lower temperature, introducing more micro / mesoporous structures inside the hard carbon material.
[0030] The hard carbon obtained by direct carbonization of lignin without any modification has a high proportion of capacity in the slope area of the charge-discharge curve, high irreversible capacity, and low first coulombic efficiency; while the charge-discharge curve of the porous hard carbon after nitrogen doping modification and pre-sodiumization shows the typical characteristics of a high voltage slope area (above 0.1V) and a low voltage platform area (0.1-0V), and the proportion of capacity in the platform area is significantly increased, and the first coulombic efficiency is significantly improved. By controlling the addition ratio of the nitrogen source and the pre-sodium agent, the active sites and interlayer spacing can be regulated, and the high first efficiency and high specific capacity sodium storage performance of the lignin-based hard carbon material can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a charge and discharge curve diagram of a battery prepared using the hard carbon material of Example 1 of the present invention. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.
[0033] Example 1
[0034] 1. A method for preparing a hard carbon material, comprising the following steps:
[0035] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder into the sodium hydroxide solution, put it into a 40°C water bath and heat it with magnetic stirring for 3 h to obtain lignin pretreatment solution A, which is the modified lignin.
[0036] 2) Add 2.8 g of melamine and 1 g of polyvinyl alcohol to the lignin pretreatment solution A, continue to stir thoroughly, and then transfer to a polytetrafluoroethylene hydrothermal tank; put the polytetrafluoroethylene hydrothermal tank into a 120°C high-temperature oven and let it stand for 4 hours, take it out and naturally cool it to room temperature, wash and dry the reaction product to obtain a nitrogen-doped carbon material B, which is a nitrogen-doped modified lignin-based carbon material.
[0037] 3) Take 20g of nitrogen-doped carbon material B and mix it with 1.5g of pre-sodium agent Na3PO4, then put it into a ball mill for thorough ball milling at a speed of 150r / min and a ball milling time of 1h; put the ball-milled mixture into a tubular furnace and heat it at a temperature program of 2℃ / min to 500℃ and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h, wait for it to cool to room temperature, wash it with ethanol and deionized water after the reaction, and then dry it to obtain a nitrogen-doped modified lignin-based carbon material, and obtain the final product, a nitrogen-modified pre-sodium porous hard carbon material.
[0038] 2. Preparation of sodium ion battery: 3.2g nitrogen-modified pre-sodium porous hard carbon material was mixed with 0.4g binder (CMC) and 0.4g conductive agent Super-P to form a water-based slurry, which was evenly coated on copper foil. After drying in an oven at 120°C for 12h, the negative electrode was punched into a 13mm diameter disc. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0MNaPF6 (EC / DEC=1:1 volume ratio), and the separator was glass fiber (GF / F). The battery was assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester. The test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V. Figure 1 The charge and discharge curve is shown.
[0039] Example 2
[0040] 1. A method for preparing a hard carbon material, comprising the following steps:
[0041] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder into the sodium hydroxide solution, put it into a 40°C water bath and heat it with magnetic stirring for 3 h to obtain lignin pretreatment solution A, which is the modified lignin.
[0042] 2) Add 4 g of melamine and 1 g of polyvinyl alcohol to the lignin pretreatment solution A, continue to stir thoroughly, and then transfer to a polytetrafluoroethylene hydrothermal tank; put the polytetrafluoroethylene hydrothermal tank into a 120°C high-temperature oven and let it stand for 4 hours, take it out and naturally cool it to room temperature, wash and dry the reaction product to obtain a nitrogen-doped carbon material B, which is a nitrogen-doped modified lignin-based carbon material.
[0043] 3) Take 20g of nitrogen-doped carbon material B and mix it with 1.5g of pre-sodium agent Na3PO4, then put it into a ball mill for thorough ball milling at a speed of 150r / min and a ball milling time of 1h; put the ball-milled mixture into a tubular furnace and heat it at a temperature program of 2℃ / min to 500℃ and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h, wait for it to cool to room temperature, wash it with ethanol and deionized water after the reaction, and then dry it to obtain a nitrogen-doped modified lignin-based carbon material, and obtain the final product, a nitrogen-modified pre-sodium porous hard carbon material.
[0044] 2. Preparation of sodium ion battery: 3.2g nitrogen-modified pre-sodium porous hard carbon material was mixed with 0.4g binder (CMC) and 0.4g conductive agent Super-P to form a water-based slurry, which was evenly coated on copper foil. After drying in an oven at 120°C for 12h, the negative electrode was punched into a 13mm diameter disc. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0MNaPF6 (EC / DEC=1:1 volume ratio), and the separator was glass fiber (GF / F). The battery was assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester. The test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V. Figure 1 The charge and discharge curve is shown.
[0045] Example 3
[0046] 1. A method for preparing a hard carbon material, comprising the following steps:
[0047] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder to the sodium bicarbonate solution, place in a 40°C water bath and stir magnetically for 5 h to obtain lignin pretreatment solution A, which is the modified lignin.
[0048] 2) Add 1.5 g of melamine and 1 g of polyvinyl alcohol to the lignin pretreatment solution A, continue to stir thoroughly, and then transfer to a polytetrafluoroethylene hydrothermal tank; put the polytetrafluoroethylene hydrothermal tank into a 120°C high-temperature oven and let it stand for 4 hours, take it out and naturally cool it to room temperature, wash and dry the reaction product to obtain a nitrogen-doped carbon material B, which is a nitrogen-doped modified lignin-based carbon material.
[0049] 3) Take 20g of nitrogen-doped carbon material B and mix it with 1.5g of pre-sodium agent Na3PO4, then put it into a ball mill for thorough ball milling at a speed of 150r / min and a ball milling time of 1h; put the ball-milled mixture into a tubular furnace and heat it at a temperature program of 2℃ / min to 500℃ and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h, and wait for it to cool to room temperature to obtain the final product, nitrogen-modified pre-sodium porous hard carbon material.
[0050] 2. Preparation of sodium ion battery for testing: (4) 3.2g of nitrogen-modified pre-sodium porous hard carbon material was mixed with 0.4g of binder (CMC) and 0.4g of conductive agent Super-P to form an aqueous slurry, which was evenly coated on copper foil. After drying in an oven at 120℃ for 12h, the negative electrode was punched into a 13mm diameter disc. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0M NaPF6 (EC / DEC=1:1 volume ratio), and the separator was glass fiber (GF / F). The battery was assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester with a current density of 20mA / g and a voltage range of 0 to 2.5V for charge and discharge tests.
[0051] Example 4
[0052] 1. A method for preparing a hard carbon material, comprising the following steps:
[0053] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder to the ammonium bicarbonate solution, put it in a 40°C water bath and stir it magnetically for 5 hours to obtain lignin pretreatment solution A, which is the modified lignin.
[0054] 2) Add 3.2 g of melamine and 1 g of polyvinyl alcohol to the lignin pretreatment solution A, continue to stir thoroughly, and then transfer to a polytetrafluoroethylene hydrothermal tank; put the polytetrafluoroethylene hydrothermal tank into a 120°C high-temperature oven and let it stand for 4 hours, take it out and naturally cool it to room temperature, wash and dry the reaction product to obtain a nitrogen-doped carbon material B, which is a nitrogen-doped modified lignin-based carbon material.
[0055] 3) Take 20g of nitrogen-doped carbon material B and mix it with 1.5g of pre-sodium agent, then put it into a ball mill for thorough ball milling at a speed of 150r / min and a ball milling time of 1h; put the ball-milled mixture into a tubular furnace and heat it at a temperature program of 2℃ / min to 500℃ and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h, and wait for it to cool to room temperature to obtain the final product, nitrogen-modified pre-sodium porous hard carbon material.
[0056] 2. Preparation of the test sodium ion battery: 3.2g of nitrogen-modified pre-sodium porous hard carbon material was mixed with 0.4g of binder (CMC) and 0.4g of conductive agent Super-P to form an aqueous slurry, which was evenly coated on copper foil. After drying in an oven at 120°C for 12h, the negative electrode was punched into a 13mm diameter disc. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0MNaPF6 (EC / DEC=1:1 volume ratio), and the separator was glass fiber (GF / F), and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V.
[0057] Example 5
[0058] 1. A method for preparing a hard carbon material, comprising the following steps:
[0059] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder into the sodium hydroxide solution, put it into a 40°C water bath and stir it magnetically for 5 hours to obtain lignin pretreatment solution A, which is the modified lignin.
[0060] 2) Add 2.8 g of melamine and 1 g of polyvinyl alcohol to the lignin pretreatment solution A, continue to stir thoroughly, and then transfer to a polytetrafluoroethylene hydrothermal tank; put the polytetrafluoroethylene hydrothermal tank into a 120 high-temperature oven and let it stand for 4 hours, take it out and naturally cool it to room temperature, wash and dry the reaction product to obtain a nitrogen-doped carbon material B, which is a nitrogen-doped modified lignin-based carbon material.
[0061] 3) Take 20g of nitrogen-doped carbon material B and mix it with 0.8g of pre-sodium agent, then put it into a ball mill for thorough ball milling at a speed of 150r / min and a ball milling time of 1h; put the ball-milled mixture into a tubular furnace and heat it at a temperature program of 2℃ / min to 500℃ and keep it warm for 2h; then heat it to 1300℃ at 5℃ / min and keep it warm for 2h, and wait for it to cool to room temperature to obtain the final product, nitrogen-modified pre-sodium porous hard carbon material.
[0062] 2. Preparation of the test sodium ion battery: 3.2g of nitrogen-modified pre-sodium porous hard carbon material was mixed with 0.4g of binder (CMC) and 0.4g of conductive agent Super-P to form an aqueous slurry, which was evenly coated on copper foil. After drying in an oven at 120°C for 12h, the negative electrode was punched into a 13mm diameter disc. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0MNaPF6 (EC / DEC=1:1 volume ratio), and the separator was glass fiber (GF / F), and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V.
[0063] Embodiment 6:
[0064] 1. The preparation method of hard carbon material comprises the following steps:
[0065] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder into the sodium hydroxide solution, put it into a 40°C water bath and heat it with magnetic stirring for 3 h to obtain lignin pretreatment solution A, which is the modified lignin.
[0066] 2) Add 2.8 g of melamine and 1 g of polyvinyl alcohol to the lignin pretreatment solution A, continue to stir thoroughly, and then transfer to a polytetrafluoroethylene hydrothermal tank; put the polytetrafluoroethylene hydrothermal tank into a 150°C high-temperature oven and let it stand for 2 hours, take it out and naturally cool it to room temperature, wash and dry the reaction product to obtain a nitrogen-doped carbon material B, which is a nitrogen-doped modified lignin-based carbon material.
[0067] 3) Take 20g of nitrogen-doped carbon material B and mix it with 4g of pre-sodium agent Na3PO4, then put it into a ball mill for thorough ball milling at a rotation speed of 150r / min and a ball milling time of 1h; put the ball-milled mixture into a tubular furnace and heat it at a temperature program of 2℃ / min to 500℃ and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h, and wait for it to cool to room temperature to obtain the final product, nitrogen-modified pre-sodium porous hard carbon material.
[0068] 2. Preparation of sodium ion battery: 3.2g of nitrogen-modified pre-sodium porous hard carbon material was mixed with 0.4g of binder (CMC) and 0.4g of conductive agent Super-P to form a water-based slurry, which was evenly coated on copper foil. After drying in an oven at 120°C for 12h, the sheets were punched into 13mm diameter discs. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0M NaPF6 (EC / DEC=1:1 volume ratio), and the separator was glass fiber (GF / F), and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, with a current density of 20mA / g and a voltage range of 0-2.5V for charge and discharge tests.
[0069] Comparative Example 1:
[0070] 1. A method for preparing a hard carbon material (compared with Example 1, excluding melamine and polyvinyl alcohol), comprising the following steps:
[0071] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder into the sodium hydroxide solution, put it into a 40°C water bath and heat it with magnetic stirring for 3 h to obtain lignin pretreatment solution A, which is the modified lignin.
[0072] 2) The lignin pretreatment solution was transferred to a polytetrafluoroethylene hydrothermal tank; the polytetrafluoroethylene hydrothermal tank was placed in a 120° C. high-temperature oven for 4 hours, and then naturally cooled to room temperature after being taken out. The reaction product was washed and dried to obtain carbon material B.
[0073] 3) Take 20g of carbon material B and 1.5g of pre-sodium agent Na3PO4, mix them and put them into a ball mill for thorough ball milling at a speed of 150r / min and a ball milling time of 1h; put the ball-milled mixture into a tubular furnace and heat it at a temperature program of 2℃ / min to 500℃ and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h, and wait for it to cool to room temperature to obtain the final product, a pre-sodiumized porous hard carbon material.
[0074] 2. Preparation of sodium ion battery: 3.2g pre-sodiumized porous hard carbon material, 0.4g binder (CMC), 0.4g conductive agent Super-P mixed water slurry was evenly coated on copper foil, and then punched into 13mm diameter discs after drying in an oven at 120℃ for 12h. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0M NaPF6 (EC / DEC=1:1 volume ratio), and the diaphragm was glass fiber (GF / F), and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V.
[0075] Comparative Example 2
[0076] 1. A method for preparing a hard carbon material (compared with Example 1, excluding the pre-sodium agent Na3PO4), comprising the following steps:
[0077] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder into the sodium hydroxide solution, put it into a 40°C water bath and heat it with magnetic stirring for 3 h to obtain lignin pretreatment solution A, which is the modified lignin.
[0078] 2) Add 2.8 g of melamine and 1 g of polyvinyl alcohol to the lignin pretreatment solution A, continue to stir thoroughly, and then transfer to a polytetrafluoroethylene hydrothermal tank; put the polytetrafluoroethylene hydrothermal tank into a 120°C high-temperature oven and let it stand for 4 hours, take it out and naturally cool to room temperature, wash and dry the reaction product to obtain nitrogen-doped carbon material B.
[0079] 3) Take 20g of nitrogen-doped carbon material B and put it into a tubular furnace for heating. The heating program is to heat it to 500℃ at 2℃ / min and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h. After cooling to room temperature, the final product, nitrogen-modified hard carbon material, is obtained.
[0080] 2. Preparation of sodium ion battery: 3.2g nitrogen-modified hard carbon material, 0.4g binder (CMC), 0.4g conductive agent Super-P mixed water slurry was evenly coated on copper foil, and then punched into 13mm diameter discs after drying in an oven at 120℃ for 12h. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0MNaPF6 (EC / DEC=1:1 volume ratio), and the diaphragm was glass fiber (GF / F), and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V.
[0081] Comparative Example 3
[0082] 1. A method for preparing a hard carbon material (compared with Example 1, excluding melamine, polyvinyl alcohol and pre-sodium agent Na3PO4), comprising the following steps:
[0083] 1) Pour 200 mL of 2 mol / L sodium hydroxide solution into a beaker, then add 15 g of sodium lignin sulfonate powder into the sodium hydroxide solution, put it into a 40°C water bath and heat it with magnetic stirring for 3 h to obtain lignin pretreatment solution A, which is the modified lignin.
[0084] 2) The lignin pretreatment solution A is transferred to a polytetrafluoroethylene hydrothermal tank; the polytetrafluoroethylene hydrothermal tank is placed in a 120°C high-temperature oven for 4 hours, and then naturally cooled to room temperature after being taken out. The reaction product is washed and dried to obtain a hydrothermal carbon material B, which is a nitrogen-doped lignin-based carbon material.
[0085] 3) Take 20g of hydrothermal carbon material B and put it into a tubular furnace for heating. The heating program is to heat it to 500℃ at 2℃ / min and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h. After cooling to room temperature, the final product hard carbon material is obtained.
[0086] 2. Preparation of sodium ion battery test: 3.2g hard carbon material, 0.4g binder (CMC), 0.4g conductive agent Super-P mixed water slurry was evenly coated on copper foil, and after drying in an oven at 120℃ for 12h, the sheet was punched into a 13mm diameter disc. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0MNaPF6 (EC / DEC=1:1 volume ratio), and the diaphragm was glass fiber (GF / F), and assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester, the test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V. Table 1 shows the performance test data of different embodiments and comparative materials.
[0087] Comparative Example 4
[0088] 1. A method for preparing a hard carbon material, comprising the following steps: (Compared with Example 1, the lignin is not subjected to alkaline treatment)
[0089] 1) Take 15 g of sodium lignin sulfonate powder and dissolve it in 200 mL of deionized water, put it in a 40° C. water bath and heat it with magnetic stirring for 3 h to obtain lignin pretreatment solution A, which is the modified lignin.
[0090] 2) Add 2.8 g of melamine and 1 g of polyvinyl alcohol to the lignin pretreatment solution A, continue to stir thoroughly, and then transfer to a polytetrafluoroethylene hydrothermal tank; put the polytetrafluoroethylene hydrothermal tank into a 120°C high-temperature oven and let it stand for 4 hours, take it out and naturally cool it to room temperature, wash and dry the reaction product to obtain a nitrogen-doped carbon material B, which is a nitrogen-doped modified lignin-based carbon material.
[0091] 3) Take 20g of nitrogen-doped carbon material B and mix it with 1.5g of pre-sodium agent Na3PO4, then put it into a ball mill for thorough ball milling at a speed of 150r / min and a ball milling time of 1h; put the ball-milled mixture into a tubular furnace and heat it at a temperature program of 2℃ / min to 500℃ and keep it warm for 2h; then heat it to 1100℃ at 5℃ / min and keep it warm for 2h, wait for it to cool to room temperature, wash it with ethanol and deionized water after the reaction, and then dry it to obtain a nitrogen-doped modified lignin-based carbon material, and obtain the final product, a nitrogen-modified pre-sodium porous hard carbon material.
[0092] 2. Preparation of sodium ion battery: 3.2g nitrogen-modified pre-sodium porous hard carbon material was mixed with 0.4g binder (CMC) and 0.4g conductive agent Super-P to form a water-based slurry, which was evenly coated on copper foil. After drying in an oven at 120°C for 12h, the negative electrode was punched into a 13mm diameter disc. In a glove box filled with argon, a metal sodium sheet was used as the counter electrode, the electrolyte was 1.0MNaPF6 (EC / DEC=1:1 volume ratio), and the separator was glass fiber (GF / F). The battery was assembled into a CR2032 button cell. At room temperature, the battery was tested using a blue battery tester. The test conditions were a current density of 20mA / g, and the voltage range of the charge and discharge test was 0-2.5V. Figure 1 The charge and discharge curve is shown.
[0093] Table 1
[0094]
[0095] According to the characterization results of the physical and chemical structure and electrochemical properties of the hard carbon materials in the embodiments in Table 1 above, it can be known that the higher the nitrogen content, the larger the interlayer spacing of the hard carbon material and the higher the disorder; when the proportion of the pre-sodium agent increases, the first coulombic efficiency and specific surface area of the hard carbon material increase; however, the nitrogen content and the pre-sodium agent content mixed in the hard carbon need to be controlled within a reasonable range. For example, if the mixed nitrogen content is too high, the specific surface area of the hard carbon will be too large, and it is easy to have more side reactions with the electrolyte, causing the first coulombic efficiency to decrease; if the pre-sodium agent mixing ratio is too low, it cannot provide enough sodium source to combine with all active sites in the hard carbon, and the purpose of improving the first efficiency cannot be achieved. Under the synergistic effect of the coupling of nitrogen doping modification and pre-sodiumization in an appropriate ratio, the method of the present invention prepares biomass-based hard carbon with high capacity and ultra-high first coulombic efficiency.
[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a hard carbon material, characterized in that: The method comprises the following steps: 1) performing modification treatment on lignin to obtain modified lignin; 2) The modified lignin is subjected to a hydrothermal reaction with melamine and polyvinyl alcohol to obtain a nitrogen-doped lignin-based carbon material; 3) The lignin-based carbon material is then mixed with a pre-sodium agent and subjected to a sintering treatment to finally obtain a nitrogen-modified pre-sodium porous hard carbon material.
2. The method for preparing a hard carbon material according to claim 1, characterized in that: The specific steps of step 1) are: dissolving lignin in an alkaline solution, stirring at 20-50° C. for 2-5 hours to obtain modified lignin; Preferably, the lignin includes one or more of lignin with a p-hydroxyphenylpropane structure, lignin with a guaiacylphenylpropane structure, and lignin with a syringylphenylpropane structure; Preferably, the alkaline solution includes one or more of sodium hydroxide, sodium bicarbonate, and ammonium bicarbonate; Preferably, the concentration of the alkaline solution is 1-10 mol / L; Preferably, the mass ratio of the lignin in the alkaline solution is 5-40%.
3. The method for preparing a hard carbon material according to claim 1, characterized in that: In step 2), the hydrothermal reaction temperature is 90-150° C. and the reaction time is 2-8 h; Preferably, after the hydrothermal reaction is completed, the lignin-based carbon material is washed with ethanol and deionized water and then dried to obtain a nitrogen-doped modified lignin-based carbon material.
4. The method for preparing a hard carbon material according to claim 1, characterized in that: In step 2), the mass ratio of modified lignin: melamine: polyvinyl alcohol is (10-20): (1-10): (0.5-2); Preferably, the mass ratio of modified lignin:melamine:polyvinyl alcohol is 15:(1.5-4):1, more preferably 15:(2.8-3.2):
1.
5. The method for preparing a hard carbon material according to claim 1, characterized in that: In step 3), the pre-sodium agent is Na3PO4; preferably, the amount of the pre-sodium agent added relative to the lignin-based carbon material is 4-20wt%, more preferably 7.5wt%.
6. The method for preparing a hard carbon material according to claim 1, characterized in that: The sintering process in step 3) includes a pre-carbonization process and a high-temperature carbonization process; Preferably, the pre-carbonization step is: heating to 300-600°C, heating rate 0.5-3°C / min, and holding time 1-3h. Preferably, the high temperature carbonization process: heating to 900-1800°C, heating rate 1-5°C / min, holding time 2-5h; Preferably, the inert atmosphere includes one or more of nitrogen, argon, and a hydrogen-argon mixture.
7. A negative electrode sheet, characterized in that: The invention comprises a hard carbon material obtained by the preparation method according to any one of claims 1 to 6, a binder, and a conductive agent.
8. The negative electrode sheet according to claim 7, characterized in that: The binder is one or more of PVDF, SBR, CMC and PTFE; The conductive agent is one or more of conductive carbon black, conductive graphite, carbon nanotubes, carbon nanofibers, and graphene.
9. A method for preparing a negative electrode sheet according to claim 7 or 8, characterized in that: The method comprises the following steps: mixing hard carbon material, a binder, a conductive agent and water to obtain a negative electrode active slurry, coating the negative electrode current collector, preferably copper foil, and drying the mixture.
10. A sodium ion battery, characterized in that: Including the negative electrode sheet as described in claim 7 or 8.