Precipitated silica-based matting agent
By using specific physicochemical parameters and preparation processes to precipitate silica, the issues of dosage and dispersibility of matting agents in paints have been resolved, achieving efficient matting effects and improved transparency while reducing the tendency for reaggregation.
Patent Information
- Application Number
- CN202410536568.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-05
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-05
AI Technical Summary
Existing matting agents are difficult to reduce in paint while maintaining the gloss level, transparency, and tactile properties, and fine particles are prone to reaggregation, resulting in poor dispersibility.
Precipitated silica with specific physicochemical parameters, including BET 150m²/g–400m²/g, DOA 220ml/100g–400ml/100g, d50 3.0μm–5.0μm, particle size ratio d5:d50:d95:>0.3:<2, and particle size distribution between 1.3 and 1.7, is prepared by spray drying and graded grinding, with preferred wax coating to improve dispersibility.
It reduces the amount of matting agent used, improves the transparency and dispersibility of the paint, reduces the tendency to reaggregate, and maintains the stability of the gloss level.
Smart Images

Figure CN118894533A_ABST
Abstract
Description
[0001] The invention relates to matting agents based on precipitated silica, a process for their preparation and their use in paints and coatings.
[0002] Coatings are applied to surfaces or substrates for decorative, functional or protective purposes. They decorate, protect and preserve materials such as wood, metal or plastic. Coatings can be high gloss or matte.
[0003] In the past, coatings such as paints and printing inks were subsequently matted by controlled roughening of the surface on a microscale. As a result, light incident on the roughened surface is not reflected in a directional manner, but diffusely scattered. The more diffusely the light is scattered, the more matte the surface appears to the human eye.
[0004] Nowadays, matting agents are used which are incorporated into paint systems. Matting agents usually consist of precipitated or fumed silica, silicone gels, polymethylureas or waxes. They are subject to many requirements. Thus, on the one hand, a good matting effect is required; on the other hand, they should not have an adverse effect on the tactile properties and / or transparency of the paint film surface. Furthermore, they should have good dispersibility in paint production.
[0005] It should be possible to give the paint film surface a soft matte (silky matt) to a dull matt appearance at various matting levels, but it should not look rough. Therefore, the roughness of the matte surface is also determined by the particle size and shape of the matting agent. In the case of a coarse matting agent, the paint film looks matte but rough.
[0006] Matting agents are based on the action of silica particles protruding from the surface, which form a microstructure when the paint system dries. Light is scattered in all directions at the resulting peaks and valleys. An established method for quantifying mattness / gloss is to measure the reflected light component at an angle of 60°.
[0007] Basically, coarse particles are easier to disperse than fine particles, because in the case of fine particles a much higher surface area must be wetted. In addition, fine particles have a much stronger tendency to reaggregate due to the high surface energy.
[0008] In order to avoid or reduce this tendency, which is particularly important in paint production, it is desirable to provide matting agents that can reduce the amount of matting agent used while maintaining the same gloss level without adversely affecting transparency, dispersion and / or tactile properties.
[0009] Therefore, the present invention provides precipitated silica characterized by the following physicochemical parameters:
[0010] BET: 150m2 / g–400m 2 / g, preferably 200m 2 / g–300m 2 / g, measured according to ISO 9277,
[0011] DOA: 220ml / 100g–400ml / 100g, preferably 250ml / 100g–350ml / 100g, measured according to ISO 19246,
[0012] d 50 : 3.0 μm–5.0 μm, measured by laser diffraction on a Coulter LS according to ISO 13320,
[0013] Particle size ratio d5:d 50 :d 95 :>0.3:1:<2,
[0014] Particle size distribution Between 1.3 and 1.7.
[0015] The median particle size of the precipitated silica according to the invention can be determined by laser diffraction particle size analysis in accordance with ISO 13320:2009. The resulting measured particle size distribution is used to define the median d 50 , which reflects the particle size that does not exceed 50% of all particles, as the average particle size.
[0016] The specific surface area, also referred to as BET surface area for short, is determined in accordance with DIN 9277:2014 by the Brunauer-Emmett-Teller method by nitrogen adsorption.
[0017] The DOA absorption value is determined with the aid of an absorptometer equipped with a torque measurement and handling system. It can be used to assess the liquid absorption capacity of silica, calcium silicate and sodium aluminosilicate. The daily absorption value indicates the carrier capacity of the filler.
[0018] Experience has shown that a larger amount of precipitated silica having a smaller particle size is required to achieve the same gloss level than precipitated silica having a larger particle size.
[0019] It has been found that, unexpectedly, the amount of precipitated silica according to the invention can be reduced compared to commercially available finely divided matting agents. For example, the amount in various paint systems can be reduced over a wide range of gloss levels measured at an angle of 60°. Reference is made here to the examples.
[0020] The reduced amount of precipitated silica used according to the invention also constitutes an important product property with regard to efficiency (economic viability). The more efficient the silica, the less silica is used in the corresponding paint system to achieve a defined gloss level.
[0021] In addition, it has been determined that the transparency of clearcoats can be increased. According to DIN 55988, the density Dy (transparency) of matted clearcoats was measured with an eXact densitometer from X-Rite. Here, matted clearcoats in different paint systems were applied to black PMMA sheets and various matting agents were compared by always adjusting the gloss level to the same gloss level measured at 60 ° considered in the specific case. The transparency was then determined by diffuse reflection at an angle of 45 ° via logarithmic calculation. The parameters for the measurement were set as follows:
[0022] parameter set up Measurement conditions M0(None): No filter Density state ISO Status E Density White Base Absolute All densities CMYK Density / tone value Solid color: CMYK Density / tone value Color: Hue value Tone Value / Spot SCTV (ISO20654) Light source / Observer D65 / 2° / 10°
[0023] It should be noted here that the transparency of matted clearcoat systems can only be compared with one another if the gloss level is the same. A comparison with the same dosage of silica is not permitted. The measured transparency value Dy is a logarithmic value. Therefore, the higher the Dy value, the more transparent the matted clearcoat.
[0024] The median pore size of the precipitated silica according to the invention is preferably less than 7.0 μm, preferably less than 5.0 μm, more preferably less than 3.0 μm, measured according to ISO 15901-1 with an Autopore IV 9520 with the following instrument settings: contact angle of 140° and pressure range of 0.003-420 MPa, and measured in the pore size range of 3.5 nm-500 μm, measured after grinding the silica.
[0025] The silicon dioxide according to the invention preferably has a unique morphology, especially its porosity, which can be demonstrated by mercury porosimetry.
[0026] The precipitated silica according to the invention preferably has a pore volume of 2.20 ml / g Hg (d=0.1 μm-d=3.0 μm)-2.90 ml / g Hg (d=0.1 μm-d=3.0 μm), determined by means of a Hg porosimeter.
[0027] The precipitated silica according to the invention preferably has a pore volume of 2.40 ml / g Hg (d=0.1 μm-d=4.0 μm)-3.10 ml / g Hg (d=0.1 μm-d=4.0 μm), determined by means of a Hg porosimeter.
[0028] The precipitated silica according to the invention preferably has a pore volume of 2.50 ml / g Hg (d=0.1 μm-d=5.0 μm)-3.30 ml / g Hg (d=0.1 μm-d=5.0 μm), determined by means of a Hg porosimeter.
[0029] The determination of the Hg pore size (d<4 μm or d<5 μm) is based on mercury intrusion according to DIN 66133 and uses an AutoPore V 9600 instrument from Micromeritics. The method principle is based on measuring the volume of mercury injected into a porous solid as a function of the applied pressure.
[0030] Figure 4 The diagram for the determination of the pore volume by means of an Hg porosimeter is shown. It shows, for example, the unique morphology of the silica K2 according to the invention. The vertical lines at d = 0.1 μm and d = 4.0 μm indicate the region specified according to the invention. The difference in the cumulative pore volume (ml / g) indicates the pore volume of this region (see Table C). For the calculation, the intersection of the respective vertical line with the diagram is read in each case and calculated.
[0031] Furthermore, it can be inferred from the graph that in the region of pore diameters d < 1 μm, the cumulative pore volume is 4.9 ml / g. For this purpose, a vertical dashed line is set at d = 1 μm. The value at the intersection with the graph can be read. In the case of pore volumes less than 4.9 ml / g, the graph would have a flatter progression and the silica particles would therefore have a smaller pore volume.
[0032] The silicas according to the invention have a much smaller average pore size than comparable commercial silicas used as matting agents. Despite the much smaller pore size, it was found that they can absorb more mercury. The higher number of average smaller pores brings crucial advantages in terms of transparency, especially in the case of water-based paint systems.
[0033] Figure 1 An SEM image of a varnish coating incorporating silica particles is shown in cross section. Due to the morphology or porosity of the silica, they behave like a sponge and are filled entirely with a transparent binder. Since the binder and silica have similar refractive indices, the matted varnish remains essentially transparent after drying.
[0034] Aqueous adhesives are dispersions of polymer particles in an aqueous phase. The diameter of the spherical polymer particles can be between a few tens of nanometers and a few micrometers. As the paint film dries, water and any cosolvents evaporate, which reduces the volume, and the dispersion begins to coagulate. The dispersed particles get closer and closer to each other and eventually begin to merge, which can be called coalescence. At the end of coalescence, a uniform adhesive film is formed, in which the particle boundaries of the adhesive have disappeared. The adhesive particles can effectively penetrate into many pores and form a film in the pores. The more pores there are, the more blurred the refractive index difference between silica and adhesive is, which leads to an increase in transparency, which has been found in the corresponding adhesive system according to the silica of the present invention.
[0035] The dispersibility of the precipitated silica according to the invention in various paint systems is also surprisingly improved. A grindometer can be used to indirectly determine the dispersibility. The determination with the grindometer is in accordance with DIN EN ISO 1524. It can be correlated with the speckle formation in the dry paint film, so that unwanted specks or oversizes can be identified with the aid of the grindometer. In addition, the tendency of the precipitated silica to reagglomerate can also be identified via this method, which generally increases with decreasing particle size distribution. Reference is here made to Figure 2 and Figure 3 .
[0036] In the case of many precipitated silicas with d50 values of less than 5 μm, the silica particles have a tendency to reaggregate during storage, which can be recognized over time by an increasing number of spots in the fineness meter image. In general, the reaggregation tendency of untreated silicas is higher than in the case of those with an organic coverage of the surface. In the case of silicas with a high reaggregation tendency, this may occur after a few days or, in the case of a higher stability, after a few weeks or months. In the case of the silicas according to the invention, on the other hand, this is not observed, thus confirming a very low tendency to spot formation. Without being bound by any theory, it is believed that the specific morphology and pore distribution of the silicas according to the invention not only have a favorable influence on the dispersibility, but also lead to a high stability against reaggregation.
[0037] The tamped density of various powdery or coarse-grained granular materials can be determined in accordance with DIN ISO 787-11:1995 "General methods of test for pigments and extenders--Part 11: Determination of tamped volume and apparent density after tamping". This involves measuring the bulk density of the bulk material after mixing and tamping.
[0038] For a uniform matting effect, a very narrow particle size distribution is the goal. The particle size distribution can be determined in a simple manner, for example by measuring the d5, d50 and d95 values. Thus, the particle size distribution (span) defined by the quotient (d95-d5):d50 of the untreated or wax-coated precipitated silica according to the invention is between 1.3 and 1.7.
[0039] Another property is also the particle size ratio d5:d 50 :d 95 .
[0040] The precipitated silica according to the invention preferably has a d value of 3.5-4.5 μm. 50 .
[0041] In addition to untreated hydrophilic silicas, it is also known to use wax-coated silicas as matting agents. Such wax treatments significantly improve the precipitation properties of precipitated silicas.
[0042] Therefore, the present invention further provides a wax-coated precipitated silica, characterized in that
[0043] BET: 150m 2 / g–400m 2 / g, preferably 200m 2 / g–300m 2 / g, measured according to ISO 9277,
[0044] DOA: 220ml / 100g–400ml / 100g, preferably 250ml / 100g–350ml / 100g, measured according to ISO 19246,
[0045] d 50 : 3.0 μm–5.0 μm, measured by laser diffraction (Coulter LS) according to ISO 13320,
[0046] Particle size ratio d5:d 50 :d95 :>0.3:1:<2,
[0047] Particle size distribution Between 1.3 and 1.7.
[0048] Carbon content: 1.0-6.0 wt. %, preferably 2.4-3.8 wt. %, determined by LECO according to ISO 3262-19.
[0049] The procedure for preparing the precipitated silica according to the invention is, for example, as follows.
[0050] At 50°C, under continuous stirring, the precipitation vessel was initially charged with 13.5 ml 3 of water, with 14.85m 3 / h rate to add commercial water glass, and the addition is completed after 10-15 minutes. Subsequently, the mixture is heated to a temperature of 70°C. Then, in 25-35 minutes, 0.27m 3 96% sulfuric acid was added at 1 0.5 % sulphuric acid / h with constant shearing and stirring, and the temperature was maintained at 85°C by closed loop control. After a period of 1.5 to 3.5 hours, the suspension was acidified with sulfuric acid over 50-80 minutes until the pH was in the range of 3.5 to 3.9.
[0051] Solids can be separated from the suspension by known filtering operations, such as filter presses (membrane filter presses). The filter cake washed with demineralized water should then be dried. For this purpose, many drying methods are known to those skilled in the art (Ullmann's Encyclopedia of industrial chemistry, 1992, 5th edition, volume B1, pages 7-25). It has been found that advantageous drying operations are those with the aid of a flow dryer, a spray dryer, a layered dryer (Etagentrockner), a belt dryer, a rotary tube dryer, a rotary flash dryer or a nozzle tower. Drying is more preferably carried out by a spray dryer or a layered dryer.
[0052] For drying by spray drying, the filter cake is liquefied with water under the effect of shear forces and adjusted to a solids content of <15%, preferably 7.0-14.0%, more preferably 9-12%.
[0053] The precipitated silica obtained after drying can be subjected to direct classifying grinding, or the silica according to the invention can also be coated with wax simultaneously during classifying grinding, in which case a coating with 2-15 wt. %, preferably 5-10 wt. %, more preferably 3-6 wt. % has been found to be useful.
[0054] Besides the wax impregnation of silicon dioxide mentioned, other processes are also known for this and can be found, for example, in DE 1006 100, DE 1592 865 or EP 0922 691. The wax suspension is reacted here with the silicon dioxide suspension, optionally with the aid of a dispersant.
[0055] In order to obtain the desired narrow particle size distribution of precipitated silica and the desired d of 3.0-5.0 μm 50 The classifying grinding operation is carried out using a conventional air jet mill such as a Netzsch CGS 50.
[0056] The untreated or waxed precipitated silicas according to the invention can be used as matting agents in paints or coatings. In particular, they can be used to prepare dispersions, millbases, paints, coatings or printing inks, inkjet inks, grinding resins, pigment concentrates, colour preparations, pigment preparations, filler preparations or coating compositions.
[0057] The following examples are intended to further illustrate the present invention, but are not intended to limit the scope of protection described in the claims:
[0058] method
[0059] The tapped density [g / l] is determined in accordance with DIN ISO 787-11:1995.
[0060] BET specific surface area [m 2 / g] was determined by nitrogen adsorption according to DIN 9277:2014 by the Brunauer-Emmett-Teller method.
[0061] The DOA absorption value is determined in accordance with ISO 19246 with the aid of an absorptometer from Brabender equipped with a torque measurement and handling system. It can be used to assess the liquid absorption capacity of silicon dioxide, calcium silicate and sodium aluminosilicate. The daily absorption value indicates the carrier capacity of the filler.
[0062] The density Dy (transparency) of the matted clearcoats was measured in accordance with DIN 55988 with an eXact densitometer from X-Rite.
[0063] Here, matted clearcoats from different paint systems were applied to black PMMA sheets and the various matting agents were compared by always adjusting the gloss level to the same gloss level measured at 60° considered in the specific case. The transparency was then determined via logarithmic calculations by diffuse reflection at an angle of 45°. The parameters for the measurement were set as follows:
[0064] parameter set up Measurement conditions M0(None): No filter Density state ISO Status E Density White Base absolute All densities CMYK Density / tone value Solid color: CMYK Density / tone value Color: Hue value Tone Value / Spot SCTV (ISO20654) Light source / Observer D65 / 2° / 10°
[0065] The determination by means of a fineness meter is in accordance with DIN EN ISO 1524.
[0066] The dispersion properties of various matting agents were evaluated using a black melamine baking varnish and a TIDAS instrument from Labman for automatic fineness gauge drawdowns for determining the fineness of dispersion.
[0067] In order to produce Figure 2 and Figure 3 The fineness meter images shown were obtained using a black medium-solids baking varnish from AXALTA Coating Systems Austria GmbH (designated DUPLEX D 1326, formulation number B11830875) together with an appropriate V 0003 diluent (from AXALTA).
[0068] Here the appropriate amount of precipitated silica required to adjust the gloss level of the dry paint layer to 20 GU, measured at an angle of 60°, was stirred into 100 g of paint with a paddle stirrer at 2000 rpm for 10 minutes. The paint was then applied in liquid form to a grindometer block with a maximum channel depth of 70 μm and applied automatically by knife coating and evaluated with the TIDAS instrument.
[0069] Carbon content [wt%] is determined according to EN ISO 3262-20:2000 (Chapter 8) by elemental analysis with a C632 carbon determination system (manufacturer: LECO). The sample to be analyzed is weighed into a ceramic crucible, mixed with a combustion additive and heated in an induction furnace under an oxygen flow. The carbon present is oxidized to CO2. The amount of CO2 gas is quantified by an infrared detector (IR). SiC, if present, does not burn and therefore does not affect the carbon content value.
[0070] The Hg pore volume (d<4 μm, d<5 μm) was determined after grinding the silica based on mercury intrusion according to DIN 66133 using an AutoPore V 9520 instrument from Micromeritics with the following device settings: contact angle of 140° and pressure range of 0.003–420 MPa, and in the pore size range of 3.5 nm–500 μm. BRIEF DESCRIPTION OF THE DRAWINGS
[0071] Figure 1 An SEM image of a varnish coating incorporating silica particles is shown in cross section. Figure 2Fineness meter images of K1 and K2 are shown. Figure 3 Fineness meter images of VG1 and VG2 are shown. Figure 4 A diagram showing the determination of the pore volume by means of a Hg porosimeter is shown. Example 1. Preparation of precipitated silica K1 and K2 of the present invention
[0072] At 50°C, under continuous stirring, 3 The sedimentation vessel was initially filled with 13.5 m 3 of water, with 14.85m 3 Commercially available water glass (27.1% SiO2; 8.07% Na2O; density 1.335) was added thereto at a rate of / h, and the addition was terminated after 13 minutes. Subsequently, the mixture was heated to a temperature of 70°C. Then, the mixture was heated at 0.27 m / s for 30 minutes. 3 / h adding 96% sulfuric acid with constant shearing and stirring, the temperature being maintained at 85°C by closed-loop control. After a period of 120 minutes, the suspension is acidified again with sulfuric acid within 60 minutes until the pH reaches a value in the range of 3.5 to 3.9. The solid is separated from the suspension using a membrane filter press, the filter cake is washed with demineralized water and then dried using a spray dryer. For drying by spray dryer, the filter cake is liquefied with water under the action of shear forces and adjusted to a solids content of <10%.
[0073] The dried precipitated silica according to the invention is classified and ground according to the desired particle distribution with the aid of a Netzsch CGS 50 air jet mill.
[0074] K1 is an untreated silica according to the invention having the physicochemical properties according to Table AC.
[0075] During classification and grinding in a grinder, K2 was similarly prepared, where the surface of K2 was covered with a commercial PE wax, where the amount of wax was adjusted to a carbon content of 3.4%, measured with a LECO elemental analyzer. The physicochemical indices of K2 can also be seen from Tables A–C.
[0076] The comparative example cited is a commercially available precipitated silica from Tosoh.
[0077] Table A:
[0078]
[0079] Table B:
[0080]
[0081] Table C:
[0082]
[0083] Table AC shows the physicochemical indices of the precipitated silicas according to the invention and the comparative silicas VG1 and VG2. K1 is an untreated precipitated silica according to the invention. K2 is a wax-treated precipitated silica according to the invention. Comparative examples VG1 and VG2 are Tosoh precipitated silicas with the trade names Nipsil E-1011 (organic post-treatment according to the data sheet) (VG2) and Nipsil E-220A (VG1). The average particle size of these commercially available precipitated silicas has a similar d 50 VG1 and VG2 are known to be used as matting additives.
[0084] Compared to VG1 and VG2 from Tosoh, which have comparable particle size distributions, the inventive precipitated silicas K1 and K2 show much higher DOA values (see Table A).
[0085] The specific porosity of the silicas K1 and K2 according to the invention can be demonstrated by mercury porosimetry. The corresponding values are shown in Table C.
[0086] Compared to precipitated Nipsil E 1011 (VG2) of 8.9 μm and Nipsil E-220A (VG1) of 8.0 μm, the silicas K1 and K2 of the invention exhibit a much smaller average pore size of about 2.8 μm. However, K1 and K2 are able to absorb more mercury in the pore ranges of 0.1-3.0 μm, 0.1-4.0 μm and 0.1-5.0 μm. The higher number of average smaller pores brings a crucial advantage in terms of transparency, especially in the case of waterborne paint systems.
[0087] 2. Preparation of paint system
[0088] Various paint systems were produced for paint testing.
[0089] 2.1 Paint system 1: 2K PUR paint (DD paint)
[0090] A solvent based 2K PUR paint was prepared according to the details in Table 1.
[0091] Table 1: Paint system 1
[0092]
[0093] Weigh each paint raw material step by step in the above order and homogenize with a laboratory dissolver. Homogenization is required after each of items 4, 5, 6 and 7. Final homogenization of the paint is performed after item 8.
[0094] 2.2 Paint system 2: 1K PU acrylate, wb (clear varnish)
[0095] A water based 1K PU acrylate paint was prepared according to the details in Table 2.
[0096] Table 2: Paint system 2
[0097]
[0098] The pH was adjusted to 8.5-9.0 by adding AMP 95, and preliminary mixture 1 was prepared from items 2 and 3. Likewise, preliminary mixture 2 was prepared from items 6 and 7. Then, item 1 was added first, and preliminary mixture 1 was added while stirring. After the continuous addition of items 4 and 5, preliminary mixture 2 was added. Finally, the varnish was homogenized at 1500 rpm for 10 minutes and introduced into an airtight can.
[0099] 2.3 Paint system 3: 1K acrylic, wb (clear coat)
[0100] A water-based 1K acrylic paint was prepared according to the details in Table 3.
[0101] Table 3: Paint system 3
[0102]
[0103] A preliminary mixture was prepared from items 4 and 5 by adjusting the pH to 8.5-9.0 by adding AMP 95. Then, item 1 was added first and the preliminary mixture was added while stirring. After the continuous addition of items 2 and 3, the varnish was homogenized at 1500 rpm for 10 minutes and introduced into an airtight can.
[0104] 3 Application of paint systems and evaluation of surface properties
[0105] 3.1 Adding silica to paint system
[0106] Paint system 1:
[0107] According to the weight of Table 3.1, the silica was introduced into 100 parts by weight of paint system 1 in a 350 ml PE cup. Here it was ensured that the silica was properly incorporated and did not adhere to the edge of the cup. Subsequently, the subsequently matted paint system 1 was dispersed with a 4.2 cm paddle stirrer at 2000 rpm for 10 minutes.
[0108] Paint system 2:
[0109] 95 parts by weight of Paint System 2 and 5 parts by weight of Dowanol DPM (dipropylene glycol methyl ether, Dow Chemical) were mixed under stirring and stirred at 1000 rpm for 5 minutes using a paddle stirrer.
[0110] The appropriate weight of silica was incorporated into the mixture according to Table 3.2, except that the mixture was continuously stirred with a paddle stirrer while the silica was being added.
[0111] Paint system 3:
[0112] Silica was incorporated in a similar manner to paint system 2 according to the weights in Table 3.3.
[0113] VG1 and VG2 were similarly incorporated into the corresponding paint systems, with the weights shown in Tables 3.1–3.3.
[0114] 3.2 Application of matte paint systems and evaluation of surface properties
[0115] After the 30-minute degassing phase, the corresponding matt paint system was scraped onto the black PMMA sheet with a Coatmaster 509MC film applicator. For this purpose, a box coating rod with a gap height of 200 μm was used. The scraping rate was set to 25 mm / s. Under climate control conditions of 21°C-25°C and 40%-60% relative humidity, the coated PMMA sheet was dried overnight. The gloss level at 60° and the transparency of the dry matt surface were measured one day after application.
[0116] Table 3.1: Paint performance results for paint system 1
[0117]
[0118] Table 3.2: Paint performance results for paint system 2
[0119]
[0120] Table 3.3: Paint performance results for paint system 3
[0121]
[0122] The three paint systems shown are representative of many standard binder systems in which a high-quality matte surface is desired. Aspects such as transparency and tactile properties play an important role here, particularly in matte coatings.
[0123] Compared to conventional precipitated silicas, the silicas K1 and K2 according to the invention show a higher efficiency (economic feasibility) in all three paint systems over the entire gloss range from 20 gloss points measured at 60° to deep matt at 2 gloss values at 60°. This means that, in order to achieve the gloss levels shown in Tables 3.1–3.3, less silica needs to be used than is the case with the conventional comparison silicas VG1 and VG2. A comparison of the efficiency is only meaningful if the silicas compared to one another have similar particle size distributions [see Table A (d5, d50 and d95)].
[0124] Compared to conventional silicas in solvent-based paint system 1, the silicas K1 and K2 according to the invention show higher transparency values Dy in the gloss range of 20 to 2 gloss points at 60° (Table 3.1). Likewise in the two water-based paint systems 2 and 3 (Tables 3.2 and 3.3), the transparency values in the gloss range of 20 to 5 gloss units (60° angle) are generally higher. It should be noted here that the transparency of the matted clearcoat systems 1, 2 and 3 can only be compared if the gloss levels are the same. Comparison with the same dosage of matting agent is not permitted. The measured transparency values Dy are logarithmic values. Therefore, the higher the Dy value, the more transparent the matted clearcoat is.
[0125] For example, the untreated silica K1 precipitated in a 1K acrylate paint system (paint system 3) has a Dy value of 2.19 at 20 gloss units (60° angle), while the untreated precipitated comparative silica Nipsil E-220A (VG1) has a transparency value of only 2.10. K1 thus has a transparency that is approximately 23% higher. Even a value difference of 0.03 determined by measurement can be visually perceived by a trained eye.
[0126] This specific porosity of the silicas K1 and K2 according to the invention therefore has a positive influence on the efficiency and transparency in different coating systems.
[0127] 4. Dispersion characteristics measured by fineness meter
[0128] 100 g of DUPLEX D 1326 paint were weighed into a 350 ml polyethylene cup and 20 g of V 0003 thinner were weighed. Then the amount of silica specified in Table 4 was weighed and carefully incorporated into the diluted test paint using a spatula. Thereafter, a paddle stirrer ( ) The mixture was dispersed at 2000 rpm for 10 minutes while covering the PE cup to avoid evaporation losses. After incorporation of silica, the matted paint was placed in a closed beaker for degassing for 30 minutes.
[0129] To ensure comparability of the different silicas, the Duplex D 1326 black paint was adjusted in each case using the matting agents listed in Table 4 to a gloss level of 20 gloss units (±0.1) measured at an angle of 60°.
[0130] Gloss level adjustment is checked as follows:
[0131] After degassing is complete, the paint is applied to clean glass plates (130×90×3 mm) at a speed of 25 mm / s using a square coating rod with a gap height of 120 μm using an electric knife coating device (Erichsen Coatmaster 509MC). The square coating rod is weighted down with a VA steel block (dimensions: 71×30×24 mm, weight: about 420 g) to increase the applied load. Two glass plates should be coated for each dispersed sample. The applied paint is flashed using fixed flash conditions:
[0132] Temperature: 20℃ to 25℃
[0133] Relative humidity: 40% to 60%
[0134] Flash time: 10 minutes to 20 minutes
[0135] The paint was then baked in a circulating paint drying cabinet at 150° C. for 20 minutes. After the glass plate had cooled (at least 30 minutes), the reflectometer value was measured by means of the BYK haze gloss. The reflectometer value was formed from the average of the duplicate determinations.
[0136] Figure 2 Fineness gauge image showing K1 and K2
[0137] Figure 3 Fineness gauge image showing VG1 and VG2
[0138] Table 4: Evaluation of fineness meter images
[0139]
[0140] Figure 2 and Figure 3 The fineness meter images of the inventive silicas K1 and K2 shown in show values of 3 μm lower than those of the comparative silicas VG1 and VG2. This also correlates with the lower d95% values in Table A, since the fineness meter values are largely determined by the coarser components of the particle assembly. As in the case of the clearcoat systems 1, 2 and 3 shown above, the silicas according to the invention also show a higher efficiency in the black pigment Duplex D 1326 test paint, since less matting agent needs to be added in order to establish a gloss level of 20 measured at an angle of 60°. It is also noteworthy that Figure 2 K1 and K2 in the present invention have a much smaller transition range and no spots at all. In the case of many precipitated silicas with d50 values of less than 5 μm, the silica particles have a tendency to reaggregate during storage, which can be recognized over time by an increasing number of spots in the fineness meter image. In general, the aggregation tendency of untreated silicas is higher than in the case of those with an organic coverage of the surface. In the case of silicas with a high reaggregation tendency, this may occur after a few days or, in the case of higher stability, after weeks or months. In the case of silicas K1 and K2 according to the invention, by contrast, this was not observed, thus confirming a very low tendency to spot formation. It is believed that the specific morphology and pore distribution of silicas K1 and K2 not only have a favorable influence on the dispersibility, but also lead to a high stability against reaggregation.
Claims
1. Precipitated silica, characterized in that BET: 150m 2 / g–400m 2 / g, preferably 200m 2 / g–300m 2 / g, measured according to ISO 9277, DOA: 220ml / 100g–400ml / 100g, preferably 250ml / 100g–350ml / 100g, measured according to ISO 19246, d 50 : 3.0 μm–5.0 μm, measured by laser diffraction on a Coulter LS according to ISO 13320, Particle size ratio d5:d 50 :d 95 :>0.3:1:<2, Particle size distribution Between 1.3 and 1.
7.
2. The precipitated silica according to claim 1, characterized in that The median pore size is less than 7.0 μm, preferably less than 5.0 μm, more preferably less than 3.0 μm, measured according to ISO 15901-1 using an Autopore IV 9520 with the following instrument settings: contact angle of 140° and pressure range of 0.003-420 MPa, calculated over the pore size range of 3.5 nm-500 μm.
3. The precipitated silica according to any one of claims 1 to 2, characterized in that The pore volume is greater than 2.40 ml / g (d=0.1 μm-d=4.0 μm)-3.10 ml / g (d=0.1 μm-d=4.0 μm), as determined with the aid of a Hg porosimeter.
4. The precipitated silica according to any one of claims 1 to 3, characterized in that The pore volume is greater than 2.50 ml / g (d=0.1 μm-d=5.0 μm)-3.30 ml / g (d=0.1 μm-d=5.0 μm), determined with the aid of a Hg porosimeter.
5. The precipitated silica according to any one of claims 1 to 4, characterized in that d 50 3.5-4.5μm.
6. Use of the precipitated silica according to claims 1 to 5 as a matting agent for the preparation of dispersions, mill bases, paints, coatings or printing inks, inkjet inks, grinding resins, pigment concentrates, color preparations, pigment preparations, filler preparations or coating compositions.
7. Wax-coated precipitated silica, characterized in that BET: 150m 2 / g–400m 2 / g, preferably 200m 2 / g–300m 2 / g, measured according to ISO 9277, DOA: 220ml / 100g–400ml / 100g, preferably 250ml / 100g–350ml / 100g, measured according to ISO 19246, d 50 : 3.0 μm–5.0 μm, measured by laser diffraction (Coulter LS) according to ISO 13320, Particle size ratio d5:d 50 :d 95 :>0.3:1:<2, Particle size distribution Between 1.3 and 1.7, Carbon content: 1.0-6.0 wt. %, preferably 2.4-3.8 wt. %, measured by LECO according to ISO 3262-19.
8. Use of the precipitated silica according to claim 7 as a matting agent for the preparation of dispersions, mill bases, paints, coatings or printing inks, inkjet inks, grinding resins, pigment concentrates, color preparations, pigment preparations, filler preparations or coating compositions.