Preparation method and application of superfine high-nickel ternary precursor

By preparing ultrafine high-nickel ternary precursors under high pH and high stirring rate, the problems of inaccurate particle size distribution and inconsistent morphology were solved, and ultrafine high-nickel ternary precursors with good morphological consistency and sphericity were obtained, which are suitable for lithium-ion battery cathode materials.

CN118894559AInactive Publication Date: 2024-11-05GUILIN UNIV OF ELECTRONIC TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411327920.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing continuous production of ternary precursors, particle size distribution control is not precise, particle morphology is inconsistent, sphericity is poor, and process parameters are difficult to control precisely.

Method used

Ultrafine high-nickel ternary precursors were prepared by co-precipitation reaction under high pH and high stirring rate conditions. The pH of the reaction system was controlled at 11.0–12.0 and the ammonia concentration at 4–8 g/L. The particle size was monitored and the feed was stopped when it reached 1.5–3.0 μm, and the reaction continued until complete.

Benefits of technology

It achieves excellent morphological consistency and sphericity of ultrafine high-nickel ternary precursors, with a simple process and easy parameter control, making it suitable for lithium-ion battery cathode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894559A_ABST
    Figure CN118894559A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a superfine high-nickel ternary precursor, which comprises the following steps: 1) simultaneously adding a ternary metal salt solution, a liquid alkali solution and an ammonia water solution into a reaction kettle containing a base solution in a parallel flow manner, carrying out a coprecipitation reaction at a stirring rate of 300-400r / min, and controlling the pH value of a reaction system to be 11.0-12.0 and the ammonia concentration to be 4-8g / L in the reaction process, and continuously monitoring the particle size, stopping feeding when the particle size D50 reaches 1.5-3.0 [mu] m, and continuously reacting until the materials are completely reacted to obtain the superfine high-nickel ternary precursor. The superfine high-nickel ternary precursor obtained through the method is good in morphology consistency, especially the superfine sphericity degree and primary crystal grains can be kept consistent with large particles, the technological process is simple, technological parameters are easy to control, and precision is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ternary precursor preparation, and specifically relates to a preparation method of an ultrafine high-nickel ternary precursor and application thereof. Background Art

[0002] In the continuous production of ternary precursors, when the particle size is close to the target particle size, process parameters such as ternary flow, liquid alkali flow, ammonia flow, rotation speed, temperature, etc. are usually added or subtracted in the reacting system, so that the reaction system in the growth state fluctuates through the change of process parameters, thereby generating new crystal nuclei and new small particles; in addition, by the method of growing and overflowing, continuous reaction and continuous discharge are achieved, and stable productivity is good; however, in order to maintain the particle size distribution, this conventional continuous method usually needs to generate small particles by adjusting various process parameters of the reaction process, and the morphology of the small particles generated by adjusting the parameters is generally rough, the sphericity is poor, and the particle size control is difficult, and the stability of various indicators is not good. In addition, since there are many parameters that need to be adjusted in the reaction process, it is easy to cause the problem that each parameter is not easy to control and the control accuracy is poor. Summary of the invention

[0003] In view of this, the present application provides a method for preparing an ultrafine high-nickel ternary precursor, which solves the problem of inaccurate particle size distribution control and inconsistent particle morphology caused by adjusting process parameters to produce small particles to maintain particle size distribution in the existing continuous method.

[0004] Another object of the present invention is to provide an application of an ultrafine high-nickel ternary precursor prepared by the above-mentioned method for preparing an ultrafine high-nickel ternary precursor in a continuous process for preparing a high-nickel ternary precursor.

[0005] The third object of the present invention is to provide an application of an ultrafine high-nickel ternary precursor prepared by the above-mentioned method for preparing a high-nickel ternary precursor in a positive electrode material for a lithium-ion battery.

[0006] To achieve the above object, the technical solution of the present invention is implemented as follows: a method for preparing an ultrafine high-nickel ternary precursor, the method comprising: The ternary metal salt solution, liquid alkali solution and ammonia solution are simultaneously added to a reactor containing a base liquid and a co-precipitation reaction is carried out at a stirring rate of 200-400 r / min. During the reaction, the pH of the reaction system is controlled to be 11.0-12.0, the ammonia concentration is 4-8 g / L, and the particle size is continuously monitored. When the particle size D50 reaches 1.5-3.0 μm, the feeding is stopped and the reaction is continued until the material reaction is complete to obtain an ultrafine high-nickel ternary precursor.

[0007] Preferably, the concentration of aqueous ammonia in the base liquid is 4-8 g / L, the temperature of the base liquid is 40-60° C., and the pH of the base liquid is 11.0-12.0.

[0008] Preferably, the feed rate of the ternary metal salt solution is 100 to 300 L / h.

[0009] Preferably, the feed rate of the liquid alkali solution is 50 to 100 L / / h.

[0010] Preferably, the feed rate of the aqueous ammonia is 10 to 30 L / h.

[0011] Preferably, the ternary metal salt solution is a nickel-cobalt-manganese ternary mixed salt solution, and the concentration of the nickel-cobalt-manganese ternary mixed salt solution is 80-120 g / L.

[0012] Preferably, the mass concentration of the liquid caustic soda in the liquid caustic soda solution is 28-32%, and the mass concentration of the aqueous ammonia in the aqueous ammonia solution is 10-20%.

[0013] Preferably, the nickel content in the obtained ultrafine high-nickel ternary precursor is 80-85 mol%.

[0014] Preferably, the nickel-cobalt-manganese ternary mixed salt solution is at least one of a nickel-cobalt-manganese ternary mixed sulfuric acid solution, a nickel-cobalt-manganese ternary mixed hydrochloric acid solution, and a nickel-cobalt-manganese ternary mixed nitric acid solution.

[0015] Another technical solution of the present invention is achieved as follows: an application of a high-nickel ternary precursor prepared by the above-mentioned method for preparing a high-nickel ternary precursor in a positive electrode material for a lithium-ion battery.

[0016] Compared with the prior art, the present invention synthesizes a 1.5-3.0 single crystal ultrafine high nickel ternary precursor under high pH and high stirring rate conditions, and has good morphology consistency and sphericity, and the process is simple, and the process parameters are easy to control with high precision. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a SEM image of the ultrafine high-nickel ternary precursor obtained in Example 1 of the present invention; Figure 2 is a SEM image of the ternary precursor obtained in Comparative Example 1 of the present invention; Figure 3 is a SEM image of the ternary precursor obtained in Comparative Example 2 of the present invention; Figure 4 It is a SEM picture of the ternary precursor obtained in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0019] The present invention uses a laser particle size analyzer to measure the particle size of the particles in the process of generating the ultrafine high-nickel ternary precursor and the particle size of the finally obtained cobalt oxide particles. The chemical reagents used in the embodiments of the present invention are obtained through conventional commercial channels unless otherwise specified.

[0020] An embodiment of the present invention provides a method for preparing an ultrafine high-nickel ternary precursor, the method comprising: A nickel-cobalt-manganese ternary mixed salt solution with a concentration of 80-120 g / L, a liquid alkali solution with a mass concentration of 28-32%, and an ammonia solution with a mass concentration of 10-20% are simultaneously and concurrently added to a reactor containing a base liquid with a temperature of 40-60° C., an ammonia concentration of 4-8 g / L, and a pH of 11.0-12.0 at a feed rate of 100-300 L / h, 50-100 L / h, and 10-30 L / h, respectively, and a coprecipitation reaction is carried out at a stirring rate of 200-400 r / min. During the reaction, the pH of the reaction system is controlled to be 11.0- 12.0, ammonia concentration of 4-8g / L, temperature of 40-60°C, continuous monitoring of particle size, before the particle size does not meet the requirements, the reaction process will use a high-efficiency concentrator to collect all the particles and return them to the reactor at any time for continuous reaction and growth, when the particle size D50 reaches 1.5-3.0μm, stop feeding, continue the reaction until the material reacts completely, and obtain an ultrafine nickel-cobalt-manganese ternary precursor with a nickel content of 80-85mol%; wherein the nickel-cobalt-manganese ternary mixed salt solution is at least one of a nickel-cobalt-manganese ternary mixed sulfuric acid solution, a nickel-cobalt-manganese ternary mixed hydrochloric acid solution, and a nickel-cobalt-manganese ternary mixed nitric acid solution.

[0021] The embodiment of the present invention also provides an application of an ultrafine high-nickel ternary precursor prepared by the above-mentioned method for preparing an ultrafine high-nickel ternary precursor in a positive electrode material for a lithium-ion battery.

[0022] After adopting the above scheme, the single crystal ultrafine high nickel ternary precursor of 1.5-3.0 is synthesized under high pH and high stirring rate conditions, and the morphology is consistent and the sphericity is good. The process is simple, and the process parameters are easy to control with high precision. In order to better explain the solution of the present invention, further description is given below in conjunction with specific embodiments. Example

[0023] Nickel sulfate, cobalt sulfate and manganese sulfate are mixed to prepare a ternary mixed sulfuric acid solution of nickel, cobalt and manganese with a concentration of 100 mol / L, a liquid alkali solution with a mass concentration of 30% and an ammonia solution with a mass concentration of 15%; The above-mentioned 100 mol / L nickel-cobalt-manganese ternary mixed sulfuric acid solution, 30% liquid alkali solution and 15% ammonia solution were added simultaneously and concurrently into a reactor containing a base liquid with a temperature of 50°C, an ammonia concentration of 6 g / L and a pH of 11.0-11.5 at feed rates of 200 L / h, 50 L / h and 20 L / h, respectively, and a co-precipitation reaction was carried out at a stirring rate of 300 r / min. During the reaction, the pH of the reaction system was controlled to be 11.0-11.5, the ammonia concentration was 6 g / L, and the temperature was 50°C. The particle size was continuously monitored. When the particle size D50 reached 2.0 μm, the feeding was stopped and the reaction was continued until the material reaction was complete to obtain an ultrafine nickel-cobalt-manganese ternary precursor.

[0024] The nickel content in the ultrafine nickel-cobalt-manganese ternary precursor obtained in Example 1 was detected, and it was found that the nickel content was 83 mol%. Example

[0025] Nickel sulfate, cobalt sulfate and manganese sulfate are mixed to prepare a nickel-cobalt-manganese ternary mixed sulfuric acid solution with a concentration of 80 g / L, a liquid alkali solution with a mass concentration of 28%, and an ammonia solution with a mass concentration of 10%; The above-mentioned nickel-cobalt-manganese ternary mixed sulfuric acid solution with a concentration of 80 mol / L, the liquid alkali solution with a mass concentration of 28%, and the ammonia solution with a mass concentration of 10% are added simultaneously and concurrently to a reactor containing a base liquid with a temperature of 40°C, an ammonia concentration of 4 g / L, and a pH of 11.5-12.0 at feed rates of 100 L / h, 50 L / h, and 10 L / h, respectively, and a co-precipitation reaction is carried out at a stirring rate of 300 r / min. During the reaction, the pH of the reaction system is controlled to be 11.5-12.0, the ammonia concentration is 4 g / L, and the temperature is 40°C. The particle size is continuously monitored. When the particle size D50 reaches 1.5 μm, the feeding is stopped, and the reaction is continued until the material reaction is complete to obtain an ultrafine nickel-cobalt-manganese ternary precursor with a nickel content of 80 mol%.

[0026] The nickel content in the ultrafine nickel-cobalt-manganese ternary precursor obtained in Example 2 was detected, and it was found that the nickel content was 80 mol%. Example

[0027] Nickel sulfate, cobalt sulfate and manganese sulfate are mixed to prepare a ternary mixed sulfuric acid solution of nickel, cobalt and manganese with a concentration of 120 mol / L, a liquid alkali solution with a mass concentration of 32% and an ammonia solution with a mass concentration of 20%; The above-mentioned nickel-cobalt-manganese ternary mixed sulfuric acid solution with a concentration of 120g / L, the liquid alkali solution with a mass concentration of 32%, and the ammonia solution with a mass concentration of 20% are added simultaneously and concurrently to a reactor containing a base liquid with a temperature of 60°C, an ammonia concentration of 8g / L, and a pH of 11.3-11.6 at feed rates of 300L / h, 100L / h, and 30L / h, respectively, and a co-precipitation reaction is carried out at a stirring rate of 350r / min. During the reaction, the pH of the reaction system is controlled to be 11.3-11.6, the ammonia concentration is 8g / L, and the temperature is 60°C. The particle size is continuously monitored. When the particle size D50 reaches 3.0μm, the feeding is stopped, and the reaction is continued until the material reaction is complete to obtain an ultrafine nickel-cobalt-manganese ternary precursor with a nickel content of 85mol%.

[0028] The nickel content in the ultrafine nickel-cobalt-manganese ternary precursor obtained in Example 3 was detected, and it was found that the nickel content was 85 mol%.

[0029] Comparative Example 1 Nickel sulfate, cobalt sulfate and manganese sulfate are mixed to prepare a ternary mixed sulfuric acid solution of nickel, cobalt and manganese with a concentration of 100 mol / L, a liquid alkali solution with a mass concentration of 30% and an ammonia solution with a mass concentration of 15%; The above-mentioned 100 mol / L nickel-cobalt-manganese ternary mixed sulfuric acid solution, 30% liquid alkali solution and 15% ammonia solution were added simultaneously and concurrently into a reactor containing a base liquid with a temperature of 50°C, an ammonia concentration of 6 g / L and a pH of 11.0-11.5 at feed rates of 200 L / h, 50 L / h and 20 L / h, respectively, and a co-precipitation reaction was carried out at a stirring rate of 100 r / min. During the reaction, the pH of the reaction system was controlled to be 11.0-11.5, the ammonia concentration was 6 g / L, and the temperature was 50°C. The particle size was continuously monitored. When the particle size D50 reached 2.0 μm, the feeding was stopped and the reaction was continued until the material reaction was complete to obtain a nickel-cobalt-manganese ternary precursor.

[0030] The nickel content in the ultrafine nickel-cobalt-manganese ternary precursor obtained in Comparative Example 1 was detected, and it was found that the nickel content was less than 80 mol%.

[0031] Comparative Example 2 Nickel sulfate, cobalt sulfate and manganese sulfate are mixed to prepare a ternary mixed sulfuric acid solution of nickel, cobalt and manganese with a concentration of 100 mol / L, a liquid alkali solution with a mass concentration of 30% and an ammonia solution with a mass concentration of 15%; The above-mentioned 100 mol / L nickel-cobalt-manganese ternary mixed sulfuric acid solution, 30% liquid alkali solution and 15% ammonia solution were added simultaneously and concurrently into a reactor containing a base liquid with a temperature of 50°C, an ammonia concentration of 6 g / L and a pH of 10.5-11.0 at feed rates of 200 L / h, 50 L / h and 20 L / h, respectively, and a co-precipitation reaction was carried out at a stirring rate of 300 r / min. During the reaction, the pH of the reaction system was controlled to be 10.5-11.0, the ammonia concentration was 6 g / L, and the temperature was 50°C. The particle size was continuously monitored. When the particle size D50 reached 2.0 μm, the feeding was stopped and the reaction was continued until the material reaction was complete to obtain a nickel-cobalt-manganese ternary precursor.

[0032] The nickel content in the ultrafine nickel-cobalt-manganese ternary precursor obtained in Comparative Example 2 was detected, and it was found that the nickel content was less than 80 mol%.

[0033] Comparative Example 3 Nickel sulfate, cobalt sulfate and manganese sulfate are mixed to prepare a ternary mixed sulfuric acid solution of nickel, cobalt and manganese with a concentration of 100 mol / L, a liquid alkali solution with a mass concentration of 30% and an ammonia solution with a mass concentration of 15%; The above-mentioned 100 mol / L nickel-cobalt-manganese ternary mixed sulfuric acid solution, 30% liquid alkali solution and 15% ammonia solution were added simultaneously and concurrently into a reactor containing a base liquid with a temperature of 50°C, an ammonia concentration of 6 g / L and a pH of 10.5-11.0 at feed rates of 200 L / h, 50 L / h and 20 L / h, respectively, and a co-precipitation reaction was carried out at a stirring rate of 100 r / min. During the reaction, the pH of the reaction system was controlled to be 10.5-11.0, the ammonia concentration was 6 g / L, and the temperature was 50°C. The particle size was continuously monitored. When the particle size D50 reached 2.0 μm, the feeding was stopped and the reaction was continued until the material reaction was complete to obtain a nickel-cobalt-manganese ternary precursor.

[0034] The nickel content in the ultrafine nickel-cobalt-manganese ternary precursor obtained in Comparative Example 3 was detected, and it was found that the nickel content was less than 80 mol%.

[0035] The difference between Comparative Example 1 and Example 1 is that the stirring speed during the coprecipitation reaction is different, the difference between Comparative Example 2 and Example 1 is that the pH of the reaction system during the coprecipitation reaction is different; the difference between Comparative Example 3 and Example 1 is that the stirring speed during the coprecipitation reaction and the pH of the reaction system are different. The reaction parameters in the above examples and comparative examples are specifically shown in Table 1: Reaction parameters of Example 1-Example 3 and Comparative Example 1-Comparative Example 3 In order to verify whether the morphology of the particles of the ternary precursor prepared by this embodiment is consistent and whether the sphericity is good, the ternary precursors obtained in Example 1 and Comparative Example 1, Comparative Example 2 and Comparative Example 3 are respectively subjected to electron microscope scanning detection. Figure 1 , Figure 2 , Figure 3 , Figure 4 As shown, from Figure 1 It can be seen that the ultrafine ternary precursor particles obtained in the present invention have consistent morphology and good sphericity, while the ultrafine ternary precursor particles obtained from Comparative Example 1, Comparative Example 2, and Comparative Example 3 have poor morphology and poor sphericity and are relatively loose.

[0036] In addition, by comparing the SEM image of the ternary precursor obtained in Example 1 with the SEM image of the ultrafine ternary precursor obtained in the comparative example, it can be seen that, under the premise of determining the concentrations of the ternary metal salt solution, the precipitant solution and the complexing agent, the flow ratio and the base liquid concentration, high pH value and high stirring rate are the key factors for the successful preparation of a ternary precursor with good morphology consistency and good sphericity.

[0037] In summary, by synthesizing 1.5-3.0 single crystal ultrafine high nickel ternary precursors under high pH and high stirring rate conditions, the morphology consistency is good, the sphericity is good, and the process is simple, and the process parameters are simple and precise to control. Example

[0038] This embodiment discloses an application of the ultrafine nickel-cobalt-manganese ternary precursor prepared by Example 1 in a positive electrode material for a lithium-ion battery.

[0039] The ultrafine nickel-cobalt-manganese ternary precursor prepared in Example 1 was mixed with a lithium source and placed in a Ma furnace, and calcined at 800° C. After cooling, a nickel-cobalt-manganese lithium oxide positive electrode material was obtained.

[0040] The above materials were used as positive electrode materials for lithium-ion batteries, and the metal lithium sheet was used as the negative electrode. Button batteries were assembled for charge and discharge tests. The results were as follows: the charge and discharge voltage range was 3.1 to 4.8 V. After 200 cycles at a rate of 0.5C, the reversible capacity was 415 mAh / g, indicating that the battery obtained by using the ultrafine nickel-cobalt-manganese ternary precursor as the raw material for preparing the positive electrode material of lithium-ion batteries still has a good reversible capacity.

[0041] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing an ultrafine high-nickel ternary precursor, characterized in that: The method is: The ternary metal salt solution, liquid alkali solution and ammonia solution are simultaneously added to a reactor containing a base liquid and a co-precipitation reaction is carried out at a stirring rate of 200-400 r / min. During the reaction, the pH of the reaction system is controlled to be 11.0-12.0, the ammonia concentration is 4-8 g / L, and the particle size is continuously monitored. When the particle size D50 reaches 1.5-3.0 μm, the feeding is stopped and the reaction is continued until the material reaction is complete to obtain an ultrafine high-nickel ternary precursor.

2. The method for preparing an ultrafine high-nickel ternary precursor according to claim 1, characterized in that: The concentration of ammonia water in the base liquid is 4-8 g / L, the temperature of the base liquid is 40-60° C., and the pH of the base liquid is 11.0-12.

0.

3. The method for preparing an ultrafine high-nickel ternary precursor according to claim 2, characterized in that: The feed rate of the ternary metal salt solution is 100-300 L / h.

4. The method for preparing an ultrafine high-nickel ternary precursor according to claim 3, characterized in that: The feed rate of the liquid alkali solution is 50-100 L / h.

5. The method for preparing an ultrafine high-nickel ternary precursor according to claim 4, characterized in that: The feed rate of the ammonia water is 10 to 30 L / h.

6. The method for preparing an ultrafine high-nickel ternary precursor according to claim 5, characterized in that: The ternary metal salt solution is a nickel-cobalt-manganese ternary mixed salt solution, and the concentration of the nickel-cobalt-manganese ternary mixed salt solution is 80-120 g / L.

7. The method for preparing an ultrafine high-nickel ternary precursor according to claim 6, characterized in that: The mass concentration of the liquid caustic soda in the liquid caustic soda solution is 28-32%, and the mass concentration of the aqueous ammonia in the aqueous ammonia solution is 10-20%.

8. The method for preparing an ultrafine high-nickel ternary precursor according to claim 6, characterized in that: The nickel content in the obtained ultrafine high-nickel ternary precursor is 80-85 mol%.

9. The method for preparing an ultrafine high-nickel ternary precursor according to claim 7, characterized in that: The nickel-cobalt-manganese ternary mixed salt solution is at least one of a nickel-cobalt-manganese ternary mixed sulfuric acid solution, a nickel-cobalt-manganese ternary mixed hydrochloric acid solution, and a nickel-cobalt-manganese ternary mixed nitric acid solution.

10. Use of a high-nickel ternary precursor prepared by the method for preparing a high-nickel ternary precursor according to any one of claims 1 to 8 in a positive electrode material for a lithium-ion battery.