Biochar-nano iron-based composite material for repairing organic pollution and application of biochar-nano iron-based composite material

Biochar-nanoferro-based composite materials prepared by ultrasonic treatment and ultra-high pressure microjet homogenization technology solve the problems of low organic pollutant removal efficiency and limitations of nano-iron repair in situ in the existing technology, achieving high efficiency and environmental protection The effect of organic pollutants repair.

CN118894586APending Publication Date: 2024-11-05山东省土壤污染防治中心

Patent Information

Application Number
CN202411163625.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art has low removal efficiency and may produce secondary contamination when dealing with organic pollutants, especially chlorinated hydrocarbons and benzene, and there are limitations in in-situ repair and storage of nano-zero-valent iron.

Method used

Ultrasonic treatment and ultra-high pressure microjet homogenization technology are used to mix biochar with nano-ferrous oxides to prepare biochar-nanoferro-based composite materials, and homogenized pulverization and rapid reaction are achieved through mechanical mechanical effects, forming 20-100nm The particles significantly improve the repair effect of organic pollution.

Benefits of technology

It significantly improves the removal effect of trichloroethylene, chlorobenzene and polychlorinated biphenyls, realizes the recycling of waste biological straw, is safe and environmentally friendly, has a small amount, and has high organic pollution removal efficiency, which is suitable for large-scale promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894586A_ABST
    Figure CN118894586A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of organic pollution treatment, and relates to a biochar-nano-iron-based composite material for organic pollution remediation and application thereof.The ultrahigh-pressure micro-jet technology is creatively applied to preparation of the biochar-nano-iron-based composite material, ultrasonic treatment and ultrahigh-pressure micro-jet homogenization treatment are combined, and the biochar-nano-iron-based composite material for organic pollution remediation is obtained. The prepared biochar-nano iron-based composite material has a remarkable removal effect on trichloroethylene, chlorobenzene and polychlorinated biphenyl. The biochar-nano iron-based composite material provided by the invention realizes recycling of waste biological straws, is low in dosage and high in organic pollution removal efficiency, is beneficial to large-scale popularization, and has wide economic benefits and social benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic pollution control, and relates to a biochar-nano iron-based composite material for organic pollution remediation, and a preparation method and application thereof. Background Art

[0002] Organic pollutants are one of the main environmental pollutants. There are many types of organic pollutants in the environment, such as halogenated hydrocarbons, polychlorinated biphenyls, polycyclic aromatic hydrocarbons, azo dyes, pesticides, etc. Among them, most of the organic pollutants, mainly persistent organic matter, are highly toxic.

[0003] The treatment methods of organic pollutants can be mainly divided into physicochemical method, chemical oxidation method, biological method and catalytic oxidation method. Physicochemical method refers to the use of physical and chemical methods to treat organic pollutants, mainly including adsorption method, extraction method, etc. Adsorbents such as biochar and activated carbon are commonly used, which can adsorb and remove most organic pollutants. However, the removal efficiency of the physicochemical method is low, the operating cost is high and secondary pollution may be generated, which limits its application. The chemical oxidation method uses an oxidant with strong oxidizing properties to oxidize and degrade organic pollutants, and finally turns them into low-harm or harmless substances to achieve the purpose of removing organic pollutants. Commonly used methods include chlorination, ozone oxidation and incineration. Commonly used oxidants are mainly perchlorate, hypochlorite, chlorine dioxide, ozone, hydrogen peroxide, etc. In the application of environmental governance, the chemical oxidation method can degrade difficult-to-treat organic matter through mineralization or oxidation, thereby improving the biodegradability of these organic matter. The biochemical method mainly uses the action of microorganisms to degrade organic pollutants into low-harm or harmless substances. This technology is the most widely used technology in the treatment of organic pollutants, but it still has the defect of being unable to treat pollutants that are difficult to biodegrade. Catalytic oxidation technology is a technology that uses external media such as light, electricity, and microwaves to catalytically activate oxidants, thereby being able to efficiently treat organic pollutants. Currently, commonly used catalytic oxidation technologies include photocatalysis, electrocatalysis, and wet catalytic oxidation.

[0004] Some researchers have found that the use of zero-valent metals such as magnesium, copper, and iron has great advantages in removing organic pollution from groundwater. The chemical properties of zero-valent iron are very active, and its strong reducing property can replace the metals behind it in the metal activity sequence, and precipitate the replaced metals on the surface of the iron. It can reduce ions, compounds, and organic matter with strong oxidizing properties, so it is widely used in environmental governance. The discovery of nano zero-valent iron and its application in environmental remediation have greatly increased the application space and potential of iron-based materials. Although nano zero-valent iron has the characteristics of excellent reactivity, low cost and low toxicity, it also faces limitations in in-situ remediation and storage due to its own properties.

[0005] Biochar is a new type of material, which is a product formed by thermal cracking of biomass under anaerobic conditions. Biochar has small particles, fine distribution, and light texture. It is a black porous solid. Its main components are carbon and oxygen. The carbon content in biochar is generally above 70%. The raw materials for preparing biochar come from a wide range of sources, such as sawdust, straw, industrial organic waste, urban sludge, palm fiber, coconut fiber, etc. Biochar has the characteristics of looseness, large specific surface area, and a large amount of negative charge on the surface. These characteristics make biochar have good adsorption characteristics. As a soil structure improver or a soil pollution repair agent, biochar can increase the pH value of acidic soil and increase the cation exchange capacity, thereby adsorbing pollutants and heavy metals in the soil.

[0006] Biochar has a high specific surface area, porosity and highly aromatic structure, and can be used as a carrier for iron-based catalysts in heterogeneous catalysis, which can increase the contact opportunities between iron, oxidants, pollutants, etc. and improve the reaction efficiency. The prior art has not disclosed the preparation of biochar-nano iron-based composite materials by microfluidization to achieve efficient remediation of organic pollution. Summary of the invention

[0007] In view of this, the purpose of the present invention is to provide a biochar-nano iron-based composite material for organic pollution remediation and its preparation method and application, which can effectively solve the agglomeration and passivation problem of iron-based nanoparticles and improve the remediation effect on organic pollution such as chlorinated hydrocarbons and benzene series.

[0008] To achieve the above objectives, this application adopts the following technical solutions:

[0009] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0010] The biochar and iron oxide are mixed, and ultrasonically treated for 20-35 minutes at an ultrasonic power of 300-400W; ultra-high pressure microfluidizer is used for treatment for 3-5 minutes at a treatment pressure of 140-170Mpa and a treatment temperature of 20-30°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0011] Preferably, the mass ratio of the biochar to the iron oxide is 6:1-8:1.

[0012] Preferably, the method for preparing the biochar is as follows: the washed corn stalks are dried, crushed, placed in a muffle furnace, heated to 400°C-450°C at a rate of 10-15°C / min under a N2 atmosphere, oxygen-limited pyrolysis for 2-4h, taken out, cooled, ground through a 200-mesh sieve, and dried at 70-80°C.

[0013] Preferably, the iron oxide is Fe2O3.

[0014] Preferably, the iron oxide is α-Fe2O3.

[0015] Preferably, in a preferred embodiment of the present invention, a biochar-nano iron-based composite material for organic pollution remediation is prepared by the following method:

[0016] 1) The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, pyrolyzed for 3 hours in an oxygen-limited manner, taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar;

[0017] 2) The biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, and ultrasonically treated for 25 minutes at an ultrasonic power of 350 W; ultra-high pressure microfluidizer was used for treatment for 4 minutes at a treatment pressure of 160 MPa and a treatment temperature of 25°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0018] As a new high-energy and high-efficiency homogenization method, ultra-high pressure microfluidization technology has great application potential in the preparation of nanomaterials with advantages such as high stability, high loading rate and high bioavailability. The present invention creatively applies ultra-high pressure microfluidization technology to the preparation of biochar-nano iron-based composite materials and combines ultrasonic treatment with ultra-high pressure microfluidization homogenization treatment.

[0019] The mixed liquid of biochar and iron oxide of the present invention is subjected to ultrasonic treatment, and the mechanical force and corresponding thermal effect in the ultra-high pressure micro-jet homogenizer induce mechanical effects that can induce changes in the physical, chemical and structural properties of the material macromolecules, thereby achieving the effects of homogenization, crushing, refinement and rapid reaction. After the ultra-high pressure crushing effect of the high-pressure micro-jet homogenizer, the mixed liquid of biochar and iron oxide of the present invention is crushed and refined into a biochar-nano iron-based composite material with a particle size range of 20-100nm, uniform particles, good dispersion effect, and no obvious agglomeration phenomenon. The biochar-nano iron-based composite material prepared by the preparation method of the present invention has a significant repair effect on organic pollution.

[0020] Trichloroethylene is a semi-volatile, hydrophobic, colorless, transparent liquid that is slightly soluble in water and easily soluble in organic solvents such as ethanol and ether. It is widely used in industrial production. Trichloroethylene is prone to migration in the environment and can enter the environment through volatilization, container leakage, wastewater discharge, pesticide use, and combustion of chlorine-containing organic products, polluting the atmosphere, soil, groundwater, and surface water. Trichloroethylene not only pollutes the environment, but also has a great impact on human health. It has "three-hazard" effects. Its degradation products, dichloroethylene and vinyl chloride, are also toxic carcinogens that threaten human health. It is necessary to pay attention to and control the pollution of trichloroethylene to the environment.

[0021] PCBs are fine chemical products that are widely used in the power industry, plastic processing industry, chemical industry, printing industry, etc. PCBs are persistent organic pollutants that can accumulate and transmit in organisms and exist in ecosystems for a long time, posing threats and challenges to human reproduction and sustainable development.

[0022] Chlorobenzene can be used as a solvent and is often used to synthesize phenol, nitrochlorobenzene, dinitrochlorobenzene, dinitrophenol and picric acid. In addition, chlorobenzene can also be used to synthesize dyes, pesticide raw materials, medicines, explosives, rubber additives, paints, quick-drying inks and dry cleaning agents. Chlorobenzene is seriously harmful to the environment and can cause pollution to water, soil and air.

[0023] The present invention provides application of the biochar-nano iron-based composite material obtained by the preparation method in in-situ remediation of organic pollution in soil or water.

[0024] Preferably, the organic pollution is halogenated hydrocarbons and / or benzene pollution.

[0025] Preferably, the halogenated hydrocarbon is trichloroethylene, and the benzene series compound is chlorobenzene and / or polychlorinated biphenyls.

[0026] Compared with the prior art, the unexpected technical effects achieved by the present invention are mainly reflected in the following two aspects:

[0027] 1) The biochar-nano iron-based composite material of the present invention can effectively reduce organic pollution in soil or water, and has a significant removal effect on trichloroethylene, chlorobenzene and polychlorinated biphenyls.

[0028] 2) The biochar-nano iron-based composite material of the present invention realizes the recycling of waste biostraw, is safe and environmentally friendly, has a small amount of use, has a high efficiency in removing organic pollution, is highly practical, is conducive to large-scale promotion, and has broad economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for the specific implementation methods are briefly introduced below.

[0030] Figure 1 Removal effect of different biochar-nano iron-based composites on trichloroethylene.

[0031] Figure 2 Removal effect of different biochar-nano iron-based composite materials on soil polychlorinated biphenyls

[0032] Compared with Example 1, *** P < 0.001, **** P<0.0001.

[0033] Figure 3 Removal effect of different biochar-nano iron-based composites on chlorobenzene. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. The test reagents used in the following embodiments, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0035] Example 1

[0036] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0037] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, and pyrolyzed for 3 hours under oxygen-limited conditions. The corn stalks were taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0038] The biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, and ultrasonically treated for 25 minutes at an ultrasonic power of 350W; the ultra-high pressure microfluidizer was used for treatment for 4 minutes at a treatment pressure of 160 MPa and a treatment temperature of 25°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0039] Example 2

[0040] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0041] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 400°C at a rate of 10°C / min in a N2 atmosphere, oxygen-limited pyrolysis for 4 hours, taken out, cooled, ground through a 200-mesh sieve, and dried at 80°C to obtain biochar.

[0042] The biochar and α-Fe2O3 were mixed in a mass ratio of 8:1, and ultrasonically treated for 35 minutes at an ultrasonic power of 300 W; the ultra-high pressure microfluidizer was used for treatment for 3 minutes at a treatment pressure of 170 MPa and a treatment temperature of 30°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0043] Example 3

[0044] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0045] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 450°C at a rate of 12°C / min in a N2 atmosphere, pyrolyzed for 2 hours under oxygen-limited conditions, taken out, cooled, ground through a 200-mesh sieve, and dried at 70°C to obtain biochar.

[0046] The biochar and α-Fe2O3 were mixed in a mass ratio of 7:1, and ultrasonically treated for 20 minutes at an ultrasonic power of 300 W; the ultra-high pressure microfluidizer was used for treatment for 5 minutes at a treatment pressure of 140 MPa and a treatment temperature of 20°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0047] Example 4

[0048] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0049] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 450°C at a rate of 15°C / min in a N2 atmosphere, and pyrolyzed in oxygen-limited conditions for 2.5 hours. The corn stalks were taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0050] The biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, and ultrasonically treated for 25 minutes at an ultrasonic power of 330 W; the ultra-high pressure microfluidizer was used for treatment for 5 minutes at a treatment pressure of 150 MPa and a treatment temperature of 28°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0051] Comparative Example 1

[0052] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, and pyrolyzed for 3 hours under oxygen-limited conditions. The corn stalks were taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0053] Comparative Example 2

[0054] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0055] The washed peanut shells were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min under N2 atmosphere, oxygen-limited pyrolysis for 3 hours, taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0056] The biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, and ultrasonically treated for 25 minutes at an ultrasonic power of 350W; the ultra-high pressure microfluidizer was used for treatment for 4 minutes at a treatment pressure of 160 MPa and a treatment temperature of 25°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0057] Compared with Example 1, the difference is that the raw material for preparing biochar is peanut shell.

[0058] Comparative Example 3

[0059] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0060] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, and pyrolyzed for 3 hours under oxygen-limited conditions. The corn stalks were taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0061] The biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, and ultrasonically treated for 25 minutes at an ultrasonic power of 350W; the ultra-high pressure microfluidizer was used for treatment for 2 minutes at a treatment pressure of 120 MPa and a treatment temperature of 35°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0062] Compared with Example 1, the difference lies in that the ultra-high pressure microfluidization homogenization treatment parameters are different.

[0063] Comparative Example 4

[0064] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0065] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, and pyrolyzed for 3 hours under oxygen-limited conditions. The corn stalks were taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0066] The biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, treated with an ultra-high pressure microfluidizer for 4 minutes at a pressure of 160 MPa and a temperature of 25°C, and ultrasonically treated for 25 minutes at a power of 350 W to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0067] Compared with Example 1, the difference is that the order of ultrahigh pressure microfluidization homogenization treatment and ultrasonic treatment is different.

[0068] Comparative Example 5

[0069] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0070] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, and pyrolyzed for 3 hours under oxygen-limited conditions. The corn stalks were taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0071] Biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, and ultrasonically treated for 25 minutes at an ultrasonic power of 350 W; the mixture was placed in a stainless steel grinding jar, and the grinding balls: mixture were placed in the jar and sealed at a mass ratio of 35:1. The jar was run at a speed of 550 r / min for 6 hours, and the rotation direction was changed every 0.5 hours to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0072] Compared with Example 1, the difference is that the ultra-high pressure microfluidization homogenization treatment is replaced by a ball milling method.

[0073] Comparative Example 6

[0074] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0075] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, and pyrolyzed for 3 hours under oxygen-limited conditions. The corn stalks were taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0076] The biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, treated with an ultra-high pressure microfluidizer for 4 minutes at a pressure of 160 MPa and a temperature of 25°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0077] Compared with Example 1, the difference is that no ultrasonic treatment is performed.

[0078] Comparative Example 7

[0079] A biochar-nano iron-based composite material for organic pollution remediation, the preparation method is as follows:

[0080] The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, and pyrolyzed for 3 hours under oxygen-limited conditions. The corn stalks were taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar.

[0081] The biochar and α-Fe2O3 were mixed in a mass ratio of 4:1, and ultrasonically treated for 25 minutes at an ultrasonic power of 350W; the ultra-high pressure microfluidizer was used for treatment for 4 minutes at a treatment pressure of 160 MPa and a treatment temperature of 25°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

[0082] Compared with Example 1, the difference is that the ratio of biochar to α-Fe2O3 is different.

[0083] Effect Example 1 Removal of trichloroethylene by the biochar-nano iron-based composite material of the present invention

[0084] Prepare a trichloroethylene solution with an initial concentration of 10 mg / L. Under anaerobic conditions, take the biochar-nano iron-based composite materials of Example 1, Comparative Example 1, Comparative Example 5, and Comparative Example 6 and add them to the reaction bottle containing trichloroethylene solution, so that the dosage of the biochar-nano iron-based composite material is 1.5 g / L. Put the reaction bottle into a constant temperature oscillator at 25°C and 70 rpm to carry out dechlorination reaction. Every 20 minutes, use a sampling needle to take 100 μL of gas sample from the top space, use gas chromatography to determine the trichloroethylene in the system, and calculate the removal rate. The removal results are as follows: Figure 1 shown.

[0085] The biochar-nano iron-based composite material of Example 1 has a significant removal effect on trichloroethylene, and the removal efficiency reaches 100% after 100 minutes. The biochar of Comparative Example 1, Comparative Example 5, and Comparative Example 6 have a certain removal effect on trichloroethylene. When treated for 100 minutes, the removal rates are 40.2%, 65.0%, and 53.5%, respectively. The removal effect of the biochar of Comparative Example 1, Comparative Example 5, and Comparative Example 6 on trichloroethylene is worse than that of the biochar-nano iron-based composite material of Example 1.

[0086] The biochar-nano iron-based composite material prepared by the method of the present invention has a better repair effect on organic contaminated soil than the biochar-nano iron-based composite material obtained by mechanical ball milling. Without ultrasonic treatment, the prepared biochar-nano iron-based composite material has a poor removal effect on trichloroethylene. The removal effect of biochar alone on trichloroethylene is worse than that of the biochar-nano iron-based composite material of the present invention. The biochar-nano iron-based composite material of the present invention achieves a synergistic effect and significantly enhances the removal effect on trichloroethylene.

[0087] Effect Example 2 Removal of Polychlorinated Biphenyls by the Biochar-Nano Iron-based Composite Material of the Present Invention

[0088] 1. Methods and Materials

[0089] The test soil was from the surface soil of agricultural land, air-dried indoors, and impurities such as gravel and animal and plant remains were removed, and ground to a diameter of less than 60 mesh. The soil is yellow soil, composed of 10.5% sand, 87.1% silt and 2.4% clay, with an organic matter content of 3.3%, a pH value of 6.3, and a water holding capacity of 50.3%.

[0090] Preparation method of polychlorinated biphenyl contaminated soil: dilute 1 mL of 2,4,4-trichlorobiphenyl (1 g / L) with 5 mL of acetone and add it to 10 g of clean soil; after the acetone is completely evaporated, mix it thoroughly with another 990 g of clean soil and leave it for 24 hours to obtain 1 mg / kg 2,4,4-trichlorobiphenyl contaminated soil.

[0091] The soil was treated with the biochar-nano iron-based composite materials of Examples 1-2 and Comparative Examples 2-4.

[0092] 0.75 g of the biochar-nano iron-based composite materials of Examples 1-2 and Comparative Examples 2-4 were added to 500 g of contaminated soil respectively, and the mixture was fully mixed by mechanical stirring to make the concentration of the biochar-nano iron-based composite materials in the soil reach 1.5 g / kg. After treatment for 4 days, the removal rate of soil polychlorinated biphenyls by the biochar-nano iron-based composite materials was calculated.

[0093] Set up a blank treatment group without any treatment.

[0094] 2. Data processing

[0095] The sample determination was repeated 3 times, and the results were expressed as mean ± standard deviation. SPSS22.0 was used for one-way analysis of variance to analyze the significant differences between the soil PCB removal rate data in each treatment group, and p < 0.05 indicated a significant difference.

[0096] 3. Results

[0097] like Figure 2 As shown in the blank treatment group, the average removal efficiency of PCBs in soil was low, only 5.2%, and the volatilization or microbial degradation of PCBs under natural conditions was very limited.

[0098] The biochar-nano iron-based composite materials of Example 1-2 have obvious effects on the restoration of PCB-contaminated soil, with average removal efficiencies of 95.7% and 91.3%. The biochar-nano iron-based composite materials of Comparative Example 2-4 have certain effects on the restoration of PCB-contaminated soil, with average removal efficiencies of 57.5%, 67.5%, and 54.2%, respectively. The restoration effect of the biochar-nano iron-based composite materials of Comparative Example 2-4 on PCB-contaminated soil is worse than that of the biochar-nano iron-based composite materials of Example 1-2.

[0099] The inventors determined the remediation effects of the biochar-nano iron-based composite materials of Examples 3 and 4 on polychlorinated biphenyl-contaminated soil according to the method of Effect Example 2. The removal efficiencies of the biochar-nano iron-based composite materials of Examples 3 and 4 on polychlorinated biphenyl-contaminated soil were 92.7% and 93.8%.

[0100] Biochar is a new type of porous carrier material with high porosity and large specific surface area. Different raw materials used will greatly affect the adsorption properties of biochar-nano iron-based composites.

[0101] The operating parameters of the ultra-high pressure micro-jet homogenizer are the key technical parameters for preparing biochar-nano iron-based composite materials. The operating pressure of the ultra-high pressure micro-jet homogenizer is lower than 140Mpa, and the processing time is lower than 3min. The resulting biochar-nano iron-based composite material has a poorer repair effect on organically contaminated soil than the biochar-nano iron-based composite material prepared by the method of the present invention.

[0102] After the biochar of the present invention is mixed with iron oxides, the order of ultrasonic treatment and ultra-high pressure microfluidization homogenization treatment will also affect the repair effect of the biochar-nano iron-based composite material on organic contaminated soil.

[0103] Effect Example 3 Removal of Chlorobenzene by the Biochar-Nano Iron-based Composite Material of the Present Invention

[0104] Prepare a single solution of chlorobenzene with a concentration of 100 mg / L. Under anaerobic conditions, add the biochar-nano iron-based composite materials of Example 1 and Comparative Example 7 to a reaction bottle containing chlorobenzene solution, with a dosage of 1.5 g / L. Place the reaction bottle in a 25°C constant temperature oscillator at 70 rpm for dechlorination reaction. After 100 minutes, use liquid chromatography to determine the chlorobenzene in the system and calculate the removal rate. The removal results are as follows: Figure 3 shown.

[0105] The biochar-nano iron-based composite material of Example 1 has a significant removal effect on chlorobenzene, and the removal efficiency reaches 100% in 100 minutes. The removal rate of the biochar-nano iron-based composite material of Comparative Example 7 is 60.5%. The removal effect of the biochar-nano iron-based composite material of Comparative Example 7 on chlorobenzene is worse than that of the biochar-nano iron-based composite material of Example 1.

[0106] There is an optimal ratio for the iron loading on biochar. If there is too much iron, it will clog the pores of the biochar, thus affecting the specific surface area, and ultimately leading to a decrease in the ability to remove pollutants.

[0107] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0108] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A biochar-nano iron-based composite material for organic pollution remediation, the preparation method of which is as follows: The biochar and iron oxide are mixed, and ultrasonically treated for 20-35 minutes with an ultrasonic power of 300-400W; treated with an ultra-high pressure microfluidizer for 3-5 minutes with a treatment pressure of 140-170Mpa and a treatment temperature of 20-30°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3; the mass ratio of the biochar to the iron oxide is 6:1-8:

1.

2. The biochar-nano iron-based composite material for organic pollution remediation according to claim 1, characterized in that: The preparation method of the biochar is as follows: the washed corn stalks are dried, crushed, placed in a muffle furnace, heated to 400°C-450°C at a rate of 10-15°C / min under a N2 atmosphere, oxygen-limited pyrolysis for 2-4h, taken out, cooled, ground through a 200-mesh sieve, and dried at 70-80°C.

3. The biochar-nano iron-based composite material for organic pollution remediation according to claim 1, characterized in that: The iron oxide is Fe2O3.

4. The biochar-nano iron-based composite material for organic pollution remediation according to claim 1, characterized in that: The iron oxide is α-Fe2O3.

5. A biochar-nano iron-based composite material for organic pollution remediation, the preparation method of which is as follows: 1) The washed corn stalks were dried, crushed, placed in a muffle furnace, heated to 420°C at a rate of 15°C / min in a N2 atmosphere, pyrolyzed for 3 hours in an oxygen-limited manner, taken out, cooled, ground through a 200-mesh sieve, and dried at 75°C to obtain biochar; 2) The biochar and α-Fe2O3 were mixed in a mass ratio of 6:1, and ultrasonically treated for 25 minutes at an ultrasonic power of 350 W; ultra-high pressure microfluidizer was used for treatment for 4 minutes at a treatment pressure of 160 MPa and a treatment temperature of 25°C to obtain a biochar-nano iron-based composite material including biochar-Fe2O3.

6. Use of the biochar-nano iron-based composite material according to any one of claims 1 to 5 in in-situ remediation of organic pollution in soil or water.

7. The use according to claim 6, characterized in that: The organic pollution is halogenated hydrocarbons and / or benzene pollution.

8. The use according to claim 7, characterized in that: The halogenated hydrocarbon is trichloroethylene, and the benzene series is chlorobenzene and / or polychlorinated biphenyls.

Citation Information

Patent Citations

  • Biological activated carbon composite material and application thereof

    CN104549155A

  • Application of zero-valent iron-loaded biochar in wastewater treatment

    CN111573813A

  • Biochar for sludge composting treatment and preparation method of biochar

    CN111732463A

  • Biochar-loaded iron material for oxidizing and repairing organic pollution of soil water body as well as preparation method and application of biochar-loaded iron material

    CN113061441A

  • Iron-based biochar material, preparation therefor and use thereof in soil pollution control

    US20170282229A1

Cited By

  • Composite pollution repairing agent as well as preparation method and application thereof

    CN120903598A

  • Composite pollution remediation agent, preparation method and application thereof

    CN120903598B

  • Iron oxide composite material and preparation method and application thereof

    CN121847065A