Thioether functionalized limited geometric configuration rare earth complex and preparation method thereof as well as multi-component copolymer and preparation method thereof
By limiting the use of rare earth complex catalysts with restricted sulfide functionalization, the shortcomings of conventional conjugated diene rubbers in ozone resistance and crack growth resistance were solved, and a multi-component copolymer with high tensile strength and low temperature resistance was prepared to meet the performance requirements of tire materials.
Patent Information
- Application Number
- CN202410927053.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
In the existing technology, conventional conjugated diene rubbers such as butadiene rubber and styrene-butadiene rubber are insufficient in resisting crack growth caused by ozone and climate change, and are difficult to meet the requirements of high tensile strength, low temperature resistance and crack growth resistance.
A rare earth complex with a restricted geometry and sulfide functionalization was used as the main catalyst to form a catalytic system with organoboron salts and organoaluminum compounds. This system was used for the copolymerization of α-olefins, butadiene, and styrene or styrene derivatives to prepare multi-component copolymers, thereby improving the performance of the materials.
The prepared multi-component copolymer improved the material's high tensile strength, low-temperature resistance, and ozone resistance, and enhanced its resistance to crack growth, thus meeting the energy-saving and safety requirements of tires.
Smart Images

Figure CN118894891A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymers, and in particular to a thioether functionalized restricted geometry rare earth complex, a preparation method thereof, and a multi-component copolymer, and a preparation method thereof. Background Art
[0002] Elastomeric materials are used in various fields due to their excellent mechanical properties. In recent years, the performance requirements of elastomeric materials have become increasingly diverse, and elastomeric materials with excellent properties are expected to appear, such as high tensile strength, high elongation at break, low temperature resistance, crack growth resistance, ozone resistance, etc. For example: by regulating the vinyl content and styrene monomer sequence distribution in butadiene, and tackling technical problems such as molecular chain end modification, a solution-polymerized styrene-butadiene rubber is prepared that takes into account both rolling resistance and wet skid resistance and better meets the energy-saving and safety requirements of tires. However, conventional conjugated diene rubbers such as butadiene rubber (BR) and styrene-butadiene rubber (SBR) have excellent wear resistance, etc., but do not have resistance to crack growth caused by ozone and climate change. Therefore, in order to meet the above requirements, patent document WO2012014455A1 discloses a copolymer of a conjugated diene compound and a non-conjugated olefin, wherein the conjugated diene portion (the portion derived from the conjugated diene compound) has a cis-1,4 bond content greater than 70.5 mol% and contains more than 10 mol% of a non-conjugated olefin, and the copolymer is used to manufacture a rubber having good properties such as resistance to crack growth.
[0003] Patent document CN108137745A discloses a multi-component copolymer, a rubber composition, and a cross-linked rubber composition. The catalyst structure used in the examples is a bis-indene metallocene rare earth catalyst containing a substituent, and the content of butadiene units in the obtained copolymer is 8-48 mol%.
[0004] The catalysts used in the above patent documents for copolymerization of non-conjugated dienes, conjugated dienes and aromatic compounds are mainly monoclinic rare earth catalysts, while there are no reports on the use of restricted geometry rare earth catalysts for copolymerization of conjugated dienes, non-conjugated dienes and aromatic vinyl. Summary of the invention
[0005] The technical problem solved by the invention is a thioether functionalized restricted geometry rare earth complex, which can be used as a main catalyst for multi-component copolymers and can be used for copolymerization of alpha-olefins, butadiene and styrene or styrene derivatives.
[0006] In view of this, the present application provides a thioether functionalized constrained geometry rare earth complex as shown in formula (I),
[0007]
[0008] wherein Cp is a substituted or unsubstituted cyclopentadienyl, a substituted or unsubstituted indenyl, a substituted or unsubstituted fluorenyl, or a substituted or unsubstituted heteroatom-fused cyclopentadienyl;
[0009] R 1 , R 2 , R 3 , R 4 are independently selected from hydrogen, halogen, methyl, ethyl, isopropyl, tert-butyl or phenyl;
[0010] R is selected from methyl, ethyl, isopropyl, tert-butyl, phenyl or substituted phenyl;
[0011] Ln is a rare earth element;
[0012] X 1 , X 2 independently selected from monoanionic ligands;
[0013] L is a neutral Lewis base;
[0014] w is an integer from 0 to 3.
[0015] Preferably, the monoanionic ligand is selected from CH 2 SiMe 3 、CH(SiMe 3 ) 2 , CH 2 C 6 H 4 NMe 2 -o, 1, 3-C 3 H 5 、1,3-C 3 H 4 (Me) or 1,3-C 3 H 3 (SiMe 3 ) 2 ; The neutral Lewis base is selected from tetrahydrofuran, diethyl ether, ethylene glycol dimethyl ether or pyridine; and the Ln is selected from Sc, Y, Lu, La, Nd, Sm, Gd, Tb, Dy, Er, Tm or Yb.
[0016] Preferably, the structural formula of the rare earth complex is as shown in Complex 1, Complex 2, Complex 3, Complex 4, Complex 5, Complex 6, Complex 7 or Complex 8:
[0017]
[0018] Preferably, the preparation method of the rare earth complex is specifically as follows:
[0019] The anisyl thioether as shown in formula (III) is reacted with n-butyl lithium in a solvent, and then a cyclopentenone compound is added, heated under reflux for reaction, and dehydrated after the reaction is completed to obtain a thioether-functionalized cyclopentadiene ligand;
[0020] reacting the cyclopentadiene ligand with a trialkyl rare earth to obtain a rare earth complex;
[0021]
[0022] Wherein, R is selected from methyl, ethyl, isopropyl, tert-butyl, phenyl or substituted phenyl.
[0023] The present application also provides a multi-component copolymer, which is prepared from α-olefin, conjugated diene and styrene or styrene derivative under the action of a catalytic system;
[0024] The catalytic system is composed of an organic boron salt compound, an organic aluminum compound and a rare earth complex, and the rare earth complex is the rare earth complex described above.
[0025] Preferably, the organic boron salt compound is an ionic compound composed of an organic boron anion and a cation; the organic boron anion is selected from tetraphenylborate, tetrakis(monofluorophenyl)borate, tetrakis(difluorophenyl)borate, tetrakis(trifluorophenyl)borate, tetrakis(tetrafluorophenyl)borate, tetrakis(pentafluorophenyl)borate, tetrakis(tetrafluoromethylphenyl)borate, tetrakis(tolyl)borate, tetrakis(xylyl)borate, (triphenyl, pentafluorophenyl)borate, [tris(pentafluorophenyl) , phenyl] borate or undecyl-7, 8-dicarbon undecyl borate; the cation is selected from a carbonium cation, an oxonium cation, an ammonium cation, a phosphonium cation, a cycloheptatrienyl cation or a ferrocenium cation containing a transition metal, the carbonium cation comprises a triphenylcarbonium cation or a tri(substituted phenyl)carbonium cation, the ammonium cation comprises a trialkylammonium cation, an N,N-dialkylanilinium cation or a dialkylammonium cation, and the phosphonium cation comprises a triarylphosphonium cation;
[0026] The organoaluminum compound is selected from trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, triisopropylaluminum, triisobutylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum, triphenylaluminum, tri-p-tolylaluminum, tribenzylaluminum, ethyldibenzylaluminum or ethyldi(p-tolyl)aluminum;
[0027] The molar ratio of the organic boron salt compound to the rare earth complex is 0.3:10 to 10:1, and the molar ratio of the organic aluminum compound to the rare earth complex is 2:1 to 300:1.
[0028] Preferably, the melting point of the α-olefin is 70-130° C. or has no melting point, and the α-olefin is selected from ethylene, propylene or 1-butene; the melting point of the styrene or styrene derivative is 220-260° C. or has no melting point.
[0029] Preferably, in the main chain of the multi-polymer, the insertion rate of the styrene or styrene derivative is 10-40 mol%, the insertion rate of the conjugated diene is 20-80 mol%, and the insertion rate of the α-olefin is 10-60 mol%; the regioselectivity of the conjugated diene is that the cis-1,4-content is greater than 75 mol%; the number average molecular weight of the multi-polymer is greater than 20,000, and the molecular weight distribution of the multi-polymer is 1-10.
[0030] The present application also provides a method for preparing a multi-component copolymer, comprising:
[0031] Initiating polymerization of α-olefin, conjugated diene and styrene or styrene derivative in a reaction medium under a catalytic system to obtain a multi-component copolymer;
[0032] The catalytic system is composed of an organic boron salt compound, an organic aluminum compound and a rare earth complex, and the rare earth complex is the rare earth complex described above.
[0033] Preferably, the polymerization reaction temperature is -40 to 100°C, the polymerization reaction is carried out at 1 to 20 atmospheres, and the reaction medium is selected from one or more of aliphatic saturated hydrocarbons, aromatic hydrocarbons, aromatic halides and cycloalkanes.
[0034] The present application provides a thioether functionalized constrained geometry rare earth complex as shown in formula (I), which is used as the main catalyst of a multi-copolymer, and forms a catalytic system with an organic boron salt compound and an organic aluminum compound to copolymerize α-olefin, butadiene and styrene or styrene derivatives. The insertion rate of styrene or styrene derivatives in the obtained multi-copolymer is 10-40 mol%, the insertion rate of conjugated diene is 20-80 mol%, and the insertion rate of α-olefin is 10-60 mol%. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The ligand L2 prepared in Example 1-1 of the present invention 1 H NMR spectrum;
[0036] Figure 2 The ligand L3 prepared in Example 1-1 of the present invention 1 H NMR spectrum;
[0037] Figure 3 The ligand L4 prepared in Example 1-1 of the present invention 1 H NMR spectrum;
[0038] Figure 4 The complex Lu-L2 prepared in Example 1-2 of the present invention 1 H NMR spectrum;
[0039] Figure 5 The complex Y-L3 prepared in Example 1-2 of the present invention 1 H NMR spectrum;
[0040] Figure 6 The complex Lu-L4 prepared in Example 1-2 of the present invention 1 H NMR spectrum;
[0041] Figure 7 The copolymer sample prepared in Example 2-1 of the present invention is 1 H NMR spectrum. DETAILED DESCRIPTION
[0042] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0043] In the present application, a thioether functionalized constrained geometry rare earth complex as shown in formula (I) is first provided.
[0044]
[0045] wherein Cp is a substituted or unsubstituted cyclopentadienyl, a substituted or unsubstituted indenyl, a substituted or unsubstituted fluorenyl, or a substituted or unsubstituted heteroatom-fused cyclopentadienyl;
[0046] R 1 , R 2 , R 3 , R 4 are independently selected from hydrogen, halogen, methyl, ethyl, isopropyl, tert-butyl or phenyl;
[0047] R is selected from methyl, ethyl, isopropyl, tert-butyl, phenyl or substituted phenyl;
[0048] Ln is a rare earth element;
[0049] X 1 , X 2 independently selected from monoanionic ligands;
[0050] L is a neutral Lewis base;
[0051] w is an integer from 0 to 3.
[0052] In the rare earth complex, the substituent in the indenyl, cyclopentadienyl or fluorenyl in the Cp can be selected from methyl or ethyl, and in a specific embodiment, the substituent is methyl; the substituent in the substituted heteroatom-fused cyclopentadienyl is selected from methyl, ethyl, isopropyl, tert-butyl or trimethylsilane, and the heteroatom is selected from S or N.
[0053] In a specific embodiment, the R 1 , R 2 , R 3 , R 4 are independently selected from hydrogen; and said Ln is selected from Y, Lu, Gd, Sc or Nd.
[0054] The X 1 , X 2 Independently selected from monoanionic ligands; the monoanionic ligands are selected from CH 2 SiMe 3 、CH(SiMe 3 ) 2 , CH 2 C 6 H 4 NMe 2 -o, 1, 3-C 3 H 5 、1,3-C 3 H 4 (Me) or 1,3-C 3 H 3 (SiMe 3 ) 2 .
[0055] The L is a neutral Lewis base, specifically, the neutral Lewis base is selected from tetrahydrofuran, ether, ethylene glycol dimethyl ether or pyridine; in a specific embodiment, the neutral Lewis base is selected from tetrahydrofuran. The w is selected from 0, 1, 2 or 3.
[0056] The R is selected from methyl, ethyl, isopropyl or benzyl.
[0057] More specifically, the structural formula of the rare earth complex is shown in Complex 1, Complex 2, Complex 3, Complex 4, Complex 5, Complex 6, Complex 7 or Complex 8:
[0058]
[0059] The present application also provides a method for preparing the rare earth complex, specifically:
[0060] The anisyl thioether as shown in formula (III) is reacted with n-butyl lithium in a solvent, and then a cyclopentenone compound is added, heated under reflux for reaction, and dehydrated after the reaction is completed to obtain a thioether-functionalized cyclopentadiene ligand;
[0061] reacting the cyclopentadiene ligand with a trialkyl rare earth to obtain a rare earth complex;
[0062]
[0063] In the process of preparing the rare earth complex, the solvent can be selected from tetrahydrofuran, the n-butyl lithium can be specifically selected from n-butyl lithium-n-hexane solution, and the reaction time is 1 to 5 hours; the cyclopentenone is selected according to the substituent of Cp in the rare earth complex; for example, the anisole is selected from the following specific compounds, and the cyclopentenone is selected from the following specific compounds; the heating reflux reaction time is 12 to 24 hours.
[0064]
[0065] On the basis of the above-mentioned complex 1, complex 2, complex 3, complex 4, complex 5, complex 6, complex 7 and complex 8, the above-mentioned thioanisole and the above-mentioned cyclopentenone compound are specifically selected as described above.
[0066] The above reaction formula is specifically shown as follows:
[0067]
[0068] The present application then reacts the cyclopentadiene ligand with a trialkyl rare earth to obtain a rare earth complex; the solvent of the reaction is selected from one or more of n-hexane, tetrahydrofuran, toluene, ether and dichloromethane, and the reaction time is 12 to 24 hours.
[0069] The present application also provides a multi-component copolymer, which is prepared from α-olefin, conjugated diene and styrene or styrene derivative under the action of a catalytic system;
[0070] The catalytic system is composed of an organic boron salt compound, an organic aluminum compound and a rare earth complex, and the rare earth complex is the rare earth complex described in the above scheme.
[0071] In the multi-polymer, the catalytic system is specifically composed of an organic boron salt compound, an organic aluminum compound and a rare earth metal complex. The organic boron salt compound can be an ionic compound composed of an organic boron anion and a cation; the organic boron anion is selected from tetraphenylborate ([BPh 4 ] - ), tetrakis(monofluorophenyl)borate, tetrakis(difluorophenyl)borate, tetrakis(trifluorophenyl)borate, tetrakis(tetrafluorophenyl)borate, tetrakis(pentafluorophenyl)borate ([B(C 6 F 5 ) 4 ] -), tetrakis(tetrafluoromethylphenyl)borate, tetrakis(tolyl)borate, tetrakis(xylyl)borate, (triphenyl, pentafluorophenyl)borate, [tri(pentafluorophenyl), phenyl]borate or undecyl-7,8-dicarbonyl borate; the cation is selected from carbonium cations, oxonium cations, ammonium cations, phosphonium cations, cycloheptatrienyl cations or ferrocenium cations containing transition metals, the carbonium cations include trisubstituted carbonium cations such as and tri(substituted phenyl)carbonium cations, wherein the trisubstituted carbonium cation is selected from triphenylcarbonium cations ([Ph 3 C] + ), the tri(substituted phenyl)carbonium cation is selected from tri(tolyl)carbonium cation; the ammonium cation includes trialkylammonium cation, N,N-dialkylanilinium cation or dialkylammonium cation, wherein the trialkylammonium cation is specifically selected from trimethylammonium cation, triethylammonium cation ([NEt 3 H] + ), tripropylammonium cation or tributylammonium cation; the N,N-dialkylanilinium cation is specifically selected from N,N-dimethylanilinium cation ([PhNMe 2 H] + ), N,N-diethylanilinium cation or N,N-2,4,6-pentamethylanilinium cation; the dialkylammonium cation is selected from diisopropylammonium cation or dicyclohexylammonium cation; the phosphonium cation includes a triarylphosphonium cation, wherein the triarylphosphonium cation is selected from triphenylphosphonium cation, tri(tolyl)phosphonium cation or tri(xylyl)phosphonium cation.
[0072] The organic boron salt compound can be specifically selected from [Ph 3 C][B(C 6 F 5 ) 4 ]、[PhNMe 2 H][BPh 4 ]、[NEt 3 H][BPh 4 ]、[PhNMe 2 H][B(C 6 F 5 ) 4 ] etc.; organic boron compounds with the same functions as organic boron salt compounds can also be used, such as B(C 6 F 5 ) 3 .
[0073] The organoaluminum compound may be selected from trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, triisopropylaluminum, triisobutylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum, triphenylaluminum, tri-p-tolylaluminum, tribenzylaluminum, ethyldibenzylaluminum or ethyldi(p-tolyl)aluminum.
[0074] In the catalytic system, the molar ratio of the organic boron salt compound to the rare earth complex is 0.3:10 to 10:1. In a specific embodiment, the molar ratio of the organic boron salt compound to the rare earth complex is 0.5:1 to 5:1. More specifically, the molar ratio of the organic boron salt compound to the rare earth complex is 1:1 to 3:1. The molar ratio of the organic aluminum compound to the rare earth complex is 2:1 to 300:1. Specifically, the molar ratio of the organic aluminum compound to the rare earth complex is 5:1 to 100:1. More specifically, the molar ratio of the organic aluminum compound to the rare earth complex is 10:1 to 80:1; more specifically, the molar ratio of the organic aluminum compound to the rare earth complex is 20:1 to 50:1.
[0075] The multi-polymer is a multi-block copolymer; the main chain of the multi-polymer comprises an α-olefin unit, a conjugated diene unit and a styrene or derivative unit, the insertion rate of the styrene or styrene derivative is 10-40 mol%, the insertion rate of the conjugated diene is 20-80 mol%, and the insertion rate of the α-olefin is 10-60 mol%; the regioselectivity of the conjugated diene is that the cis-1,4-content is greater than 75 mol%; specifically, the insertion rate of the styrene or styrene derivative is 12-38 mol%, the insertion rate of the conjugated diene is 40-78 mol%, and the insertion rate of the α-olefin is 12-40 mol%; the regioselectivity of the conjugated diene is that the cis-1,4-content is greater than 78-85 mol%.
[0076] Preferably, the conjugated diene compound is selected from 1,3-butadiene, isoprene or 2,3-dimethyl-1,3-butadiene.
[0077] Preferably, the α-olefin compound is selected from ethylene, propylene or 1-butene.
[0078] Preferably, the styrene compound is selected from the following specific compounds:
[0079]
[0080] Preferably, the melting point of the α-olefin structural unit of the multi-polymer is 70-120° C. or has no melting point; the melting point of the styrene and derivative structural unit is 220-260° C. or has no melting point.
[0081] Preferably, the number average molecular weight of the multi-polymer is greater than 20,000, and the molecular weight distribution of the multi-polymer is 1 to 10; specifically, the number average molecular weight of the multi-polymer is 90,000 to 135,000, and the molecular weight distribution of the multi-polymer is 1.3 to 2.5.
[0082] The present invention also provides a method for preparing a multi-component copolymer, comprising:
[0083] The alpha-olefin compound, the conjugated diene compound, the styrene and the derivative compound are initiated to polymerize in a reaction medium under a catalytic system to obtain a multi-component copolymer.
[0084] In the above process of preparing the multi-polymer, the raw materials have been described in detail above and will not be repeated here.
[0085] In the above-mentioned multi-copolymer preparation process, the polymerization reaction temperature can be carried out at a very low temperature (such as -40°C) to a higher temperature (such as 100°C); in a specific embodiment, the polymerization temperature is preferably 10°C to 100°C, more preferably 25°C to 100°C, and more preferably 25°C to 80°C. The polymerization reaction of the present application can be carried out at 1 to 20 atmospheres, preferably at 1 to 10 atmospheres, and more preferably at 1 to 6 atmospheres. The reaction medium is carried out in a hydrocarbon solvent, specifically, the hydrocarbon solvent contains aliphatic saturated hydrocarbons, aromatic hydrocarbons, aromatic halides or cycloalkanes, preferably one or more of hexane, cyclohexane, petroleum ether, benzene, toluene, xylene, chlorobenzene, dichlorobenzene and bromobenzene.
[0086] The multi-polymer of the present application or the multi-polymer prepared by the above method can be used to prepare vinyl rubber.
[0087] In order to further understand the present invention, a thioether functionalized restricted geometry rare earth complex, its preparation method and multi-polymer, and its preparation method provided by the present invention are described in detail below in conjunction with the examples. The protection scope of the present invention is not limited by the following examples.
[0088] Example 1-1
[0089] This embodiment involves the preparation of ligands L1 to L12, wherein the preparation process of ligand L1 is as follows:
[0090] At room temperature, 1.00 g (4.92 mmol) of 2-bromothioanisole was dissolved in 24 ml of tetrahydrofuran solvent, and the mixture was transferred to -40 °C low temperature, and n-butyl lithium (2.5 M n-butyl lithium-n-hexane solution, 3 ml) was slowly added thereto for 4 h. Then, 2,3,4,5-tetramethylcyclopentenone (0.68 g, 4.92 mmol) was added dropwise to the system, and the temperature was slowly raised. The mixture was heated under reflux for 24 h, and hydrochloric acid (10 ml, mass concentration of 37%) was added for dehydration. The mixture was dried with an appropriate amount of anhydrous magnesium sulfate, and recrystallized at low temperature to obtain 0.35 g (yield 29%) of ligand L1 as a yellow-white solid, with a molecular formula of C 6 H 19 S, the reaction formula is as follows:
[0091]
[0092] By replacing appropriate reactants, ligands L2 to L7 were prepared, as shown in Table 1 below:
[0093] Table 1 Ligand structure prepared in Example 1-1 of the present invention
[0094]
[0095]
[0096] The H NMR spectra and elemental analysis data of ligands L2 to L7 are as follows:
[0097] Ligand L2 1 H NMR (500 MHz, CDCl 3 , 25℃)(e.g. Figure 1 ): δ7.41(dd,J=1.4Hz,0.5H),7.39(dd,J=3.5Hz,0.5H),7.20(dd,J=7.5,1.4Hz,2H),7.05(td ,J=8.6,1.3Hz,2H),6.94(s,1H),3.14(dd,J=64.0,22.2Hz,2H),2.02(s,3H),2.00(s,3H)ppm;
[0098] The ligand L2 obtained in Example 1-1 was analyzed by elemental analysis, and the molecular formula was C 15 H 13 S 2 The elemental analysis results were consistent with the theoretical values.
[0099] Ligand L3 1H NMR (500 MHz, C 6 D 6 , 25℃)(e.g. Figure 2 ): δ7.36(dd,J=7.6Hz,3.0Hz,0.59H), δ7.33(dd,J=7.5Hz,1.2Hz,0.41H),7.11–7.05(m ,1H),7.05–6.97(m,2H),6.59(d,J=0.85Hz,0.43H),6.57(d,J=0.85Hz,0.30H),3.16(d d,J=14.7,7.6Hz,0.41H),3.06(dd,J=15.1,7.5Hz,0.59H),2.24(s,3H),1.93(s,1.23H ),1.89(s,1.77H),1.88(s,3H),1.29(d,J=7.6Hz,1.77H),1.19(d,J=7.6Hz,1.23H)ppm;
[0100] The ligand L3 obtained in Example 1-1 was analyzed by elemental analysis, and the molecular formula was C 17 H 17 S 2 The elemental analysis results were consistent with the theoretical values.
[0101] Ligand L4 1 H NMR (500 MHz, C 6 D 6 , 25℃)(e.g. Figure 3 ): δ7.22(dt,J=6.5,1.5Hz,1H),7.03(m,3H),6.94(s,1H),3.23(s,2H),1.99(s,3H),1.80(d,J=0.7Hz,3H),1.78(s,3H)ppm;
[0102] The ligand L4 obtained in Example 1-1 was analyzed by elemental analysis, and the molecular formula was C 14 H 15 S, the elemental analysis results obtained are measured values (theoretical values) %: C 77.98 (78.09); H 6.94 (7.02); S 15.01 (14.89); the elemental analysis results are consistent with the theoretical values.
[0103] The ligand L5 obtained in Example 1-1 was analyzed by elemental analysis, and the molecular formula was C 18 H 19 S 2The elemental analysis results were consistent with the theoretical values.
[0104] The ligand L6 obtained in Example 1-1 was analyzed by elemental analysis, and the molecular formula was C 18 H 23 S, obtained elemental analysis results measured value (theoretical value) %: C 79.01 (79.65); H 8.07 (8.45); S 12.05 (11.81); the elemental analysis results are consistent with the theoretical values.
[0105] The ligand L7 obtained in Example 1-1 was analyzed by elemental analysis, and the molecular formula was C 21 H 21 S, the elemental analysis results obtained are measured values (theoretical values) %: C 81.93 (82.57); H 6.48 (6.93); S 10.18 (10.50); the elemental analysis results are consistent with the theoretical values.
[0106] Example 1-2
[0107] This example provides the preparation of a phenylene sulfide functionalized constrained geometry metallocene complex Ln-L2, wherein the rare earth metal complex Lu-L2 is synthesized according to the following reaction route:
[0108]
[0109] The specific preparation process is as follows:
[0110] Under nitrogen protection, 0.26 g (1.00 mmol) of ligand L2 was dissolved in 8 ml of n-hexane and added dropwise to a solution containing 0.58 g (1 mmol) of Lu (CH 2 SiMe 3 ) 3 (THF) 2 The reaction was continued for 12 h in a hexane solution, and the reaction solution was concentrated and recrystallized under low temperature to obtain a yellow-white lutetium complex Lu-L2, 0.48 g, with a yield of 68% and a molecular formula of C 28 H 44 LuOS 2 Si 2 ;
[0111] By replacing the ligand or trialkyl rare earth, the following metal complexes Sc-L1~Sc-L7, Y-L1~Y-L7, Lu-L1~Lu-L7, Nd-L1~Nd-L7 were prepared according to the above method.
[0112] The complex Lu-L2 obtained in Example 1-2 was analyzed by nuclear magnetic resonance to obtain its hydrogen nuclear magnetic resonance spectrum, as shown in Figure 4 The results of NMR are: 1 H NMR (500 MHz, C 6 D 6 , 25℃): δ7.31–7.25 (m, 1H), 7.08–7.03 (m, 1H), 6.95 (p, J=5.9Hz, 2H), 6.75 (d, J=5.3Hz, 1H), 6.60 (d, J=5.3Hz, 1H), 5. 89 (s, 1H), 3.63 (d, J = 6.3Hz, 4H), 2.42 (s, 3H), 2.38 (s, 3H), 1.31–1.20 (m, 5H), 0.24 (s, 18H), -1.04 (t, J = 13.1Hz, 4H);
[0113] The complex Lu-L2 obtained in Example 1-2 was analyzed by elemental analysis, and the molecular formula was C 28 H 44 LuOS 2 Si 2 , the elemental analysis results were found to be in agreement with the theoretical values.
[0114] The complex Y-L3 obtained in Example 1-2 was analyzed by nuclear magnetic resonance to obtain its hydrogen nuclear magnetic resonance spectrum, as shown in Figure 5 The results of NMR are: 1 H NMR (500 MHz, C 6 D 6 , 25℃): δ7.46–7.37 (m, 1H), 7.07–7.00 (m, 2H), 6.95 (p, J=5.1Hz, 2H), 6.23 (s, 1H), 3.64 (d, J=6.1 Hz, 4H), 2.44 (s, 4H), 2.29 (s, 4H), 2.22 (s, 4H), 2.14 (s, 4H), 0.22 (s, 18H), -0.62--0.94 (m, 4H);
[0115] The complex Y-L3 obtained in Example 1-2 was analyzed by elemental analysis, and the molecular formula was C 30 H 48 YOS 2 Si 2, the elemental analysis results were found to be in agreement with the theoretical values.
[0116] The complex Lu-L4 obtained in Example 1-2 was analyzed by nuclear magnetic resonance to obtain its hydrogen nuclear magnetic resonance spectrum, as shown in Figure 6 The results of NMR are: 1 H NMR (500 MHz, C 6 D 6 , 25℃): δ7.18 (dd, J=7.5, 1.6Hz, 1H), 6.84–6.61 (m, 1H), 6.05 (s, 2H), 3.4 9(s, 7H), 2.03(s, 3H), 1.81(s, 8H), 0.00(s, 19H), -1.11(d, J=2.2Hz, 6H).
[0117] The complex Lu-L4 obtained in Example 1-2 was analyzed by elemental analysis, and the molecular formula was C 27 H 46 LuOSSi 2 , the elemental analysis results were found to be in agreement with the theoretical values.
[0118] The complex Sc-L6 obtained in Example 1-2 was analyzed by elemental analysis, and the molecular formula was C 31 H 55 OSC 2 , the elemental analysis results were found to be in agreement with the theoretical values.
[0119] The complex Nd-L7 obtained in Example 1-2 was analyzed by elemental analysis, and the molecular formula was C 29 H 50 NdOSS 2 , the elemental analysis results were found to be in agreement with the theoretical values.
[0120] Preparation of Ethylene-Butadiene-Styrene
[0121] The following examples relate to the preparation of ethylene-butadiene-styrene. The functionalized constrained geometry metallocene complex prepared by Examples 1-2 is used as the main catalyst to catalyze the coordination polymerization of ethylene and butadiene monomers with a co-catalyst. The specific preparation process is as shown in Examples 2-1 to 2-128:
[0122] Determination of the composition of ethylene / butadiene / styrene copolymers
[0123] The contents of ethylene (E), 1,3-butadiene (BD) and styrene (St) in the copolymer are determined according to the 6 D 2 Cl 4 The copolymer was measured at 110°C. 1 H NMR spectra were calculated and the integral was based on I 6.60-7.40 The hydrogen of is 1, and n represents the molar fraction of the monomer in the overall polymer sequence, which is calculated using the following formulas:
[0124] n St =1 / 5; n BD =(I 5.50-6.00 -1) / 2+1; n E = {I 1.21-2.40 -[(I 5.50-6.00 -1) / 2]*4-3*n St -3} / 4;
[0125] f St =0.2 / (n St+ n BD+ n E )*100%;
[0126] f BD =n BD / (n St+ n BD+ n E )*100%;
[0127] f E =n E / (n St+ n BD+ n E )*100%;
[0128] The content of 1,2 structural units and 1,4 structural units in the conjugated diene structural units in the copolymer is based on the 1 HNMR and 13 CNMR spectrum determination calculation;
[0129] Determination of thermal properties of copolymers
[0130] The glass transition temperature of the copolymer (T g) and melting point (Tm): The glass transition temperature and melting point of the copolymers were determined by differential scanning calorimetry (DSC) using Mettler TOPEM TM.
[0131] Determination of molecular weight and molecular weight distribution of copolymers
[0132] The number average molecular weight of the copolymer (M n ) and molecular weight distribution (PDI): The number average molecular weight (M n ) and molecular weight distribution (PDI) were determined by gel permeation chromatography (GPC) at 150 °C using polystyrene as the standard. 6 H 6 Cl 3 For mobile phase determination.
[0133] Example 2-1
[0134] 30 ml (2.1 mol / L) of 1,3-butadiene toluene solution and 10 mmol of styrene were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0135] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Sc-L1 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.1 mL, 100 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0136] The ethylene / 1,3-butadiene / styrene copolymer obtained in Example 1 was analyzed by nuclear magnetic resonance to obtain its hydrogen nuclear magnetic resonance spectrum. Figure 7 shown.
[0137] Example 2-2
[0138] 30 ml (1.6 mol / L) of 1,3-butadiene toluene solution and 10 mmol of styrene were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0139] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Lu-L4 (10 μmol) prepared in Example 1-2, Al i Bu 3 (0.1 mL, 100 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0140] Example 2-3
[0141] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (1.3 mol / L) of 1,3-butadiene toluene solution and 10 mmol of styrene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0142] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Y-L2 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.1 mL, 100 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0143] Embodiment 2-4
[0144] 30 ml (1.0 mol / L) of 1,3-butadiene toluene solution and 10 mmol of styrene were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0145] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Lu-L3 (10 μmol) prepared in Example 1-2, Al i Bu 3 (0.1 mL, 100 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0146] Embodiment 2-5
[0147] 30 ml (0.7 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0148] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Y-L6 (10 μmol) prepared in Example 1-2 and Al i Bu 3(0.1 mL, 100 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0149] Embodiment 2-6
[0150] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (1.3 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0151] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Nd-L7 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.1 mL, 100 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0152] The test results of the copolymers prepared in Examples 2-1 to 2-6 are shown in Table 2:
[0153] Table 2 Performance test results of copolymers prepared in Examples 2-1 to 2-6 of the present invention
[0154]
[0155]
[0156] Embodiment 2-7
[0157] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (2.1 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0158] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Sc-L1 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0159] Embodiment 2-8
[0160] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (1.6 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0161] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Lu-L4 (10 μmol) prepared in Example 1-2, Al i Bu 3 (0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0162] Embodiment 2-9
[0163] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (1.3 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0164] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Y-L2 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0165] Embodiment 2-10
[0166] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (1.0 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0167] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Lu-L3 (10 μmol) prepared in Example 1-2, Al i Bu 3(0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0168] Example 2-11
[0169] 30 ml (0.7 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0170] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Y-L6 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ] (9.2 mg, 10 μmol) was dissolved in 2 mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out of the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20 mL of methanolic hydrochloric acid solution was immediately added to terminate the reaction. Then, a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0171] Example 2-12
[0172] 30 ml (0.7 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0173] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Nd-L7 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0174] Example 2-13
[0175] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (1.3 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0176] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Sc-L1 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0177] The test results of the copolymers prepared in Examples 2-7 to 2-13 are shown in Table 3:
[0178] Table 3 Performance test results of copolymers prepared in Examples 2-7 to 2-13 of the present invention
[0179]
[0180]
[0181] Embodiment 2-14
[0182] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (1.0 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0183] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Y-L4 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.2 mL, 200 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0184] Example 2-15
[0185] In a 150 ml stainless steel reactor fully purged with nitrogen, 30 ml (1.0 mol / L) of 1,3-butadiene toluene solution, 10 mmol of styrene and 50 ml of toluene were added, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0186] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Lu-L2 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.2 mL, 200 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4] (9.2 mg, 10 μmol) was dissolved in 2 mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out of the glove box and quickly added to the above polymerization reaction system at 60°C, and the ethylene pressure was increased to 6 atmospheres to initiate polymerization; after reacting for 1 hour, 20 mL of methanolic hydrochloric acid solution was immediately added to terminate the reaction. Then, a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0187] Example 2-16
[0188] 1 mol (54 g) of butadiene, 1 mol (104 g) of styrene and 1.5 L of toluene were added to a 5 L stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0189] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Lu-L6 (0.3 mmol) prepared in Example 1-2 and Al i Bu 3 (3 mL, 3 mmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ] (9.2 mg, 10 μmol) was dissolved in 2 mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out of the glove box and quickly added to the above polymerization reaction system at 80°C, and the ethylene pressure was increased to 8 atmospheres to initiate polymerization; after reacting for 1 hour, 20 mL of methanolic hydrochloric acid solution was immediately added to terminate the reaction. Then, a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0190] Example 2-17
[0191] 1 mol (54 g) of butadiene, 1 mol (104 g) of styrene and 1.5 L of toluene were added to a 5 L stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0192] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Sc-L3 (0.3 mmol) prepared in Example 1-2 and Al i Bu 3 (3 mL, 3 mmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 80°C, and the ethylene pressure was increased to 10 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0193] Example 2-18
[0194] 50 ml (1.0 mol / L) of 1,3-butadiene, 10 mmol of styrene and 50 ml of hexane were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0195] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Sc-L6 (10 μmol) prepared in Example 1-2, Al i Bu 3 (0.1 mL, 100 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ] (9.2 mg, 10 μmol) was dissolved in 2 mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out of the glove box and quickly added to the above polymerization reaction system at 25°C, and the ethylene pressure was increased to 2 atmospheres to initiate polymerization; after reacting for 1 hour, 20 mL of methanolic hydrochloric acid solution was immediately added to terminate the reaction. Then, a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0196] Example 2-19
[0197] 50 ml (1.0 mol / L) of 1,3-butadiene, 10 mmol of styrene and 50 ml of hexane were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0198] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Y-L3 (10 μmol) prepared in Example 1-2, Al i Bu3 (0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 25°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0199] Example 2-20
[0200] 50 ml (1.0 mol / L) of 1,3-butadiene, 10 mmol of styrene and 50 ml of hexane were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0201] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Y-L2 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.1 mL, 100 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 60°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0202] Example 2-21
[0203] 50 ml (1.0 mol / L) of butadiene, 10 mmol of styrene and 50 ml of hexane were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0204] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Sc-L2 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.2 mL, 200 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ] (9.2 mg, 10 μmol) was dissolved in 2 mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out of the glove box and quickly added to the above polymerization reaction system at 60°C, and the ethylene pressure was increased to 2 atmospheres to initiate polymerization; after reacting for 1 hour, 20 mL of methanolic hydrochloric acid solution was immediately added to terminate the reaction. Then, a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0205] Example 2-22
[0206] 50 ml (1.0 mol / L) of butadiene, 10 mmol of styrene and 50 ml of hexane were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0207] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Nd-L2 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.05 mL, 50 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 60°C, and the ethylene pressure was increased to 6 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0208] Example 2-23
[0209] 50 ml (1.0 mol / L) of 1,3-butadiene, 10 mmol of styrene and 100 ml of hexane were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0210] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Nd-L5 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.2 mL, 200 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 40°C, and the ethylene pressure was increased to 6 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0211] Example 2-24
[0212] 50 ml (1.0 mol / L) of 1,3-butadiene, 10 mmol of styrene and 100 ml of toluene were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0213] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Y-L1 (10 μmol) prepared in Example 1-2 and Al i Bu 3 (0.2 mL, 200 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4](9.2mg, 10μmol) was dissolved in 2mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 60°C, and the ethylene pressure was increased to 6 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0214] Example 2-25
[0215] 50 ml (1.0 mol / L) of 1,3-butadiene, 10 mmol of styrene and 50 ml of toluene were added to a 150 ml stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the toluene solution, thereby forming a polymerization reaction system;
[0216] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Nd-L1 (10 μmol) and Al i Bu 3 (0.2 mL, 200 μmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ] (9.2 mg, 10 μmol) was dissolved in 2 mL of toluene to prepare a catalyst solution; then, the catalyst solution was taken out of the glove box and quickly added to the above polymerization reaction system at 60°C, and the ethylene pressure was increased to 4 atmospheres to initiate polymerization; after reacting for 1 hour, 20 mL of methanolic hydrochloric acid solution was immediately added to terminate the reaction. Then, a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0217] Example 2-26
[0218] 1 mol (54 g) of butadiene, 1 mol (104 g) of styrene and 1.5 L of hexane were added to a 5 L stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0219] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Sc-L5 (0.3 mmol) prepared in Example 1-2 and Al i Bu 3 (3 mL, 3 mmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph3 C][B(C 6 F 5 ) 4 ] (9.2 mg, 10 μmol) was dissolved in 2 mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out of the glove box and quickly added to the above polymerization reaction system at 80°C, and the ethylene pressure was increased to 8 atmospheres to initiate polymerization; after reacting for 1 hour, 20 mL of methanolic hydrochloric acid solution was immediately added to terminate the reaction. Then, a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0220] Example 2-27
[0221] 1 mol (54 g) of butadiene, 1 mol (104 g) of styrene and 1.5 L of hexane were added to a 5 L stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0222] In a glove box, the phenyl sulfide functionalized constrained geometry metallocene complex Nd-L6 (0.3 mmol) prepared in Example 1-2 and Al i Bu 3 (3 mL, 3 mmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ] (9.2 mg, 10 μmol) was dissolved in 2 mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out of the glove box and quickly added to the above polymerization reaction system at 60°C, and the ethylene pressure was increased to 10 atmospheres to initiate polymerization; after the reaction for 1 hour, 20 mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction. Then, a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0223] Example 2-28
[0224] 1 mol (54 g) of butadiene, 1 mol (104 g) of styrene and 1.5 L of hexane were added to a 5 L stainless steel reactor fully purged with nitrogen, and 1.0 atm of ethylene was introduced into the reactor under vigorous stirring to saturate the hexane solution, thereby forming a polymerization reaction system;
[0225] In a glove box, the phenylsulfide functionalized constrained geometry metallocene complex Y-L1 (0.3 mmol) prepared in Example 1-2 and Al i Bu 3(3 mL, 3 mmol, 1.0 mol / L toluene solvent) and triphenylcarbonium tetrakis(pentafluorophenyl)borate [Ph 3 C][B(C 6 F 5 ) 4 ](9.2mg, 10μmol) was dissolved in 2mL of hexane to prepare a catalyst solution; then, the catalyst solution was taken out from the glove box and quickly added to the above polymerization reaction system at 80°C, and the ethylene pressure was increased to 10 atmospheres to initiate polymerization; after reacting for 1 hour, 20mL of methanol-hydrochloric acid solution was immediately added to terminate the reaction; then a large amount of ethanol was added to separate the copolymer, and the copolymer was vacuum dried at 40°C until the polymer weight did not change.
[0226] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0227] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A thioether functionalized constrained geometry rare earth complex as shown in formula (I), in, Cp is a substituted or unsubstituted cyclopentadienyl group, a substituted or unsubstituted indenyl group, a substituted or unsubstituted fluorenyl group, or a substituted or unsubstituted heteroatom-fused cyclopentadienyl group; R1, R2, R3, R4 are independently selected from hydrogen, halogen, methyl, ethyl, isopropyl, tert-butyl or phenyl; R is selected from methyl, ethyl, isopropyl, tert-butyl, phenyl or substituted phenyl; Ln is a rare earth element; X1 and X2 are independently selected from monoanionic ligands; L is a neutral Lewis base; w is an integer from 0 to 3.
2. The rare earth complex according to claim 1, characterized in that The monoanionic ligand is selected from CH2SiMe3, CH(SiMe3)2, CH2C6H4NMe2-o, 1,3-C3H5, 1,3-C3H4(Me) or 1,3-C3H3(SiMe3)2; the neutral Lewis base is selected from tetrahydrofuran, ether, ethylene glycol dimethyl ether or pyridine; the Ln is selected from Sc, Y, Lu, La, Nd, Sm, Gd, Tb, Dy, Er, Tm or Yb.
3. The rare earth complex according to claim 1, characterized in that The structural formula of the rare earth complex is shown in Complex 1, Complex 2, Complex 3, Complex 4, Complex 5, Complex 6, Complex 7 or Complex 8:
4. The rare earth complex according to claim 1, characterized in that The preparation method of the rare earth complex is specifically as follows: The anisyl thioether as shown in formula (III) is reacted with n-butyl lithium in a solvent, and then a cyclopentenone compound is added, heated under reflux for reaction, and dehydrated after the reaction is completed to obtain a thioether-functionalized cyclopentadiene ligand; reacting the cyclopentadiene ligand with a trialkyl rare earth to obtain a rare earth complex; Wherein, R is selected from methyl, ethyl, isopropyl, tert-butyl, phenyl or substituted phenyl.
5. A multi-component copolymer prepared from α-olefin, conjugated diene and styrene or styrene derivative under the action of a catalytic system; The catalytic system is composed of an organic boron salt compound, an organic aluminum compound and a rare earth complex, and the rare earth complex is the rare earth complex according to any one of claims 1 to 4.
6. The multi-component copolymer according to claim 5, characterized in that: The organic boron salt compound is an ionic compound composed of an organic boron anion and a cation; the organic boron anion is selected from tetraphenylborate, tetrakis(monofluorophenyl)borate, tetrakis(difluorophenyl)borate, tetrakis(trifluorophenyl)borate, tetrakis(tetrafluorophenyl)borate, tetrakis(pentafluorophenyl)borate, tetrakis(tetrafluoromethylphenyl)borate, tetrakis(tolyl)borate, tetrakis(xylyl)borate, (triphenyl, pentafluorophenyl)borate, [tris(pentafluorophenyl), benzene] The cation is selected from a carbonium cation, an oxonium cation, an ammonium cation, a phosphonium cation, a cycloheptatrienyl cation or a ferrocenium cation containing a transition metal, the carbonium cation comprises a triphenylcarbonium cation or a tri(substituted phenyl)carbonium cation, the ammonium cation comprises a trialkylammonium cation, an N,N-dialkylanilinium cation or a dialkylammonium cation, and the phosphonium cation comprises a triarylphosphonium cation; The organoaluminum compound is selected from trimethylaluminum, triethylaluminum, tripropylaluminum, tributylaluminum, triisopropylaluminum, triisobutylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum, triphenylaluminum, tri-p-tolylaluminum, tribenzylaluminum, ethyldibenzylaluminum or ethyldi(p-tolyl)aluminum; The molar ratio of the organic boron salt compound to the rare earth complex is 0.3:10 to 10:1, and the molar ratio of the organic aluminum compound to the rare earth complex is 2:1 to 300:
1.
7. The multi-component copolymer according to claim 5, characterized in that: The melting point of the α-olefin is 70-130° C. or has no melting point, and the α-olefin is selected from ethylene, propylene or 1-butene; the melting point of the styrene or styrene derivative is 220-260° C. or has no melting point.
8. The multi-component copolymer according to claim 5, characterized in that: In the main chain of the multi-polymer, the insertion rate of styrene or styrene derivatives is 10-40 mol%, the insertion rate of conjugated diene is 20-80 mol%, and the insertion rate of α-olefin is 10-60 mol%; the regioselectivity of the conjugated diene is that the cis-1,4-content is greater than 75 mol%; the number average molecular weight of the multi-polymer is above 20,000, and the molecular weight distribution of the multi-polymer is 1-10.
9. A method for preparing a multi-component copolymer, comprising: Initiating polymerization of α-olefin, conjugated diene and styrene or styrene derivative in a reaction medium under a catalytic system to obtain a multi-component copolymer; The catalytic system is composed of an organic boron salt compound, an organic aluminum compound and a rare earth complex, and the rare earth complex is the rare earth complex according to any one of claims 1 to 4.
10. The preparation method according to claim 9, characterized in that: The polymerization reaction temperature is -40 to 100° C., the polymerization reaction is carried out at 1 to 20 atmospheres, and the reaction medium is selected from one or more of aliphatic saturated hydrocarbons, aromatic hydrocarbons, aromatic halides and cycloalkanes.