Reprocessable acrylate rubber and preparation method thereof

By introducing dynamic covalent bond crosslinking technology between nitrogen-containing monomer and boric acid ester in acrylate rubber, the problem of rubber being unable to process and stick to rollers is solved, and the combination of high elongation and good processing performance is achieved, which promotes the Recyclable and environmentally friendly production of materials.

CN118894957APending Publication Date: 2024-11-05HEFEI UNIV OF TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411012127.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Acrylate rubber cannot be processed and recycled after crosslinking, resulting in environmental pollution and prone to sticking rollers at high temperatures, affecting production and processing.

Method used

Using dynamic covalent bond crosslinking technology between nitrogen-containing monomers and boric acid esters, a reversible fracture and binding mechanism is constructed through boron-nitrogen coordination, which improves the reprocessable capacity of rubber, and through boron-nitrogen coordination and boron The synergistic effect of acid ester enhances the network cross-link density and avoids sticking to rollers.

Benefits of technology

It significantly improves the elongation of break and reprocessability of acrylate rubber, maintains mechanical properties, avoids sticking rollers, and facilitates processing and recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894957A_ABST
    Figure CN118894957A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of acrylate rubber capable of being reprocessed, and belongs to the technical field of dynamic crosslinking macromolecules. The preparation method comprises the following steps: (1) preparing a dynamic cross-linking agent containing diboric acid ester from dihydroxypropyl methacrylate, 1, 4-p-phenylenediboronic acid, anhydrous dichloromethane and anhydrous magnesium sulfate; and (2) preparing the acrylate rubber capable of being reprocessed from the dynamic cross-linking agent containing diborate, butyl acrylate, dimethylaminoethyl methacrylate, N, N-dimethylacetamide and azodiisobutyronitrile. Through boric acid ester exchange and boron-nitrogen coordination, the acrylate rubber is endowed with the reprocessing performance and the characteristic of being not prone to roll sticking, the elongation at break of the acrylate rubber capable of being reprocessed is remarkably improved, the elongation at break of the acrylate rubber before reprocessing is 224.1%-770.7%, and the elongation at break of the acrylate rubber after reprocessing is still kept at 183.7%-411.2%. And moreover, the characteristic of difficulty in roll sticking is realized, and a new thought is provided for reprocessing and utilization of the acrylate rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a reprocessable acrylic rubber and a preparation method thereof. Background Art

[0002] Acrylic rubber is an elastomer obtained by copolymerization with acrylic ester as the main monomer. Its main chain is a saturated carbon chain and its side group is a polar ester group. Due to its special structure, it has many excellent characteristics, such as heat resistance, aging resistance, oil resistance, ozone resistance, and UV resistance. However, similar to other rubber varieties, acrylic rubber needs to be cross-linked to obtain better mechanical properties. Its covalent cross-linking properties make it impossible to reprocess and recycle rubber products, causing increasingly serious environmental pollution problems. In addition, when acrylic rubber is mixed at a high temperature, it is easy to produce serious roller sticking, which makes it impossible to remove the rubber from the rubber mixer. In severe cases, it may even cause the rubber to burn.

[0003] A dynamic covalent bond is a chemical bond that can undergo reversible "breaking" and "combination" under certain external conditions (light, heat, force, acid, alkali, etc.) to achieve dynamic exchange and recombination. When the stimulus is eliminated, the dynamic covalent bond polymer can show high stability comparable to that of general covalent bond polymers. Boric acid esters are commonly used dynamic covalent bonds, which have the characteristics of no need for external catalysts and low reaction activation energy. They have been used as crosslinking agents for the preparation of reprocessable polyacrylate rubbers. However, the mechanical strength and toughness of elastomeric materials crosslinked with borate esters are usually not taken into account at the same time. It is difficult to obtain reprocessable acrylic rubbers with both mechanical strength and toughness, which greatly limits the application of such materials. Summary of the invention

[0004] In order to realize the reprocessing and recycling of acrylate rubber, the present invention aims to provide a reprocessable acrylate rubber and a preparation method thereof.

[0005] The preparation steps of a reprocessable acrylic rubber are as follows:

[0006] (1) Preparation of a dynamic crosslinking agent containing a diboric acid ester (1.1) Dissolve 11 molar parts of 2-methyl-2-acrylic acid-2,3-dihydroxypropyl ester and 5 molar parts of 1,4-terephthalenediboric acid in 390 molar parts of anhydrous dichloromethane, add 12.5 molar parts of anhydrous magnesium sulfate, and stir at room temperature for 24 hours to obtain a first mixture;

[0007] (1.2) filtering the first mixture, and rotary evaporating the filtrate at 30° C. to obtain a white solid powder;

[0008] (1.3) The white solid powder is subjected to column separation, and the product obtained by column separation is subjected to rotary evaporation at a temperature of 50° C. to remove the developing agent used for column separation, thereby obtaining a dynamic crosslinking agent containing diborate, wherein the dynamic crosslinking agent containing diborate is 2-methyl-2-acrylic acid-1,1'-[1,4-phenylenebis(1,3,2-dioxaborane-2,4-diylmethylene)] ester (DE); (2) Preparation of reprocessable acrylic rubber (2.1) 17-19 mol parts of butyl acrylate, 0.5-1 mol parts of a dynamic crosslinking agent containing diborate, 0.5-2 mol parts of dimethylaminoethyl methacrylate and 54 mol parts of N,N-dimethylacetamide are mixed;

[0009] (2.2) bubbling nitrogen for 30 minutes at room temperature, and then heating in an oil bath at 65° C. until all monomers are completely dissolved, to obtain a second mixture;

[0010] (2.3) adding an initiator azobisisobutyronitrile to the second mixture, wherein the amount of azobisisobutyronitrile added is 0.2% of the total mass of the second mixture; reacting in an oven at a temperature of 70° C. in a nitrogen atmosphere for 5 hours; and volatilizing the solvent in a vacuum oven at a temperature of 90° C. for 48 hours to obtain a reprocessable acrylic rubber, i.e., an acrylic rubber cross-linked by dynamic covalent bonds based on phenyl borate;

[0011] The reprocessable acrylic rubber has a tensile strength of 0.2 to 1.3 MPa, an elongation at break of 224.1 to 770.7%, an elongation at break after reprocessing of 183.7 to 554.9%, and a change rate of elongation at break of -32 to -18%.

[0012] The further technical solution is as follows:

[0013] In step (1.3), the developing solvent used in the column separation is prepared by uniformly mixing ethyl acetate and petroleum ether in a volume ratio of 4:1.

[0014] Compared with the existing technical solutions, the beneficial technical effects of the present invention are embodied in the following aspects:

[0015] (1) By introducing nitrogen-containing monomers into the cross-linked matrix, a boron-nitrogen coordination effect between molecules can be constructed. When the material is subjected to force, the coordination bond can play the role of a sacrificial bond, and reversible fracture and bonding occur, thereby significantly improving the elongation at break of the acrylic rubber. At the same cross-linking degree, the elongation at break of the sample is significantly increased from 71.8% in Comparative Example 1 to 770.7% in Example 2.

[0016] (2) Since the dynamic ester exchange process of the borate bond will undergo a rapid ester exchange reaction, the polymer network can undergo rapid reorganization and migration, thereby forming a new dynamic borate network. Therefore, the synergistic effect of boron-nitrogen coordination and borate esters gives the acrylic rubber excellent reprocessability. The elongation at break of the acrylic rubber before reprocessing is 224.1% to 770.7%, and the elongation at break of the acrylic rubber after reprocessing remains at 183.7% to 411.2%.

[0017] (3) The introduction of boron-nitrogen coordination can serve as a physical crosslinking point, further increasing the crosslinking density of the acrylic rubber network, and the long-chain structure has a certain barrier effect. Figure 1 The reprocessable acrylic rubber does not stick to the roller during the sheeting process, has good flexibility, and adjacent films are not easy to adhere to each other, making it easy to produce and process. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a comparison of photos before and after hot pressing of acrylic rubber. DETAILED DESCRIPTION

[0019] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the scope of the present invention.

[0020] In the embodiments, 2-methyl-2-acrylic acid-2,3-dihydroxypropyl ester was purchased from Jiangsu Aikang Company; 1,4-terephthalenediboric acid was purchased from McLean Co., Ltd.; butyl acrylate was purchased from Aladdin Co., Ltd.; dimethylaminoethyl methacrylate was purchased from Aladdin Co., Ltd.; azobisisobutyronitrile was purchased from Aladdin Co., Ltd.; and N,N-dimethylacetamide was purchased from Sinopharm Chemical Reagent Co., Ltd.

[0021] The raw material formulas of the embodiments of the present invention and the comparative examples are shown in Table 1

[0022] Table 1 Raw materials (molar fractions) of reprocessable acrylic rubber examples and comparative examples

[0023]

[0024] Example 1

[0025] A method for preparing a reprocessable polyacrylate rubber based on dynamic covalent crosslinking of phenyl borate is as follows:

[0026] (1) Preparation of a dynamic crosslinker containing diboric acid ester (1.1) Dissolve 1.76 g (11 mmol) of 2-methyl-2-acrylate-2,3-dihydroxypropyl ester and 0.83 g (5 mmol) of 1,4-terephthalenediboric acid in 25 mL (390 mmol) of anhydrous dichloromethane, add 1.5 g (12.5 mmol) of anhydrous magnesium sulfate, and stir at room temperature for 24 hours to obtain a first mixture.

[0027] (1.2) Filter the first mixture, and rotary evaporate the filtrate at 30° C. to obtain a white solid powder.

[0028] (1.3) The white solid powder was separated by column. The developing solvent used in the column separation was prepared by mixing ethyl acetate and petroleum ether in a volume ratio of 4:1.

[0029] The product obtained by column separation was subjected to rotary evaporation at a temperature of 50° C. to remove the developing agent used for column separation, thereby obtaining a dynamic crosslinking agent containing diboric acid ester, wherein the dynamic crosslinking agent containing diboric acid ester is 2-methyl-2-acrylic acid-1,1'-[1,4-phenylenebis(1,3,2-dioxaborane-2,4-diylmethylene)]ester (DE),

[0030]

[0031] The above formula is the structural formula of 2-methyl-2-acrylate-1,1'-[1,4-phenylenebis(1,3,2-dioxaborolane-2,4-diylmethylene)]ester (DE).

[0032] (2) Preparation of Reprocessable Acrylic Rubber (2.1) 2.44 g (19 mmol) of butyl acrylate, 0.21 g (0.5 mmol) of a diboric acid ester-containing dynamic crosslinker, 0.08 g (0.5 mmol) of dimethylaminoethyl methacrylate and 5 mL (54 mmol) of N,N-dimethylacetamide were mixed.

[0033] (2.2) The mixture was bubbled with nitrogen for 30 minutes at room temperature and then heated in an oil bath at 65° C. until all monomers were completely dissolved to obtain a second mixture.

[0034] (2.3) Adding initiator azobisisobutyronitrile to the second mixture, the amount of azobisisobutyronitrile added is 0.2% of the total mass of the second mixture; reacting in an oven at a temperature of 70°C in a nitrogen atmosphere for 5 hours; and volatilizing the solvent in a vacuum oven at a temperature of 90°C for 48 hours to obtain a reprocessable acrylic rubber, i.e., an acrylic rubber based on dynamic covalent crosslinking of phenyl borate.

[0035] Acrylic rubber mechanical properties test:

[0036] The acrylic rubber was cut into several small specimens (35mm×2mm×0.5mm) using a standard dumbbell cutter and tested using an electronic universal material testing machine according to the GB / T 1040.3-2006 test standard. sample The tensile strength and elongation at break of the original sample were measured at a tensile rate of 50 mm / min. Three samples were tested in each group, and the median of the tensile strength and elongation at break of each group of test samples was taken. The tensile strength of the original sample of Example 1 was 0.2 MPa, and the elongation at break was 604.8%.

[0037] Mechanical properties test of reprocessable acrylic rubber:

[0038] Cut the reprocessable acrylic rubber into small particles, place them in a flat vulcanizer and heat press them for 30 minutes at 8MPa and 110℃. Cut the samples into several small specimens (35mm×2mm×0.5mm) with a standard dumbbell cutter. According to the GB / T1040.3-2006 test standard, use an electronic universal material testing machine to test the tensile strength and elongation at break of the samples. The tensile rate is set to 50mm / min. Three specimens are tested in each group. The median of the tensile strength and elongation at break of each group of test specimens is taken, and the tensile strength and elongation at break before and after reprocessing are compared. After reprocessing, the tensile strength is 0.18MPa, with a change rate of -9%, and the elongation at break is 411.2%, with a change rate of -32%.

[0039] Test of mucous membrane and roller adhesion:

[0040] When the reprocessable acrylic rubber is processed and mixed, the acrylic rubber is observed for sticking to the roller, and ten cases are observed for each case. Here, the sticking to the mold and the roller is divided into sticking to the roller, slight sticking to the roller, and no sticking to the roller. The reprocessed acrylic rubber prepared in Example 1 did not stick to the roller during the processing and mixing process.

[0041] Example 2

[0042] A method for preparing a reprocessable polyacrylate rubber based on dynamic covalent crosslinking of phenyl borate is as follows:

[0043] (1) Preparation of a dynamic crosslinking agent containing a diboric acid ester (1.1) Dissolve 1.76 g (11 mmol) of 2-methyl-2-acrylic acid-2,3-dihydroxypropyl ester and 0.83 g (5 mmol) of 1,4-terephthalenediboric acid in 25 mL (390 mmol) of anhydrous dichloromethane, add 1.5 g (12.5 mmol) of anhydrous magnesium sulfate, and stir at room temperature for 24 hours to obtain a first mixture;

[0044] (1.2) filtering the first mixture, and rotary evaporating the filtrate at 30° C. to obtain a white solid powder;

[0045] (1.3) The white solid powder was separated by column. The developing solvent used in the column separation was prepared by mixing ethyl acetate and petroleum ether in a volume ratio of 4:1.

[0046] The product obtained by column separation was subjected to rotary evaporation at a temperature of 50° C. to remove the developing agent used for column separation, thereby obtaining a dynamic crosslinking agent containing diboric acid ester, wherein the dynamic crosslinking agent containing diboric acid ester is 2-methyl-2-acrylic acid-1,1′-[1,4-phenylenebis(1,3,2-dioxaborane-2,4-diylmethylene)]ester (DE);

[0047] (2) Preparation of reprocessable acrylic rubber (2.1) 2.37 g (18.5 mmol) of butyl acrylate, 0.21 g (0.5 mmol) of a dynamic crosslinking agent containing a diboric acid ester, 0.16 g (1 mmol) of dimethylaminoethyl methacrylate and 5 mL (54 mmol) of N,N-dimethylacetamide were mixed;

[0048] (2.2) bubbling nitrogen for 30 minutes at room temperature, and then heating in an oil bath at 65° C. until all monomers are completely dissolved, to obtain a second mixture;

[0049] (2.3) adding an initiator azobisisobutyronitrile to the second mixture, wherein the amount of azobisisobutyronitrile added is 0.2% of the total mass of the second mixture; reacting in an oven at a temperature of 70° C. in a nitrogen atmosphere for 5 hours; and volatilizing the solvent in a vacuum oven at a temperature of 90° C. for 48 hours to obtain a reprocessable acrylic rubber, i.e., an acrylic rubber cross-linked by dynamic covalent bonds based on phenyl borate;

[0050] Acrylic rubber mechanical properties test:

[0051] The acrylic rubber was cut into several small specimens (35 mm × 2 mm × 0.5 mm) using a standard dumbbell cutter. According to the GB / T 1040.3-2006 test standard, the tensile strength and elongation at break of the specimens were tested using an electronic universal material testing machine. The tensile rate was set to 50 mm / min. Three specimens were tested in each group, and the median of the tensile strength and elongation at break of each group of test specimens was taken. The tensile strength of the original sample of Example 2 was 0.3 MPa, and the elongation at break was 770.7%.

[0052] Mechanical properties test of reprocessable acrylic rubber:

[0053] Cut the reprocessable acrylic rubber into small particles, place them in a flat vulcanizer and heat press them for 30 minutes at 8MPa and 110℃. Cut the samples into several small specimens (35mm×2mm×0.5mm) with a standard dumbbell cutter. According to the GB / T1040.3-2006 test standard, use an electronic universal material testing machine to test the tensile strength and elongation at break of the samples. The tensile rate is set to 50mm / min. Three specimens are tested in each group. The median of the tensile strength and elongation at break of each group of test specimens is taken, and the tensile strength and elongation at break before and after reprocessing are compared. After reprocessing, the tensile strength is 0.28MPa, with a change rate of -7%, and the elongation at break is 554.9%, with a change rate of -28%.

[0054] Test of mucous membrane and roller adhesion:

[0055] When the reprocessable acrylic rubber is processed and mixed, the acrylic rubber sticking to the roller is observed, and ten cases are observed for each case. Here, the sticking to the mold and the roller is divided into sticking to the roller, slight sticking to the roller, and no sticking to the roller. The reprocessed acrylic rubber prepared in Example 2 did not stick to the roller during the processing and mixing process.

[0056] Example 3

[0057] A method for preparing a reprocessable polyacrylate rubber based on dynamic covalent crosslinking of phenyl borate is as follows:

[0058] (1) Preparation of a dynamic crosslinking agent containing a diboric acid ester (1.1) Dissolve 1.76 g (11 mmol) of 2-methyl-2-acrylic acid-2,3-dihydroxypropyl ester and 0.83 g (5 mmol) of 1,4-terephthalenediboric acid in 25 mL (390 mmol) of anhydrous dichloromethane, add 1.5 g (12.5 mmol) of anhydrous magnesium sulfate, and stir at room temperature for 24 hours to obtain a first mixture;

[0059] (1.2) filtering the first mixture, and rotary evaporating the filtrate at 30° C. to obtain a white solid powder;

[0060] (1.3) The white solid powder was separated by column. The developing solvent used in the column separation was prepared by mixing ethyl acetate and petroleum ether in a volume ratio of 4:1.

[0061] The product obtained by column separation was subjected to rotary evaporation at a temperature of 50° C. to remove the developing agent used for column separation, thereby obtaining a dynamic crosslinking agent containing diboric acid ester, wherein the dynamic crosslinking agent containing diboric acid ester is 2-methyl-2-acrylic acid-1,1′-[1,4-phenylenebis(1,3,2-dioxaborane-2,4-diylmethylene)]ester (DE);

[0062] (2) Preparation of reprocessable acrylic rubber (2.1) 2.31 g (18 mmol) of butyl acrylate, 0.41 g (1 mmol) of a dynamic crosslinking agent containing a diboric acid ester, 0.16 g (1 mmol) of dimethylaminoethyl methacrylate and 5 mL (54 mmol) of N,N-dimethylacetamide were mixed;

[0063] (2.2) bubbling nitrogen for 30 minutes at room temperature, and then heating in an oil bath at 65° C. until all monomers are completely dissolved, to obtain a second mixture;

[0064] (2.3) adding an initiator azobisisobutyronitrile to the second mixture, wherein the amount of azobisisobutyronitrile added is 0.2% of the total mass of the second mixture; reacting in an oven at a temperature of 70° C. in a nitrogen atmosphere for 5 hours; and volatilizing the solvent in a vacuum oven at a temperature of 90° C. for 48 hours to obtain a reprocessable acrylic rubber, i.e., an acrylic rubber cross-linked by dynamic covalent bonds based on phenyl borate;

[0065] Acrylic rubber mechanical properties test:

[0066] The acrylic rubber was cut into several small specimens (35 mm × 2 mm × 0.5 mm) using a standard dumbbell cutter. According to the GB / T 1040.3-2006 test standard, the tensile strength and elongation at break of the samples were tested using an electronic universal material testing machine. The tensile rate was set to 50 mm / min. Three specimens were tested in each group, and the median of the tensile strength and elongation at break of each group of test specimens was taken. The tensile strength of the original sample of Example 3 was 0.7 MPa, and the elongation at break was 260.5%.

[0067] Mechanical properties test of reprocessable acrylic rubber:

[0068] Cut the reprocessable acrylic rubber into small particles, place them in a flat vulcanizer and heat press them for 30 minutes at 8MPa and 110℃. Cut the samples into several small specimens (35mm×2mm×0.5mm) with a standard dumbbell cutter. According to the GB / T1040.3-2006 test standard, use an electronic universal material testing machine to test the tensile strength and elongation at break of the samples. The tensile rate is set to 50mm / min. Three specimens are tested in each group. The median of the tensile strength and elongation at break of each group of test specimens is taken, and the tensile strength and elongation at break before and after reprocessing are compared. After reprocessing, the tensile strength is 0.61MPa, with a change rate of -12%, and the elongation at break is 205.7%, with a change rate of -21%.

[0069] Test of mucous membrane and roller adhesion:

[0070] When the reprocessable acrylic rubber is processed and mixed, the acrylic rubber sticking to the roller is observed, and ten cases are observed for each case. Here, the sticking to the mold and the roller is divided into sticking to the roller, slight sticking to the roller, and no sticking to the roller. The reprocessed acrylic rubber prepared in Example 3 did not stick to the roller during the processing and mixing process.

[0071] Example 4

[0072] A method for preparing a reprocessable polyacrylate rubber based on dynamic covalent crosslinking of phenyl borate is as follows:

[0073] (1) Preparation of a dynamic crosslinking agent containing a diboric acid ester (1.1) Dissolve 1.76 g (11 mmol) of 2-methyl-2-acrylic acid-2,3-dihydroxypropyl ester and 0.83 g (5 mmol) of 1,4-terephthalenediboric acid in 25 mL (390 mmol) of anhydrous dichloromethane, add 1.5 g (12.5 mmol) of anhydrous magnesium sulfate, and stir at room temperature for 24 hours to obtain a first mixture;

[0074] (1.2) filtering the first mixture, and rotary evaporating the filtrate at 30° C. to obtain a white solid powder;

[0075] (1.3) The white solid powder was separated by column. The developing solvent used in the column separation was prepared by mixing ethyl acetate and petroleum ether in a volume ratio of 4:1.

[0076] The product obtained by column separation was subjected to rotary evaporation at a temperature of 50° C. to remove the developing agent used for column separation, thereby obtaining a dynamic crosslinking agent containing diboric acid ester, wherein the dynamic crosslinking agent containing diboric acid ester is 2-methyl-2-acrylic acid-1,1′-[1,4-phenylenebis(1,3,2-dioxaborane-2,4-diylmethylene)]ester (DE);

[0077] (2) Preparation of reprocessable acrylic rubber (2.1) 2.18 g (17 mmol) of butyl acrylate, 0.41 g (1 mmol) of a dynamic crosslinking agent containing a diboric acid ester, 0.31 g (2 mmol) of dimethylaminoethyl methacrylate and 5 mL (54 mmol) of N,N-dimethylacetamide were mixed;

[0078] (2.2) bubbling nitrogen for 30 minutes at room temperature, and then heating in an oil bath at 65° C. until all monomers are completely dissolved, to obtain a second mixture;

[0079] (2.3) adding an initiator azobisisobutyronitrile to the second mixture, wherein the amount of azobisisobutyronitrile added is 0.2% of the total mass of the second mixture; reacting in an oven at a temperature of 70° C. in a nitrogen atmosphere for 5 hours; and volatilizing the solvent in a vacuum oven at a temperature of 90° C. for 48 hours to obtain a reprocessable acrylic rubber, i.e., an acrylic rubber cross-linked by dynamic covalent bonds based on phenyl borate;

[0080] Acrylic rubber mechanical properties test:

[0081] The acrylic rubber was cut into several small specimens (35 mm × 2 mm × 0.5 mm) using a standard dumbbell cutter. The tensile strength and elongation at break of the specimens were tested using an electronic universal material testing machine according to the GB / T 1040.3-2006 test standard. The tensile rate was set to 50 mm / min. Three specimens were tested in each group, and the median of the tensile strength and elongation at break of each group of test specimens was taken. The tensile strength of the original sample of Example 4 was 1.3 MPa, and the elongation at break was 224.1%.

[0082] Mechanical properties test of reprocessable acrylic rubber:

[0083] Cut the reprocessable acrylic rubber into small particles, place them in a flat vulcanizer and heat press them for 30 minutes at 8MPa and 110℃. Cut the samples into several small specimens (35mm×2mm×0.5mm) with a standard dumbbell cutter. According to the GB / T1040.3-2006 test standard, use an electronic universal material testing machine to test the tensile strength and elongation at break of the samples. The tensile rate is set to 50mm / min. Three specimens are tested in each group. The median of the tensile strength and elongation at break of each group of test specimens is taken, and the tensile strength and elongation at break before and after reprocessing are compared. After reprocessing, the tensile strength is 1.17MPa, with a change rate of -10%, and the elongation at break is 183.7%, with a change rate of -18%.

[0084] Test of mucous membrane and roller adhesion:

[0085] When the reprocessable acrylic rubber is processed and mixed, the acrylic rubber sticking to the roller is observed, and ten cases are observed for each case. Here, the sticking to the mold and the roller is divided into sticking to the roller, slight sticking to the roller, and no sticking to the roller. The reprocessed acrylic rubber prepared in Example 4 did not stick to the roller during the processing and mixing process.

[0086] Table 2 Mechanical properties test results before and after reprocessing of Examples 1 to 4 and Comparative Examples 1 to 2

[0087]

[0088]

[0089] Table 3: Film adhesion to roller of Examples 1 to 4 and Comparative Examples 1 to 2

[0090] Test items Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 The incidence of mold sticking 0% 0% 0% 0% 40% 50% Sticky roller Non-stick roller Non-stick roller Non-stick roller Non-stick roller Slightly sticky roller Slightly sticky roller

[0091] Comparative Example 1

[0092] A method for preparing a reprocessable polyacrylate rubber based on dynamic covalent crosslinking of phenyl borate is as follows:

[0093] (1) Preparation of a dynamic crosslinking agent containing a diboric acid ester (1.1) Dissolve 1.76 g (11 mmol) of 2-methyl-2-acrylic acid-2,3-dihydroxypropyl ester and 0.83 g (5 mmol) of 1,4-terephthalenediboric acid in 25 mL (390 mmol) of anhydrous dichloromethane, add 1.5 g (12.5 mmol) of anhydrous magnesium sulfate, and stir at room temperature for 24 hours to obtain a first mixture;

[0094] (1.2) filtering the first mixture, and rotary evaporating the filtrate at 30° C. to obtain a white solid powder;

[0095] (1.3) The white solid powder was separated by column. The developing solvent used in the column separation was prepared by mixing ethyl acetate and petroleum ether in a volume ratio of 4:1.

[0096] The product obtained by column separation was subjected to rotary evaporation at a temperature of 50° C. to remove the developing agent used for column separation, thereby obtaining a dynamic crosslinking agent containing diboric acid ester, wherein the dynamic crosslinking agent containing diboric acid ester is 2-methyl-2-acrylic acid-1,1′-[1,4-phenylenebis(1,3,2-dioxaborane-2,4-diylmethylene)]ester (DE);

[0097] (2) Preparation of reprocessable acrylic rubber (2.1) 2.50 g (19.5 mmol) of butyl acrylate, 0.21 g (0.5 mmol) of a dynamic crosslinking agent containing a diboric acid ester and 5 mL (54 mmol) of N,N-dimethylacetamide were mixed;

[0098] (2.2) bubbling nitrogen for 30 minutes at room temperature, and then heating in an oil bath at 65° C. until all monomers are completely dissolved, to obtain a second mixture;

[0099] (2.3) adding an initiator azobisisobutyronitrile to the second mixture, wherein the amount of azobisisobutyronitrile added is 0.2% of the total mass of the second mixture; reacting in an oven at a temperature of 70° C. in a nitrogen atmosphere for 5 hours; and volatilizing the solvent in a vacuum oven at a temperature of 90° C. for 48 hours to obtain a reprocessable acrylic rubber, i.e., an acrylic rubber cross-linked by dynamic covalent bonds based on phenyl borate;

[0100] Acrylic rubber mechanical properties test:

[0101] The acrylic rubber was cut into several small specimens (35mm×2mm×0.5mm) with a standard dumbbell cutter, and the tensile strength and elongation at break of the specimens were tested using an electronic universal material testing machine according to the GB / T 1040.3-2006 test standard. The tensile rate was set to 50mm / min, and 3 specimens were tested in each group. The median of the tensile strength and elongation at break of each group of test specimens was taken. The tensile strength of the original sample of Comparative Example 1 was 0.2MPa, and the elongation at break was 81.6%.

[0102] Mechanical properties test of reprocessable acrylic rubber:

[0103] The acrylic rubber was cut into small particles, placed in a flat vulcanizer and hot-pressed for 30 minutes at 8MPa and 110°C. The sample was cut into several small specimens (35mm×2mm×0.5mm) with a standard dumbbell cutter. According to the GB / T1040.3-2006 test standard, the tensile strength and elongation at break of the sample were tested using an electronic universal material testing machine. The tensile rate was set to 50mm / min. Three specimens were tested in each group. The median of the tensile strength and elongation at break of each group of test specimens was taken, and the tensile strength and elongation at break before and after reprocessing were compared. After reprocessing, the tensile strength was 0.18MPa, with a change rate of -9%, and the elongation at break was 71.8%, with a change rate of -12%.

[0104] Test of mucous membrane and roller adhesion:

[0105] When the acrylic rubber is processed and mixed, the acrylic rubber sticking to the roller is observed, and ten cases are observed for each case. Here, the sticking to the mold and the roller is divided into sticking to the roller, slight sticking to the roller, and no sticking to the roller. The reprocessed acrylic rubber prepared in Comparative Example 1 had slight sticking to the roller during the processing and mixing process.

[0106] Comparative Example 2

[0107] A method for preparing a reprocessable polyacrylate rubber based on dynamic covalent crosslinking of phenyl borate is as follows:

[0108] (1) Preparation of a dynamic crosslinking agent containing a diboric acid ester (1.1) Dissolve 1.76 g (11 mmol) of 2-methyl-2-acrylic acid-2,3-dihydroxypropyl ester and 0.83 g (5 mmol) of 1,4-terephthalenediboric acid in 25 mL (390 mmol) of anhydrous dichloromethane, add 1.5 g (12.5 mmol) of anhydrous magnesium sulfate, and stir at room temperature for 24 hours to obtain a first mixture;

[0109] (1.2) filtering the first mixture, and rotary evaporating the filtrate at 30° C. to obtain a white solid powder;

[0110] (1.3) The white solid powder was separated by column. The developing solvent used in the column separation was prepared by mixing ethyl acetate and petroleum ether in a volume ratio of 4:1.

[0111] The product obtained by column separation was subjected to rotary evaporation at a temperature of 50° C. to remove the developing agent used for column separation, thereby obtaining a dynamic crosslinking agent containing diboric acid ester, wherein the dynamic crosslinking agent containing diboric acid ester is 2-methyl-2-acrylic acid-1,1′-[1,4-phenylenebis(1,3,2-dioxaborane-2,4-diylmethylene)]ester (DE);

[0112] (2) Preparation of reprocessable acrylic rubber (2.1) 2.44 g (19 mmol) of butyl acrylate, 0.41 g (1 mmol) of a dynamic crosslinking agent containing a diboric acid ester and 5 mL (54 mmol) of N,N-dimethylacetamide were mixed;

[0113] (2.2) bubbling nitrogen for 30 minutes at room temperature, and then heating in an oil bath at 65° C. until all monomers are completely dissolved, to obtain a second mixture;

[0114] (2.3) adding an initiator azobisisobutyronitrile to the second mixture, wherein the amount of azobisisobutyronitrile added is 0.2% of the total mass of the second mixture; reacting in an oven at a temperature of 70° C. in a nitrogen atmosphere for 5 hours; and volatilizing the solvent in a vacuum oven at a temperature of 90° C. for 48 hours to obtain a reprocessable acrylic rubber, i.e., an acrylic rubber cross-linked by dynamic covalent bonds based on phenyl borate;

[0115] Acrylic rubber mechanical properties test:

[0116] The acrylic rubber was cut into several small specimens (35mm×2mm×0.5mm) with a standard dumbbell cutter. According to the GB / T 1040.3-2006 test standard, the tensile strength and elongation at break of the samples were tested using an electronic universal material testing machine. The tensile rate was set to 50mm / min. Three specimens were tested in each group, and the median of the tensile strength and elongation at break of each group of test specimens was taken. The tensile strength of the original sample of Comparative Example 2 was 1.0MPa, and the elongation at break was 63.2%.

[0117] Mechanical properties test of reprocessable acrylic rubber:

[0118] The acrylic rubber was cut into small particles, placed in a flat vulcanizer and hot-pressed for 30 minutes at 8MPa and 110°C. The sample was cut into several small specimens (35mm×2mm×0.5mm) with a standard dumbbell cutter. According to the GB / T1040.3-2006 test standard, the tensile strength and elongation at break of the sample were tested using an electronic universal material testing machine. The tensile rate was set to 50mm / min. Three specimens were tested in each group. The median of the tensile strength and elongation at break of each group of test specimens was taken, and the tensile strength and elongation at break before and after reprocessing were compared. After reprocessing, the tensile strength was 1.0MPa, with a change rate of -12%, and the elongation at break was 59.4%, with a change rate of -6%.

[0119] Test of mucous membrane and roller adhesion:

[0120] When the acrylic rubber is processed and mixed, the acrylic rubber sticking to the roller is observed, and ten cases are observed for each case. Here, the sticking to the mold and the roller is divided into sticking to the roller, slight sticking to the roller, and no sticking to the roller. The reprocessed acrylic rubber prepared in Comparative Example 2 had slight sticking to the roller during the processing and mixing process.

[0121] It is easy for those skilled in the art to understand that Examples 1-4 are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a reprocessable acrylic rubber, characterized in that: The steps are as follows: (1) Preparation of dynamic crosslinking agent containing diboric acid ester (1.1) dissolving 11 molar parts of 2-methyl-2-acrylic acid-2,3-dihydroxypropyl ester and 5 molar parts of 1,4-terephthalenediboric acid in 390 molar parts of anhydrous dichloromethane, adding 12.5 molar parts of anhydrous magnesium sulfate, and stirring at room temperature for 24 hours to obtain a first mixture; (1.2) filtering the first mixture, and rotary evaporating the filtrate at 30° C. to obtain a white solid powder; (1.3) separating the white solid powder by column separation, and performing rotary evaporation on the product obtained by column separation at a temperature of 50° C. to remove the developing agent used for column separation, thereby obtaining a dynamic crosslinking agent containing a diboric acid ester, wherein the dynamic crosslinking agent containing a diboric acid ester is 2-methyl-2-acrylic acid-1,1′-[1,4-phenylenebis(1,3,2-dioxaborane-2,4-diylmethylene)]ester (DE); (2) Preparation of reprocessable acrylic rubber (2.1) mixing 17-19 mole parts of butyl acrylate, 0.5-1 mole parts of a dynamic crosslinking agent containing a diborate ester, 0.5-2 mole parts of dimethylaminoethyl methacrylate, and 54 mole parts of N,N-dimethylacetamide; (2.2) bubbling nitrogen for 30 minutes at room temperature, and then heating in an oil bath at 65° C. until all monomers are completely dissolved, to obtain a second mixture; (2.3) adding an initiator azobisisobutyronitrile to the second mixture, wherein the amount of azobisisobutyronitrile added is 0.2% of the total mass of the second mixture; reacting in an oven at a temperature of 70° C. in a nitrogen atmosphere for 5 hours; and volatilizing the solvent in a vacuum oven at a temperature of 90° C. for 48 hours to obtain a reprocessable acrylic rubber, i.e., an acrylic rubber cross-linked by dynamic covalent bonds based on phenyl borate; The reprocessable acrylic rubber has a tensile strength of 0.2 to 1.3 MPa, an elongation at break of 224.1 to 770.7%, an elongation at break after reprocessing of 183.7 to 554.9%, and a change rate of elongation at break of -32 to -18%.

2. The preparation method according to claim 1, characterized in that: In step (1.3), the developing solvent used in the column separation is prepared by uniformly mixing ethyl acetate and petroleum ether in a volume ratio of 4:1.

Citation Information

Cited By

  • Photosensitive functional monomer and method for preparing photocuring 3D printing polyurethane elastomer by using same

    CN119462718A

  • A photosensitive functional monomer and a method for preparing a light-cured 3D printing polyurethane elastomer using the same

    CN119462718B