High-temperature-resistant flame-retardant polyvinyl chloride cable material and preparation method thereof
Through the combination of polyvinyl chloride, polyphenylene sulfide resin, epoxy resin and nanofiller, combined with silane coupling agent modification technology, the problem of softening and combustion of polyvinyl chloride cables at high temperatures is solved, and the flexibility and resistance are improved Flammability extends the service life of the cable and prevents cracking.
Patent Information
- Application Number
- CN202410821103.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
PVC cables are prone to soften, burn and produce smoke under high temperature conditions, and their flexibility is greatly reduced after adding a large amount of inorganic filler, making it prone to cracking.
Using a combination of polyvinyl chloride, polyphenylene sulfide resin, epoxy resin, nanofiller, light calcium carbonate, compatibility agent, thermal stabilizer and flame retardant, the nanofiller is modified by silane coupling agent to improve the cable Flexibility, high temperature resistance and flame retardancy reduce the amount of nanofiller to prevent cracking.
It achieves excellent flexibility, high temperature resistance, insulation and flame retardancy of the cable, extends service life, avoids cracking, and improves mechanical strength and impact resistance.
Smart Images

Figure BDA0004909115230000061 
Figure BDA0004909115230000071 
Figure BDA0004909115230000081
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of cable material processing, and more specifically, to a high temperature resistant and flame retardant polyvinyl chloride cable material and a preparation method thereof. Background Art
[0002] Polyvinyl chloride (PVC) is a material with excellent mechanical properties, aging resistance and electrical properties, and is often used in the preparation of cables. PVC will decompose at around 100°C, making it easy for PVC to soften at temperatures above 100°C, greatly reducing the original structural stability of wires and cables, and thus greatly reducing the mechanical properties and insulation of the cables. At the same time, PVC will burn and produce a lot of smoke under continuous high temperature conditions, causing great harm to the human body and the environment.
[0003] In order to improve the high temperature resistance and flame retardancy of polyvinyl chloride, a large amount of inorganic filler is usually added to polyvinyl chloride. The amount of inorganic filler exceeds 50% of the amount of polyvinyl chloride. Combined with high temperature resistant plasticizers and flame retardants, its heat resistance and flame retardancy can be improved, allowing it to remain stable at higher temperatures.
[0004] However, by adding a large amount of nano-fillers, the flexibility of the cable will be greatly reduced, and it is easy to crack during use. Especially when used outdoors for a long time, it will further accelerate the cracking of the cable. Summary of the invention
[0005] In order to solve the problem that adding a large amount of inorganic fillers into polyvinyl chloride will greatly reduce the flexibility of the cable, the present application provides a high temperature resistant and flame retardant polyvinyl chloride cable material and a preparation method.
[0006] In the first aspect, the present application provides a high temperature resistant flame retardant polyvinyl chloride cable material, which adopts the following technical scheme: a high temperature resistant flame retardant polyvinyl chloride cable material is prepared from the following raw materials in parts by weight: Polyvinyl chloride 50-80 parts Polyphenylene sulfide resin 5-9 parts Epoxy resin 10-15 parts Nano filler 15-20 parts Light calcium carbonate 5-10 parts Compatibilizer 1-3 parts Heat stabilizer 4-7 parts Flame retardant 4-6 parts 3-5 parts of plasticizer.
[0007] By adopting the above technical scheme, the prepared cable material has excellent flexibility, high temperature resistance, insulation, weather resistance and flame retardancy, and is not prone to cracking during use. At the same time, a large amount of nanofillers does not need to be added in this application. The addition of polyphenylene sulfide resin in this application can increase the stability of the cable structure and greatly improve the high temperature resistance and flame retardancy of the cable. However, the flexibility of polyphenylene sulfide resin is poor, which will cause the flexibility of the cable to deteriorate. In the case of frequent bending or movement, the cable may break or break due to stress concentration, thereby affecting the use of the cable. This application adds an appropriate amount of epoxy resin to share with polyphenylene sulfide resin, which can not only effectively solve the problem of poor flexibility of polyphenylene sulfide resin, but also further improve the high temperature resistance and insulation of the cable. At the same time, the use of polyvinyl chloride, polyphenylene sulfide resin and epoxy resin in common can significantly improve the weather resistance of the cable and extend the service life of the cable.
[0008] The compatibility between polyvinyl chloride, polyphenylene sulfide resin and epoxy resin is poor, and it is difficult to mix the three together. By adding an appropriate amount of compatibilizer, the compatibility between the three can be greatly improved. By adding a small amount of nanofiller, the mechanical strength and flame retardancy of the cable material can be improved, and the cable cracking can be effectively prevented.
[0009] The addition of light calcium carbonate is to improve the strength and impact resistance of the cable, and to improve the processing performance of polyvinyl chloride, polyphenylene sulfide resin and epoxy resin. In the melt processing of polyvinyl chloride, light calcium carbonate can play a lubricating role, reduce melt viscosity, and improve fluidity, thereby helping to reduce energy consumption in the processing process and improve production efficiency.
[0010] By adding heat stabilizers, the cable can maintain stable electrical and mechanical properties in high temperature environments, thereby improving the safety and reliability of the cable; flame retardants can reduce the flammability of cable materials, slow down the spread of flames, and reduce toxic smoke produced during combustion; plasticizers can improve the flexibility and impact resistance of cables in low temperature environments.
[0011] Preferably, the nanofiller is a modified nanofiller prepared by the following method: A: Mix the solvent and silane coupling agent evenly, raise the temperature to 50-70°C, add the nanofiller, stir and react for 3-4 hours, filter, rinse and dry to obtain the silanized nanofiller; B: Mix epoxidized soybean oil, vinyl acrylic acid, pentaerythritol triacrylate and initiator to form a mixed solution, then heat it to 60-70°C, add silanized nanofiller, stir for 5-7h, filter, and obtain modified nanofiller.
[0012] Preferably, the nanofiller includes at least one of silicon dioxide, ceramic powder, sintered kaolin, attapulgite and barium sulfate.
[0013] Preferably, the average particle size of the nanofiller is 200-500 nm.
[0014] By adopting the above technical scheme, the compatibility of inorganic nano nanofiller with polyvinyl chloride, polyphenylene sulfide resin and epoxy resin is greatly improved, and the nano filler can be fully dispersed in the cable material system, further improving the mechanical strength of the cable. The nano filler used in this application is nano-grade, and the amount used is small, so that the dispersibility of the nano filler in the cable material system is greatly reduced. In this application, a silane coupling agent is first reacted with the nano filler to improve the dispersibility of the nano filler, and under the action of an initiator, epoxy soybean oil, vinyl acrylic acid, pentaerythritol triacrylate, and an initiator are polymerized on the surface of the silanized nano filler, so that the surface of the silanized nano filler is coated with a polymer, the dispersibility of the nano filler is improved, and the compatibility of the nano filler with polyvinyl chloride, polyphenylene sulfide resin and epoxy resin is improved, thereby improving the flexibility, high temperature resistance, insulation, weather resistance and flame retardancy of the cable, and effectively preventing the cable from cracking.
[0015] Preferably, the weight parts of the main raw materials for preparing the modified nanofiller are as follows: Silane coupling agent 3-6 parts Nano filler 15-20 parts Epoxidized soybean oil 4-9 parts Vinyl acrylic 3-5 parts Pentaerythritol triacrylate 2-6 parts Initiator 0.2-0.5 parts.
[0016] By adopting the above technical scheme, the dosage of the main raw materials for preparing modified nanofillers is optimized, the dispersibility of the nanofillers is further improved, the combination of the nanofillers with polyvinyl chloride, polyphenylene sulfide resin, and epoxy resin is promoted, the flexibility, high temperature resistance, insulation, weather resistance, and flame retardancy of the cable are improved, and the cable cracking is effectively prevented.
[0017] Preferably, the silane coupling agent includes at least one of N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N, β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-aminoethylaminopropyltrimethoxysilane.
[0018] By adopting the above technical solution, the type of silane coupling agent is optimized, the silanization efficiency of the nanofiller is improved, and the efficiency of polymer-coated nanofiller is further improved, thereby improving the dispersion effect of the nanofiller.
[0019] Preferably, each portion of the compatibilizer is obtained by mixing ethylene-butyl acrylate copolymer, maleic anhydride grafted polyethylene, ethylene-acrylate-glycidyl methacrylate terpolymer and maleic anhydride grafted ethylene-octene copolymer in a weight ratio of (4-6): (2-4): (1-3): 3.
[0020] By adopting the above technical scheme, the compatibility between polyvinyl chloride, polyphenylene sulfide resin and epoxy resin can be greatly improved, the flexibility, high temperature resistance, insulation, weather resistance and flame retardancy of the cable can be improved, and the cable cracking can be effectively prevented.
[0021] Preferably, each portion of the flame retardant is obtained by mixing zinc borate, antimony trioxide and tricresyl phosphate in a weight ratio of (15-18): (10-15):5.
[0022] By mixing the above three flame retardants, the flame retardant effect of the cable can be further improved and the generation of smoke can be reduced. Among them, zinc borate can release moisture and boric acid at high temperature, reduce the surface temperature of the material and form a protective borate glass layer; when the polyvinyl chloride material is decomposed by heat, hydrogen chloride will be released, and antimony trioxide can react with antimony oxide to form compounds such as antimony chloride and antimony oxychloride, which can form a dense protective layer on the surface of the material, isolating oxygen and heat, thereby further slowing down the combustion speed; and tricresyl phosphate can further isolate oxygen and heat by forming a dense carbon layer. The three can effectively prevent cable combustion through different flame retardant pathways.
[0023] Preferably, the plasticizer is trioctyl trimellitate and / or isooctyl alcohol (2-ethylhexanol).
[0024] Trioctyl trimellitate has good heat resistance and migration resistance, which can significantly improve the flexibility of cables. At the same time, the volatility of trioctyl trimellitate is low, which helps to maintain the durability of the plasticizing effect. Isooctanol (2-ethylhexanol has good weather resistance and helps to extend the service life of plasticized polymers. When trioctyl trimellitate and isooctanol are used in combination, the two can produce a synergistic plasticizing effect, which can further improve the flexibility and heat resistance of cables.
[0025] Preferably, the heat stabilizer is at least one of a calcium zinc stabilizer, a zinc barium stabilizer, a barium cadmium stabilizer and an organic weak acid salt.
[0026] By adopting the above technical solution, the decomposition and aging of polyvinyl chloride under high temperature conditions can be prevented in one step, and the heat resistance of polyvinyl chloride can be effectively improved, thereby improving the high temperature resistance of the cable.
[0027] In a second aspect, the present application provides a method for preparing a high temperature resistant flame retardant polyvinyl chloride cable material, using the following technical solution: A method for preparing a high temperature resistant flame retardant polyvinyl chloride cable material comprises the following preparation steps: S1. Add polyvinyl chloride, polyphenylene sulfide resin, epoxy resin and compatibilizer into a high-speed mixer, then add plasticizer into the mixer, raise the temperature to 60-65°C, mix the materials at high speed for 15-25 minutes, then stop the high-speed mixer, add nano filler, light calcium carbonate, heat stabilizer and flame retardant into the mixer, mix at high speed for 40-60 minutes, and then release the materials for standby use; S2. Feed the mixed material into the feeding hopper of the granulator, start the granulator, control the speed of the granulator to 400-500r / min, control the temperatures of zones 1-3, 4-6, 7-9, 10, 11 and 12 of the granulator to 100-125°C, 125-130°C, 135-140°C, 130-135°C, 130-135°C and 125-130°C respectively, control the material temperature to 100-105°C and the material pressure to 10-12MPa.
[0028] By adopting the above technical solution, various raw materials can be fully mixed, thereby improving the flexibility, high temperature resistance, insulation, weather resistance and flame retardancy of the cable, and it is not easy to crack during use.
[0029] In summary, this application has the following beneficial effects: 1. In this application, by adding polyphenylene sulfide resin and epoxy resin, the stability of the cable can be further improved, and the cable has good high temperature resistance, insulation and flame retardancy, and also has good flexibility. At the same time, through the action of the compatibilizer, the compatibility between polyvinyl chloride, polyphenylene sulfide resin and epoxy resin is improved, and the processing performance of the three is improved by combining light calcium carbonate, which is conducive to forming a cable with a stable structure. In this application, there is no need to add a large amount of nanofillers, and at the same time, a proper amount of plasticizer, flame retardant and heat stabilizer are combined to further improve the flexibility, high temperature resistance, insulation, weather resistance and flame retardancy of the cable material.
[0030] 2. In the present application, the nanofiller is first treated with a silane coupling agent to make the nanofiller silanized, and then epoxy soybean oil, vinyl acrylic acid, pentaerythritol triacrylate, and an initiator are mixed and reacted with the silanized nanofiller to coat the surface of the nanofiller with a polymer, thereby improving the dispersibility of the nanofiller and promoting the compatibility of the nanofiller with polyvinyl chloride, polyphenylene sulfide resin, and epoxy resin, thereby improving the flexibility, high temperature resistance, insulation, weather resistance and flame retardancy of the cable, and effectively preventing the cable from cracking. DETAILED DESCRIPTION Example
[0031] Polyvinyl chloride was purchased from Dongguan Dongying Plastic Co., Ltd. with brand number 1070 and item number HH7001G1A1OQ.
[0032] Polyphenylene sulfide resin was purchased from Dongguan Xinshengli Plastic New Material Technology Co., Ltd. with the brand number 1140A65HF2000.
[0033] The epoxy resin was purchased from Jinan Huijinchuan Trading Co., Ltd. The brand is Dow and the model is DER667E.
[0034] Ethylene-butyl acrylate copolymer was purchased from Shanghai Huzi Plastic Raw Materials Co., Ltd. with the brand number 30BA02.
[0035] Maleic anhydride grafted polyethylene was purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd. with the product number ZJ006.
[0036] Ethylene-acrylate-glycidyl methacrylate terpolymer was purchased from Dongguan Shenghao Plastic Raw Materials Co., Ltd. with the brand name PTW.
[0037] Maleic anhydride grafted ethylene-octene copolymer was purchased from Dongguan Yingxiang Plastic Raw Materials Co., Ltd., brand Dow, grade 8137.
[0038] Example 1 A high temperature resistant flame retardant polyvinyl chloride cable material is prepared by the following method: S1, 500g of polyvinyl chloride, 50g of polyphenylene sulfide resin, 100g of epoxy resin and 10g of compatibilizer are added to a high-speed mixer, and then 30g of plasticizer is added to the mixer, the temperature is raised to 60°C, the materials are mixed at high speed for 15min and then the high-speed mixer is stopped, and then 200g of nano filler, 50g of light calcium carbonate, 40g of heat stabilizer and 40g of flame retardant are added to the mixer, and the materials are discharged for standby after high-speed mixing for 40min; S2. Feed the mixed materials into the feeding hopper of the granulator, start the granulator, control the speed of the granulator to 400r / min, control the temperatures of zones 1 to 3, 4 to 6, 7 to 9, 10, 11 and 12 of the granulator to 100°C, 125°C, 135°C, 130°C, 130°C and 125°C respectively, control the material temperature to 100°C, and control the material pressure to 10MPa.
[0039] The difference between Example 2-3 and Example 1 is that the types, amounts and parameters of some raw materials for preparing high temperature resistant flame retardant polyvinyl chloride cable materials are different. The specific differences are shown in Table 1: Table 1 Types, amounts and parameters of raw materials for preparing high temperature resistant flame retardant polyvinyl chloride cable materials in Examples 1-3 Example 4 A high temperature resistant flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 1 is that the nanofiller is a modified nanofiller prepared by the following method: A: Mix 100 g of solvent and 30 g of silane coupling agent evenly, raise the temperature to 50°C, add 150 g of nanofiller, stir and react for 3 h, filter, rinse, and dry to obtain silanized nanofiller; B: 40 g of epoxidized soybean oil, 30 g of vinyl acrylate, 20 g of pentaerythritol triacrylate and 2 g of initiator were mixed, the temperature was raised to 60°C, silanized nanofiller was added, stirred for 5 h, filtered, and modified nanofiller was obtained.
[0040] The difference between Example 5-6 and Example 4 is that the types, amounts and parameters of some raw materials for preparing the modified nanofillers are different. The specific differences are shown in Table 2: Table 2 Types, amounts and parameters of raw materials for modified nanofillers in Examples 4-6 Example 7 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 4 is that the silane coupling agent is replaced with an equal amount of solvent, and the other raw material types, materials used and experimental parameters are consistent with those of embodiment 4.
[0041] Example 8 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 4 is that hydroxyethyl methacrylate is replaced with an equal amount of epoxy soybean oil, and the other raw material types, materials and experimental parameters are consistent with those of embodiment 4.
[0042] Example 9 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 4 is that hydroxyethyl methacrylate is replaced with an equal amount of vinyl acrylate, and the other raw material types, materials and experimental parameters are consistent with those of embodiment 4.
[0043] Example 10 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 4 is that hydroxyethyl methacrylate is replaced by an equal amount of pentaerythritol triacrylate, and the other raw material types, materials used and experimental parameters are consistent with those of embodiment 4.
[0044] Embodiment 11 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 1 is that the compatibilizer is obtained by mixing 4g of ethylene-butyl acrylate copolymer, 2g of maleic anhydride grafted polyvinyl chloride, 1g of ethylene-acrylate-glycidyl methacrylate terpolymer and 3g of maleic anhydride grafted ethylene-octene copolymer in a weight ratio of 4:2:1:3.
[0045] Example 12 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 4 is that the compatibilizer is obtained by mixing 3.75g of ethylene-butyl acrylate copolymer, 2.5g of maleic anhydride grafted polyvinyl chloride, 1.875g of ethylene-acrylate-glycidyl methacrylate terpolymer and 1.875g of maleic anhydride grafted ethylene-octene copolymer in a weight ratio of 6:4:3:3.
[0046] Example 13 A high temperature resistant flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 1 is that the flame retardant is obtained by mixing 20g of zinc borate, 13.4g of antimony trioxide and 6.7g of tricresyl phosphate in a weight ratio of 15:10:5.
[0047] Embodiment 14 A high temperature resistant flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 4 is that the flame retardant is obtained by mixing 18.9g of zinc borate, 15.7g of antimony trioxide and 5.3g of tricresyl phosphate in a weight ratio of 18:15:5.
[0048] Embodiment 15 A high temperature resistant flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 12 is that the flame retardant is obtained by mixing 18.9g of zinc borate, 15.7g of antimony trioxide and 5.3g of tricresyl phosphate in a weight ratio of 18:15:5.
[0049] Comparative Example Comparative Example 1 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 1 is that polyimide resin is used to replace an equal amount of polyphenylene sulfide resin, and the other raw material types, materials used and experimental parameters are consistent with those in embodiment 1.
[0050] The polyimide resin was purchased from Dongguan Deyu Plastic Co., Ltd. The brand is SABIC and the grade is XH1005.
[0051] Comparative Example 2 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 1 is that nano filler is used to replace an equal amount of polyphenylene sulfide resin, and the other raw material types, materials used and experimental parameters are consistent with those in embodiment 1.
[0052] Comparative Example 3 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 1 is that polycarbonate resin is used to replace an equal amount of epoxy resin, and the other raw material types, materials used and experimental parameters are consistent with those in embodiment 1.
[0053] Polycarbonate resin was purchased from Guangzhou Jingchen Plastic Chemical Co., Ltd. with warehouse barcode szgzsc9375.
[0054] Comparative Example 4 A high temperature resistant and flame retardant polyvinyl chloride cable material. The difference between this embodiment and embodiment 1 is that nano filler is used to replace an equal amount of epoxy resin, and the other raw material types, materials used and experimental parameters are consistent with those in embodiment 1.
[0055] Performance testing The high temperature resistant flame retardant polyvinyl chloride cable materials prepared in Examples 1-15 and Comparative Examples 1-4 were prepared into cables, and then the cables were tested for tensile strength, elongation at break, volume resistivity at 20°C, flame retardant grade and bending test.
[0056] Detection method / test method The test reference standard for tensile strength and elongation at break is GB / T 1701-2001.
[0057] 20℃ volume resistivity: refer to IEC60167.
[0058] Flame retardant grade: refer to GB / T2408, thickness is 0.8mm.
[0059] Bending test: The cables prepared from the cable materials prepared in Examples 1-15 and the comparative example were placed in an environment of 125°C, left to stand for 500 hours, taken out, left to stand at room temperature, and then bent 90°. The number of bends at which cracks appeared was recorded. The more bends, the better the flexibility. The experimental results are shown in Table 3: Table 3 Experimental results of Examples 1-15 and Comparative Examples 1-4 From Examples 1-15 and Comparative Examples 1-4 in combination with Table 3, it can be seen that in the present application, by preparing cable materials with polyvinyl chloride, polyphenylene sulfide resin, epoxy resin, nanofiller, light calcium carbonate, compatibilizer, heat stabilizer, flame retardant and plasticizer, the tensile strength, elongation at break, insulation, flame retardancy and flexibility of the cable can be significantly improved, and the cable can be used for a long time without cracking.
[0060] By comparing Example 1 with Comparative Examples 1-4, the results of tensile strength, elongation at break and bending test in Comparative Examples 1-4 are not as good as those in Example 1; among them, in Comparative Examples 2 and Comparative Examples 4, the amount of resin was reduced and the amount of nanofiller was increased, and the results of tensile strength, elongation at break and bending test decreased instead of increased; in Comparative Examples 1 and 3, other resins were used to replace polyphenylene sulfide resin and epoxy resin respectively, and the results of tensile strength, elongation at break, flame retardancy and bending test decreased instead of increased, indicating that the present application can improve the tensile strength, elongation at break, insulation, flame retardancy and flexibility of the cable by adding an appropriate amount of polyphenylene sulfide resin and epoxy resin.
[0061] Compared with Examples 4-6, the results of tensile strength, elongation at break, flame retardancy and bending test in Example 4-6 are improved; compared with Examples 7-8, the results of tensile strength, elongation at break, flame retardancy and bending test in Example 4 are the best; it shows that the nanofiller prepared by the formula and preparation method in this application can effectively improve the tensile strength, elongation at break, insulation, flame retardancy and flexibility of the cable.
[0062] Comparing Example 1 with Example 11, and Example 4 with Example 12, the results of the tensile strength, elongation at break and bending test in Example 11 and Example 12 are improved, and the flame retardancy in Example 12 is further improved, indicating that the tensile strength, elongation at break, insulation, flame retardancy and flexibility of the cable can be improved by optimizing the type of compatibilizer.
[0063] By comparing Example 1 with Example 13, Example 4 with Example 15, and Example 12 with Example 15, the flame retardancy of Examples 13-15 is significantly improved, and the tensile strength, elongation at break and bending test of Examples 13-15 are slightly improved, indicating that by optimizing the type of flame retardant, the flame retardancy of the cable can be greatly improved, and the tensile strength, elongation at break and flexibility of the cable can be promoted.
[0064] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high temperature resistant flame retardant polyvinyl chloride cable material, characterized in that: The method is prepared by including the following raw materials in parts by weight: Polyvinyl chloride 50-80 parts Polyphenylene sulfide resin 5-9 parts Epoxy resin 10-15 parts Nano filler 15-20 parts Light calcium carbonate 5-10 parts Compatibilizer 1-3 parts Heat stabilizer 4-7 parts Flame retardant 4-6 parts 3-5 parts of plasticizer.
2. The high temperature resistant flame retardant polyvinyl chloride cable material according to claim 1, characterized in that: The nanofiller is a modified nanofiller, which is prepared by the following method: A: Mix the solvent and silane coupling agent evenly, raise the temperature to 50-70°C, add the nanofiller, stir and react for 3-4 hours, filter, rinse and dry to obtain the silanized nanofiller; B: Mix epoxidized soybean oil, vinyl acrylic acid, pentaerythritol triacrylate and initiator to form a mixed solution, then heat it to 60-70°C, add silanized nanofiller, stir for 5-7h, filter, and obtain modified nanofiller.
3. The high temperature resistant flame retardant polyvinyl chloride cable material according to claim 2, characterized in that: The weight parts of the main raw materials for preparing the modified nanofiller are as follows: Silane coupling agent 3-6 parts Nano filler 15-20 parts Epoxidized soybean oil 4-9 parts Vinyl acrylic 3-5 parts Pentaerythritol triacrylate 2-6 parts Initiator 0.2-0.5 parts.
4. The high temperature resistant flame retardant polyvinyl chloride cable material according to claim 3, characterized in that: The silane coupling agent includes at least one of N-β-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N, β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, and γ-aminoethylaminopropyltrimethoxysilane.
5. The high temperature resistant flame retardant polyvinyl chloride cable material according to claim 3, characterized in that: The nano filler includes at least one of silicon dioxide, ceramic powder, sintered kaolin, attapulgite and barium sulfate.
6. The high temperature resistant flame retardant polyvinyl chloride cable material according to claim 1, characterized in that: Each portion of the compatibilizer is obtained by mixing ethylene-butyl acrylate copolymer, maleic anhydride grafted polyethylene, ethylene-acrylate-glycidyl methacrylate terpolymer and maleic anhydride grafted ethylene-octene copolymer in a weight ratio of (4-6): (2-4): (1-3):
3.
7. The high temperature resistant flame retardant polyvinyl chloride cable material according to claim 1, characterized in that: Each portion of the flame retardant is obtained by mixing zinc borate, antimony trioxide and tricresyl phosphate in a weight ratio of (15-18): (10-15):
5.
8. The high temperature resistant flame retardant polyvinyl chloride cable material according to claim 1, characterized in that: The plasticizer is trioctyl trimellitate and / or isooctyl alcohol (2-ethylhexanol).
9. The high temperature resistant flame retardant polyvinyl chloride cable material according to claim 1, characterized in that: The heat stabilizer is at least one of a calcium zinc stabilizer, a zinc barium stabilizer, a barium cadmium stabilizer and an organic weak acid salt.
10. A method for preparing the high temperature resistant flame retardant polyvinyl chloride cable material according to any one of claims 1 to 9, characterized in that: The method comprises the following preparation steps: S1. Add polyvinyl chloride, polyphenylene sulfide resin, epoxy resin and compatibilizer into a high-speed mixer, then add plasticizer into the mixer, raise the temperature to 60-65°C, mix the materials at high speed for 15-25 minutes, then stop the high-speed mixer, then add nano filler, light calcium carbonate, heat stabilizer and flame retardant into the mixer, mix at high speed for 40-60 minutes, then discharge the materials for standby use; S2. Feed the mixed material into the feeding hopper of the granulator, start the granulator, control the speed of the granulator to 400-500r / min, control the temperatures of zones 1-3, 4-6, 7-9, 10, 11 and 12 of the granulator to 100-125℃, 125-130℃, 135-140℃, 130-135℃, 130-135℃, 125-130℃, respectively, control the material temperature to 100-105℃, and control the material pressure to 10-12MPa.
Citation Information
Cited By
Flame-retardant environment-friendly PVC cable and preparation method thereof
CN119220033A
Electric wire and cable with magnetic attraction effect and preparation method of electric wire and cable
CN119964880A
Thermoplastic polyarylene sulfide-based composite cable and preparation method thereof
CN120441983A
Wire cable with magnetic attraction effect and preparation method thereof
US12437907B1