Peelable thermal gels

Through the design of two-component thermal gel, the use of primary and crosslinked silicone oils and thermal conductivity fillers, the existing thermal gels are solved in the processing difficulties and residual problems on electronic devices, and the room temperature curing and high thermal conductivity thermal gels are achieved. Suitable for compact electronics thermal dissipation applications.

CN118895050APending Publication Date: 2024-11-05SOZOTEX PERFORMANCE MATERIALS AMERICA INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410972895.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2018-10-15
Filing Date
2018-10-22
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing thermal gels are difficult to achieve easy processing, room temperature curing, high thermal conductivity and low adhesion on electronic devices, and there are difficulties in peeling and residual problems, especially in the case of intensive chip layout.

Method used

Using a two-component thermal gel, the first component contains primary silicone oil, inhibitors and catalysts, and the second component contains crosslinked silicone oil and thermal filler, by controlling the ratio of Si-H groups to vinyl groups and catalyst concentration , achieve room temperature curing and high thermal conductivity, and improve peelability through specific stirring and vacuum treatment steps.

Benefits of technology

A high thermal conductivity thermal gel that cures in-situ at room temperature can be easily applied and removed, avoiding residues, and is suitable for compact electronic heat dissipation applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895050A_ABST
    Figure CN118895050A_ABST
Patent Text Reader

Abstract

The invention relates to peelable thermal gels. The present disclosure provides a two-component peelable thermal gel that can be used to transfer heat from heat-generating electronic devices, such as computer chips, to heat dissipation structures, such as heat sinks and heat sinks. The two-component peelable thermal gels are mixed prior to the point in time of application and facilitate catalytic crosslinking. The thermal gel comprises a first component and a second component, the first component comprises primary silicone oil, an inhibitor, a catalyst and at least one heat conducting filler, and the second component comprises primary silicone oil, cross-linked silicone oil and at least one heat conducting filler. Wherein the ratio of the total content of Si-H groups to the total content of vinyl groups in the thermal gel is between 0.03 and 10. The thermal gel is peelable from the substrate to which the thermal gel is applied.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application date of October 22, 2018, application number 201880075737.6, and name “Peelable Thermal Gel”. Technical Field

[0002] The present disclosure relates generally to thermogels, and more particularly to two-component thermogels. Background Art

[0003] Thermal interface materials (TIMs) and thermal gels are widely used to dissipate heat from electronic components such as central processing units, video graphics arrays, servers, game consoles, smart phones, LED boards, etc. Thermal interface materials are typically used to transfer excess heat from electronic components to a heat sink, such as a heat sink.

[0004] In the electronics industry, it is desirable to minimize the size of the final device. This means that the size of the printed circuit board (PCB) also needs to be reduced, resulting in a greater number of semiconductor chips being required on a smaller, more compact PCB area. In some of these applications, a single heat sink can be used to cover multiple chips to achieve heat dissipation purposes and reduce assembly costs. However, there are challenges in assembling a heat sink on a chip when the available space on the chip is limited.

[0005] Due to the differences in their individual components, different chips may have different heights on the same PCB. This means that there will be different gaps between the top surface of different chips and the heat sink, i.e., a common minimum board line thickness (BLT) cannot be achieved for all chips.

[0006] Generally speaking, thermal gel is applied to a printed circuit board (PCB) including one or more chips on its surface. Many thermal gels are single-component systems in which the components are mixed together before shipping, storage and use. The thermal gel fills the gaps between the chips, thereby providing a horizontal surface on which a heat sink can be applied. However, due to the dense layout of the chips, if the thermal gel needs to be reworked or reapplied, it will be a challenge to remove the thermal gel residue between the chip spacing gaps. In addition, in order to achieve a high heat dissipation connection, the thermal gel needs to have a high thermal conductivity. In addition, in order to cure the thermal gel, heat needs to be applied, which may change the function of the chip and / or PCB.

[0007] Therefore, there is a need for improved thermal gels that provide easy handling, room temperature curing, high thermal conductivity, and low adhesion to enable peelability without residue. Summary of the invention

[0008] The present disclosure provides a two-component strippable thermal gel, which can be used to transfer heat from heat-generating electronic devices such as computer chips to heat dissipation structures such as heat sinks and heat sinks. The two-component strippable thermal gel is mixed before the time point of application and is conducive to catalytic cross-linking. The thermal gel comprises a first component and a second component, the first component comprising a primary silicone oil, an inhibitor, a catalyst and at least one thermally conductive filler, and the second component comprising a primary silicone oil, a cross-linked silicone oil and at least one thermally conductive filler, wherein the thermal gel can be stripped from a substrate on which the thermal gel is applied. In order to increase the strippability of the thermal gel, the ratio of the total content of Si-H groups in the thermal gel to the total content of vinyl groups is controlled in the range of 0.03 to 10.

[0009] In an exemplary embodiment, a thermogel is provided. The thermogel comprises: a first component, the first component comprising: a primary silicone oil; an inhibitor; a catalyst; and at least one thermally conductive filler; a second component, the second component comprising: a primary silicone oil; a cross-linked silicone oil; and at least one thermally conductive filler; wherein the primary silicone oil of the first component is a vinyl silicone oil, the primary silicone oil of the second component is a vinyl silicone oil, and the cross-linked second silicone oil of the second component is a hydrogen silicone oil; and wherein the thermogel can be peeled off from a substrate to which the thermogel is applied. In a more specific embodiment, the thermogel cures in situ at room temperature.

[0010] In a more specific embodiment, the at least one thermally conductive filler of the first component has an average particle size between 5 microns and 80 microns. In another more specific embodiment, the at least one thermally conductive filler of the first component comprises between 20% and 25% by weight of a first thermally conductive filler having an average particle size of 70 microns; and between 20% and 25% by weight of a second thermally conductive filler having an average particle size of 5 microns. In another more specific embodiment, the ratio of the total content of Si-H groups to the total content of vinyl groups is between 0.03 and 10. In another more specific embodiment, the concentration of the catalyst in the thermogel is greater than 100 ppm.

[0011] In yet another more specific embodiment, the weight ratio between the first component and the second component is between 0.5:1 and 2:1. In yet another more specific embodiment, the primary silicone oils of the first component and the second component each have a kinematic viscosity greater than 1000 cSt. In yet another more specific embodiment, the thermogel cures at a temperature between room temperature and 100°C. In a more specific embodiment of any of the above embodiments, the viscosity of the first component is at least 100 Pa.s and the viscosity of the second component is at least 100 Pa.s. In another more specific embodiment, the thermal conductivity of the thermogel is at least 2 W / mK. In a more specific embodiment of any of the above embodiments, the catalyst is a Pt-based catalyst having a weight loading of at least 2000 ppm in the first component.

[0012] In another exemplary embodiment, a method for preparing a thermal gel is provided. The method includes: preparing a first component, wherein the preparation step includes: adding silicone oil, an inhibitor, and a catalyst to a reaction vessel to form a mixture, and stirring the mixture at a first rate; adding a first thermally conductive filler to the reaction vessel, and stirring the mixture at a second rate; adding a second thermally conductive filler to the reaction vessel, and stirring the mixture at a third rate; applying a vacuum to the reaction vessel, and stirring the mixture at a fourth rate; removing the vacuum from the reaction vessel, and transferring the mixture to an ejector; compressing the mixture into a syringe; preparing a second component, wherein the preparation step includes: adding a first silicone oil and a second silicone oil to a second reaction vessel to form a second mixture, and stirring the second mixture at a sixth rate; adding a first thermally conductive filler to a second reaction vessel, and stirring the mixture at a seventh rate; adding a second thermally conductive filler to a second reaction vessel, and stirring the mixture at an eighth rate; applying a vacuum to the second reaction vessel, and stirring the mixture at a ninth rate; removing the vacuum from the second reaction vessel, and transferring the mixture to a second ejector; and compressing the mixture into a syringe.

[0013] In a more specific embodiment, the method further comprises applying a vacuum to the eductor to remove air from the mixture.

[0014] In another exemplary embodiment, an electronic device is provided. The electronic device includes: (I) at least two heat sources; (II) a thermally conductive composite material cured by a thermal gel and applied to the at least two heat sources, the thermally conductive composite material comprising: a first component, the first component comprising: silicone oil; an inhibitor; a catalyst; and at least one thermally conductive filler; a second component, the second component comprising: a first silicone oil; a second silicone oil; and at least one thermally conductive filler; wherein the silicone oil of the first component is vinyl silicone oil, the first silicone oil of the second component is vinyl silicone oil, and the second silicone oil of the second component is hydrogen silicone oil; and (III) a heat sink or a radiator applied to the thermally conductive composite material.

[0015] In a more specific embodiment of any of the above embodiments, the ratio of the total content of Si-H groups to the total content of vinyl groups in the thermal gel is between 0.03 and 10. In a more specific embodiment of any of the above embodiments, the thermally conductive composite material is cured by the gel at room temperature. In a more specific embodiment of any of the above embodiments, the thermally conductive composite material is cured by the gel at room temperature to 100°C. In a more specific embodiment, the at least two heat sources include a bare chip, or a chip covered by a heat sink, or a bare chip on a PCB, or a chip covered by a heat sink on a PCB, or a capacitor on a PCB, or a resistor on a PCB, or a printed circuit on a PCB, or a combination thereof. In an exemplary embodiment, the thermally conductive composite material leaves no residue on the heat source.

[0016] This application may include the following technical solutions.

[0017] Scheme 1. A thermal gel comprising:

[0018] A first component, the first component comprising:

[0019] Primary silicone oil;

[0020] Inhibitors;

[0021] Catalysts; and

[0022] at least one thermally conductive filler;

[0023] A second component, the second component comprising:

[0024] Primary silicone oil;

[0025] Cross-linked silicone oil; and

[0026] at least one thermally conductive filler;

[0027] wherein the primary silicone oil of the first component is vinyl silicone oil, the primary silicone oil of the second component is vinyl silicone oil, and the cross-linked second silicone oil of the second component is hydrogen-containing silicone oil; and

[0028] The thermal gel can be peeled off from the substrate on which the thermal gel is applied.

[0029] Option 2. The thermogel according to Option 1, wherein the thermogel cures in situ at room temperature.

[0030] Option 3. The thermal gel according to Option 1, wherein the at least one thermally conductive filler of the first component and the second component each has an average particle size between 5 microns and 80 microns.

[0031] Option 4. A thermal gel according to Option 1, wherein the at least one thermally conductive filler of the first component comprises between 20% by weight and 25% by weight of a first thermally conductive filler, the first thermally conductive filler having an average particle size of 70 microns; and between 20% by weight and 25% by weight of a second thermally conductive filler, the second thermally conductive filler having an average particle size of 5 microns.

[0032] Scheme 5. The thermogel according to Scheme 1, wherein the ratio of the total content of Si-H groups to the total content of vinyl groups is between 0.03 and 10.

[0033] Option 6. The thermal gel according to Option 1, wherein the concentration of the catalyst in the thermal gel is greater than 100 ppm.

[0034] Embodiment 7. The thermal gel according to embodiment 1, wherein the weight ratio between the first component and the second component is between 0.5:1 and 2:1.

[0035] Embodiment 8. The thermogel according to Embodiment 1, wherein the primary silicone oils of the first component and the second component each have a kinematic viscosity greater than 1000 cSt.

[0036] Embodiment 9. The thermogel according to embodiment 1, wherein the viscosity of the first component is at least 100 Pa.s, and the viscosity of the second component is at least 100 Pa.s.

[0037] Embodiment 10. The thermogel according to embodiment 1, wherein the thermal conductivity of the thermogel is at least 2 W / mK. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The above and other features and advantages of the present disclosure and the manner in which they are achieved will become more apparent and the invention itself will be better understood by referring to the following description of embodiments of the present invention taken in conjunction with the accompanying drawings, in which:

[0039] Figure 1 is a flow chart of a method involving preparing a first component of a thermal gel;

[0040] Figure 2 is a flow chart of a method involving preparing a second component of a thermogel;

[0041] Figure 3 It involves Figure 1 and Figure 2 A flow chart of a method for preparing a thermogel;

[0042] FIG. 4A to FIG. 4C relates to Comparative Example 1 and shows the sample applied to a substrate and its removal from the substrate;

[0043] FIG. 4D to FIG. 4F relates to Comparative Example 2 and illustrates the sample applied to a substrate and its removal from the substrate;

[0044] Figure 5A relates to Example 1 and shows the application of a sample to a substrate and its removal from the substrate;

[0045] Figure 5B relates to Example 1 and illustrates a sample applied between a first substrate and a second substrate and its removal from the first substrate and the second substrate; and

[0046] Figure 6 Methods of applying and removing samples for electronics applications are shown.

[0047] Corresponding reference characters indicate corresponding parts throughout the several views.The exemplifications set forth herein illustrate exemplary embodiments of the invention, and such exemplifications are not to be construed as limiting the scope of the invention in any way. DETAILED DESCRIPTION

[0048] A. Thermal gel

[0049] The present disclosure provides a two-component peelable thermal gel, which can be used to transfer heat from heat-generating electronic devices such as computer chips to heat-dissipating structures such as heat sinks and heat sinks. The two-component peelable thermal gel is mixed before the time point of application and is conducive to catalytic cross-linking. The thermal gel comprises a first component and a second component, the first component comprising a primary silicone oil, an inhibitor, a catalyst and at least one thermally conductive filler, and the second component comprising a primary silicone oil, a cross-linked silicone oil and at least one thermally conductive filler, wherein the thermal gel can be peeled from a substrate on which the thermal gel is applied.

[0050] 1. First component

[0051] In some exemplary embodiments, the viscosity of the first component of the thermogel described below is as low as at least 50 Pa.s, at least 75 Pa.s, at least 100 Pa.s, as high as at least 150 Pa.s, at least 175 Pa.s, at least 200 Pa.s, or in any range defined between any two of the above values, such as between at least 50 Pa.s and at least 200 Pa.s, at least 75 Pa.s and at least 175 Pa.s, or at least 100 Pa.s and 150 Pa.s. In an exemplary embodiment, the viscosity of the first component is at least 100 Pa.s.

[0052] a. Primary silicone oil

[0053] The thermogel comprises a primary silicone oil. In an exemplary embodiment, the primary silicone oil may comprise one or more polysiloxanes. The polysiloxanes are used to wet the thermally conductive filler and form a dispensable fluid of the thermogel. The polysiloxanes comprise one or more crosslinkable groups such as vinyl, hydride, hydroxyl and acrylate functional groups that are crosslinked by a catalyst. In one embodiment, the one or more polysiloxanes comprise vinyl silicone oil.

[0054] Exemplary silicone oils may include vinyl silicone oils having the general formula shown below:

[0055]

[0056] The molar ratio of vinyl groups in silicone oil is tested by iodine titration. The iodine titration method includes: weighing 1-2 grams of silicone oil and placing it in a conical flask wrapped in tin foil. An excess of iodine bromide (IBr) solution (in n-pentane solution with an available rate) is added to the flask, and the flask is further sealed to avoid exposure. Then, after one hour, the seal is opened and 50mL of a 1% by weight potassium iodide (KI) aqueous solution is added. The solution is then vibrated for 1-2 minutes. A standard 0.1mol / L sodium thiosulfate (Na2S2O3) aqueous solution is added, and the sample solution is titrated while vibrating. 1mL of a 1% by weight starch aqueous solution is added to the solution as an indicator. When the color of the solution (e.g., blue) changes, the titration is stopped and the consumption of sodium thiosulfate is calculated. This process is then repeated for other samples. To prepare a control sample, this process is repeated without using silicone oil. The molar ratio (mmol / g) of vinyl groups is as follows:

[0057]

[0058] Wherein N1 is the molar ratio of vinyl groups (mmol / g); Va is the volume of sodium thiosulfate solution titrated with the vinyl silicone oil sample (ml); Vb is the volume of sodium thiosulfate solution titrated with the blank sample (ml); G1 is the weight of the vinyl silicone oil (g); M1 is the molar concentration of the standard sodium thiosulfate solution (mol / l).

[0059] The amount of the molar ratio (mmol / g) of the vinyl group in the silicone oil can be as low as 0.0001, 0.001, 0.01, 0.1, as high as 0.5, 1, 5, 10, or in any range defined between any two of the above values, such as 0.01 to 1, 0.1 to 0.5, or 0.0001 to 10. In an exemplary embodiment, the amount of the molar ratio of the vinyl group is between 0.1 and 0.3.

[0060] The vinyl functional silicone oil comprises an organosilicon component having Si-CH=CH2 groups. Exemplary vinyl functional silicone oils include vinyl terminated silicone oils, and vinyl grafted silicone oils in which Si-CH=CH2 groups are grafted onto the polymer chain, and combinations thereof.

[0061] Exemplary vinyl terminated silicone oils include vinyl terminated polydimethylsiloxanes such as DMS-V05, DMS-V21, DMS-V22, DMS-V25, DMS-V25R, DMS-V35, DMS-V35R, DMS-V51, and DMS-V52, all available from Gelest, Inc.

[0062] Exemplary vinyl grafted silicone oils include vinyl methylsiloxane-dimethylsiloxane copolymers, such as trimethylsiloxy terminated silicone oils, silanol terminated silicone oils, and vinyl terminated silicone oils. Exemplary trimethylsiloxy terminated silicone oils include VDT-127, VDT-431, and VDT-731; exemplary silanol terminated silicone oils include VDS-1013; and exemplary vinyl terminated silicone oils include VDV-0131; all available from Gelest, Inc.

[0063] In an exemplary embodiment, the vinyl grafted silicone oil is a vinyl methyl siloxane terpolymer, including a vinyl methyl siloxane-octyl methyl siloxane-dimethyl siloxane terpolymer, such as VAT-4326, or a vinyl methyl siloxane-phenyl methyl siloxane-dimethyl siloxane terpolymer, such as VPT-1323. In some exemplary embodiments, the vinyl grafted silicone oil is a vinyl methoxy siloxane homopolymer, such as VMM-010, or a vinyl ethoxy siloxane-propyl ethoxy siloxane copolymer, such as VPE-005. VAT-4326, VPT-1323, VMM-010, and VPE-005 are all available from Gelest, Inc.

[0064] In an exemplary embodiment, the vinyl functional silicone oil includes a vinyl T resin or a vinyl Q resin. Vinyl T resins are vinyl silsesquioxanes having three (trisubstituted) oxygens that replace all or some of the silicon atoms in the polymer. Exemplary T resins include poly (phenyl-vinyl silsesquioxanes), such as SST-3PV1 purchased from Gelest, Inc. Vinyl Q resins have four (tetrasubstituted) oxygens that replace all or some of the silicon atoms in the polymer. Exemplary Q resins include VQM-135, VQM-146 purchased from Gelest, Inc. One type of vinyl Q resin is an activated curing specialty silicone rubber having the following base polymer structure:

[0065]

[0066] Exemplary Q resins include VQM-135, VQM-146 available from Gelest, Inc. In an exemplary embodiment, the polysiloxane is a vinyl functional oil, such as RH-Vi303, RH-Vi301 available from RUNHE, such as RH-Vi303, RH-Vi301 available from AB Specialty Silicones, and RH-Vi303, ... VS200, VS1000.

[0067] The kinematic viscosity of an exemplary primary silicone oil can be as low as 5 cSt, 100 cSt, 500 cSt, as high as 5,000 cSt, 10,000 cSt, 50,000 cSt, or any range defined between any two of the above values, as measured according to ASTM D445. In an exemplary embodiment, the kinematic viscosity of the vinyl silicone oil is in the range of 1000 cSt to 5000 cSt. A thermogel with too low a kinematic viscosity may result in evaporation of components of the thermogel or oil exudation of the thermogel when applied to a device.

[0068] Based on the total weight of the thermogel, the amount of the primary silicone oil gel can be as low as 1 wt%, 2 wt%, 4 wt%, as high as 6 wt%, 8 wt%, 10 wt%, or in any range defined between any two of the above values, such as 1 wt% to 10 wt%, 1 wt% to 5 wt%, or 4 wt% to 5 wt%. In an exemplary embodiment, the first component of the thermogel comprises a primary silicone oil in an amount of 4.854 wt%.

[0069] The weight (M) of the exemplary silicone oil w ) The average molecular weight can be as low as 50 Daltons, 100 Daltons, 1000 Daltons, 10,000 Daltons, 50,000 Daltons, 70,000 Daltons, 100,000 Daltons, as high as 1,000,000 Daltons, 10,000,000 Daltons, 100,000,000 Daltons, or in any range defined between any two of the above values, such as between 50 Daltons and 100,000,000 Daltons, 1000 Daltons to 10,000,000 Daltons, or 50,000 Daltons to 1,000,000 Daltons.

[0070] The vinyl group content (mmol) of the primary silicone oil in the first component was calculated by dividing the molar ratio of the vinyl group (mmol / g) by the weight (g) of the primary silicone oil of the first component.

[0071] b. Catalyst

[0072] The thermogel also includes one or more catalysts for catalyzing the addition reaction. Exemplary catalysts include platinum-containing materials. The presence of the catalyst allows a higher crosslinking rate at room temperature. For the purposes of this disclosure, room temperature is defined as between 15° C. and 25° C. An exemplary platinum-containing catalyst may have a general formula as shown below:

[0073]

[0074] Exemplary platinum-containing catalysts include: such as platinum cyclovinylmethylsiloxane complex (Ashby Karstedt catalyst), platinum carbonyl cyclovinylmethylsiloxane complex (Ossko catalyst), platinum divinyltetramethyldisiloxane dimethylfumarate complex, platinum divinyltetramethyldisiloxane dimethylmaleate complex, etc. Examples of platinum carbonyl cyclovinylmethylsiloxane complexes include SIP6829.2, examples of platinum divinyltetramethyldisiloxane complexes include SIP6830.3 and SIP6831.2, and examples of platinum cyclovinylmethylsiloxane complexes include SIP6833.2, all of which are available from Gelest, Inc.

[0075] Without wishing to be bound by any particular theory, it is believed that the platinum catalyst reacts with the vinyl silicone oil and the hydrogen containing silicone oil as shown below.

[0076]

[0077] Based on the total weight of the silicone oil, the thermal gel can be as low as 5ppm, 10ppm, 15ppm, 20ppm, 25ppm, 30ppm, 40ppm, 50ppm, 100ppm, as high as 200ppm, 500ppm, 1000ppm, 5000ppm, 10000ppm, 100000ppm, or in any range defined between any two values ​​above, such as 10ppm to 200ppm, 20ppm to 1000ppm or 5ppm to 10000ppm The amount of one or more catalysts. In an exemplary embodiment, the catalyst is a Pt-based catalyst with at least 2000ppm weight loading in the first component. The presence of the catalyst makes the crosslinking rate at room temperature higher.

[0078] In an exemplary embodiment, the catalyst is provided in the form of a mixture with one or more silicone oils. In an exemplary embodiment, the catalyst is mixed with a vinyl functional silicone oil, such as KE-1012-A, KE-1031-A, KE-109E-A, KE-1051J-A, KE-1800T-A, KE1204A, KE1218A available from Shin-Etsu, such as KE-1060-A, KE-1061-A, KE-1062-A, KE-1063-A, KE-1064-A, KE-1065-A, KE-1066-A, KE-1067-A, KE-1068-A, KE-1069-A, KE-1110-A, KE-1121-B, KE-1130-B, KE-1131 RT Gel 4725SLD A, such as available from Wacker 612A, LR 3153A, LR 3003A, LR3005A, 961A, 927A, 205A, 9212A, 2440, such as available from Momentive LSR 2010A, such as available from Dow Corning RBL-9200A, RBL-2004A, RBL-9050A, RBL-1552A, FL 30-9201A, 9202A, 9204A, 9206A, 184A, Dow QP-1A, Dow C6A, Dow CV9204 A. In an exemplary embodiment, the catalyst is mixed with a vinyl and hydride functional silicone oil, such as KE-1056, KE-1151, KE-1820, KE-1825, KE-1830, KE-1831, KE-1833, KE-1842, KE-1884, KE-1885, KE-1886, FE-57, FE-61 available from Shin-Etsu, such as KE-1151, KE-1820, KE-1825, KE-1830, KE-1831, KE-1833, KE-1842, KE-1884, KE-1885, KE-1886, FE-57, FE-61 available from Dow Corning, 7395, 7610, 7817, 7612, 7780.

[0079] Based on the total weight of the thermogel, the thermogel can contain a catalyst in an amount as low as 0.001 wt%, 0.005 wt%, 0.01 wt%, as high as 0.015 wt%, 0.020 wt%, 0.025 wt%, or in any range defined between any two of the above values. In an exemplary embodiment, the thermogel contains a catalyst in an amount of 0.019 wt%.

[0080] c. Inhibitors

[0081] The thermogel comprises one or more addition inhibitors for inhibiting or limiting the reaction of the primary silicone oil and the crosslinked silicone oil (as discussed herein) of the second component. Without wishing to be bound by any particular theory, it is believed that in the absence of the addition inhibitor, the primary silicone oil reacts very rapidly with the crosslinked functional silicone oil based on an addition hydrosilylation mechanism to form a solid phase that cannot be automatically distributed by typical methods. The addition inhibitor comprises at least one acetylenic compound, and optionally, the addition inhibitor further comprises a polyvinyl functional polysiloxane.

[0082] Exemplary addition inhibitors include alkynols such as 1-ethynyl-1-cyclohexanol, 2-methyl-3-butyn-2-ol, 2-phenyl-3-butyn-2-ol, 2-ethynyl isopropanol, 2-ethynyl-butane-2-ol, and 3,5-dimethyl-1-hexyn-3-ol; silylated alkynols such as trimethyl(3,5-dimethyl-1-hexyn-3-oxy)silane, dimethyl-bis(3-methyl-1-butyn-oxy)silane, methylvinylbis(3-methyl-1-butyn-3-oxy)silane, and ((1,1-dimethyl-2-propynyl)oxy)trimethylsilane; unsaturated carboxylic acid esters such as diallyl maleate, dimethyl maleate, diethyl fumarate, diallyl fumarate, and bis-2-methoxy-1-methylethyl maleate, maleic acid fumarate / alcohol mixtures, such as wherein the alcohol is selected from benzyl alcohol or 1-octanol and ethynylcyclohexyl-1-ol; conjugated enynes, such as 2-isobutyl-1-butene-3-yne, 3,5-dimethyl-3-hexene-1-yne, 3-methyl-3-pentene-1-yne, 3-methyl-3-hexene-1-yne, 1-ethynylcyclohexene, 3-ethyl-3-butene-1-yne and 3-phenyl-3-butene-1-yne; vinyl cyclosiloxanes, such as 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, and mixtures of conjugated enynes and vinyl cyclosiloxanes. In an exemplary embodiment, the addition inhibitor is selected from 2-methyl-3-butyn-2-ol or 3-methyl-1-pentyn-3-ol.

[0083] In some exemplary embodiments, the addition inhibitor further comprises a polyvinyl functional polysiloxane. An exemplary polyvinyl functional polysiloxane is a vinyl terminated polydimethylsiloxane in ethynyl cyclohexanol, such as Pt inhibitor 88 available from Wacker Chemie AG. Without wishing to be bound by any particular theory, it is believed that the platinum catalyst forms a complex with the ethynyl cyclohexanol and the vinyl terminated polydimethylsiloxane, as shown below.

[0084]

[0085] It is believed that the formation of the complex reduces the catalyst activity at room temperature and thus maintains the dispensability and wettability of the TIM. At higher cure step temperatures, the Pt is released from the complex and aids in the hydrosilylation of the vinyl-functional silicone oil and the hydride-functional silicone oil, providing better control of the "crosslinking".

[0086] In some exemplary embodiments, the thermogel may include one or more addition inhibitors in an amount as low as 0.001 wt%, 0.002 wt%, 0.005 wt%, 0.01 wt%, 0.015 wt%, as high as 0.02 wt%, 0.025 wt%, 0.03 wt%, 0.05 wt%, 0.1 wt%, or in any range defined between any two of the foregoing values, such as 0.001 wt% to 0.1 wt%, 0.001 wt% to 0.05 wt%, or 0.005 wt% to 0.02 wt%, based on the total weight of the thermogel. In an exemplary embodiment, the thermogel includes an addition inhibitor in an amount of 0.005 wt%.

[0087] In an exemplary embodiment, the addition inhibitor is mixed with a functional silicone oil, such as KE-1056, KE-1151, KE-1820, KE-1825, KE-1830, KE-1831, KE-1833, KE-1842, KE-1884, KE-1885, KE-1886, FE-57, FE-61 available from Shin-Etsu, such as KE-1151, KE-1820, KE-1825, KE-1830, KE-1831, KE-1833, KE-1842, KE-1884, KE-1885, KE-1886, FE-57, FE-61 available from Dow Corning, 7395, 7610, 7817, 7612, 7780.

[0088] 2. Second component

[0089] a. Primary silicone oil

[0090] According to the above description, the second component of the thermogel contains primary silicone oil. Within the scope of the present disclosure, the primary silicone oil of the first component and the primary silicone oil of the second component are different silicone oil compounds. Also within the scope of the present disclosure, the primary silicone oil of the first component and the primary silicone oil of the second component are the same silicone oil compound.

[0091] The vinyl group content (mmol) of the primary silicone oil in the second component was calculated by dividing the molar ratio (mmol / g) of the vinyl group by the weight (g) of the primary silicone oil of the second component.

[0092] The total content of vinyl groups in the total formulation (T 乙烯基 , mmol).

[0093] b. Cross-linked silicone oil

[0094] The thermogel may also include a crosslinked silicone oil. The crosslinked silicone oil may include Si-H groups. Exemplary silicone oils include hydrogenated silicone oils having the general formula shown below. Exemplary hydrogenated silicone oils act as a crosslinking agent in an addition reaction with a primary silicone oil.

[0095]

[0096] The molar ratio of Si-H groups in cross-linked silicone oil is tested by iodine titration. The iodine titration method includes: weighing about 0.1 grams of hydrogenated silicone oil and placing it in a conical flask wrapped in tin foil. 20mL of carbon tetrachloride (CCl4) is added to the flask to dissolve the silicone oil, and the flask is further sealed to avoid exposure. Then, an excess of bromoacetic acid solution (available rate is about 10mL) is added to the flask together with 10mL of water. The flask is further sealed to avoid exposure. After thirty minutes, the seal is opened and 25ml of 10% by weight potassium iodide (KI) aqueous solution is added to the solution. The solution is then vibrated for 1 to 2 minutes. Then a standard 0.1mol / L sodium thiosulfate (Na2S2O3) aqueous solution is added, and the sample solution is titrated while vibrating. 1mL of 1% by weight starch aqueous solution is added to the solution as an indicator. When the color of the solution (e.g., blue) changes, the titration is stopped and the consumption of sodium thiosulfate is calculated. This process is then repeated for other samples. In order to prepare a control sample, this process is repeated without using silicone oil. The content of Si-H groups (mmol / g) is as follows

[0097]

[0098] Wherein: N2 is the molar ratio of Si-H groups (mmol / g); Vd is the volume of sodium thiosulfate solution titrated with the hydrogenated silicone oil sample (ml); Vc is the volume of sodium thiosulfate solution titrated with the blank sample (ml); G2 is the weight of hydrogenated silicone oil (g); M2 is the molar concentration of standard sodium thiosulfate solution (mol / l).

[0099] The amount of the molar ratio (mmol / g) of Si-H groups in the silicone oil can be as low as 0.0001, 0.001, 0.01, 0.1, as high as 1, 5, 10, 50, or in any range defined between any two of the above values, such as 0.01 to 1, 0.1 to 5, or 0.0001 to 50. In an exemplary embodiment, the amount of the molar ratio of Si-H groups is 0.2 to 2.

[0100] In an exemplary embodiment, the crosslinked silicone oil includes a hydride functional silicone oil having an organosilicon component and Si-H groups. Exemplary hydride functional silicone oils include hydride terminated silicone oils, and hydride grafted silicone oils in which Si-H groups are grafted onto polymer chains, and combinations thereof.

[0101] In an exemplary embodiment, the hydride-terminated silicone oil is a hydride-terminated polydimethylsiloxane, such as DMS-H05, DMS-H21, DMS-H25, DMS-H31 or DMS-H41, all available from Gelest, Inc. In an exemplary embodiment, the hydride-terminated silicone oil is a methylhydrogensiloxane-dimethylsiloxane copolymer, such as trimethylsiloxy-terminated or hydride-terminated. Exemplary trimethylsiloxy-terminated copolymers include HMS-013, HMS-031, HMS-064, HMS-071, HMS-082, HMS-151, HMS-301, HMS-501; exemplary hydride-terminated copolymers include HMS-H271; all available from Gelest, Inc. In an exemplary embodiment, the hydride-grafted silicone oil is a trimethylsiloxy-terminated polymethylhydrogensiloxane, such as HMS-991, HMS-992, HMS-993, all available from Gelest, Inc.

[0102] In an exemplary embodiment, the hydride grafted silicone oil is a triethylsiloxy terminated polyethylhydrogensiloxane, such as HES-992 available from Gelest, Inc. In an exemplary embodiment, the hydride grafted silicone oil is a methylhydrogensiloxane-octylmethylsiloxane copolymer, such as HAM-301 available from Gelest, Inc.

[0103] In an exemplary embodiment, the hydride functional oil is a Q resin or a T resin. Exemplary T resins include SST-3MH1.1, and exemplary Q resins include HQM-105 and HQM-107, all available from Gelest, Inc.

[0104] In an exemplary embodiment, the polysiloxane is a hydride functional oil such as AB Specialty Silicones. XL-10, XL-12, such as RH-DH04 and RH-H503 purchased from RUNHE, such as KE-1012-B, KE-1031-B, KE-109E-B, KE-1051J-B, KE-1800T-B, KE1204B, KE1218B purchased from Shin-Etsu, such as KE-1012-B, KE-1031-B, KE-109E-B, KE-1051J-B, KE-1800T-B, KE1204B, KE1218B purchased from Bluestar RT Gel 4725SLD B, such as available from Wacker 612B, LR 3153B, LR 3003B, LR 3005B, 961B, 927B, 205B, 9212B, 2440, such as available from Momentive LSR 2010B, such as available from Dow Corning RBL-9200B, RBL-2004B, RBL-9050B, RBL-1552B, FL 30-9201B, 9202B, 9204B, 9206B, 184B, Dow QP-1B, Dow C6 B, Dow CV9204B.

[0105] In an exemplary embodiment, the polysiloxane comprises a silicone rubber, such as the KE series products available from Shin-Etsu, such as the PTFE series products available from Bluestar, Such as those purchased from Wacker and Such as those purchased from Momentive Such as Dow Corning (Dow Corning) and Such as those available from AB Specialty Silicones Other polysiloxanes were purchased from Wacker, Shin-etsu, Dowcoring, Momentive, Bluestar, RUNHE, AB Specialty Silicones, and Gelest.

[0106] As measured according to ASTM D445, the kinematic viscosity of exemplary cross-linked silicone oils can be as low as 0.5 cSt, 5 cSt, 100 cSt, 200 cSt, as high as 1,000 cSt, 10,000 cSt, 100,000 cSt, or in any range defined between any two of the above values, such as between 0.5 cSt and 100,000 cSt, 5 cSt and 10,000 cSt, 100 cSt and 1,000 cSt, or 200 cSt and 1,000 cSt. In an exemplary embodiment, the kinematic viscosity of the cross-linked silicone oil is between 300 cSt and 700 cSt.

[0107] The cross-linked silicone oil can be present in an amount as low as 0.1 wt%, 0.2 wt%, 0.4 wt%, as high as 0.6 wt%, 0.8 wt%, 1.0 wt%, or in any range defined between any two of the above values, such as 0.1 wt% to 1.0 wt%, 0.1 wt% to 0.5 wt%, or 0.1 wt% to 0.4 wt%, based on the total weight of the thermogel.

[0108] In an exemplary embodiment, the second component of the thermogel comprises the primary silicone oil in the first component in an amount of 4.746 wt % and the cross-linked silicone oil in an amount of 0.26 wt %.

[0109] The weight (M) of the exemplary silicone oil w) The average molecular weight can be as low as 50 Daltons, 100 Daltons, 1000 Daltons, 10,000 Daltons, 50,000 Daltons, 70,000 Daltons, 100,000 Daltons, as high as 1,000,000 Daltons, 10,000,000 Daltons, 100,000,000 Daltons, or in any range defined between any two of the above values, such as between 50 Daltons and 100,000,000 Daltons, 1000 Daltons to 10,000,000 Daltons, or 50,000 Daltons to 1,000,000 Daltons.

[0110] The total content of Si-H groups in the total formulation (T) was calculated by dividing the molar ratio of Si-H groups of the cross-linked silicone oil in the second component (mmol / g) by the weight of the cross-linked silicone oil in the second component (g). Si-H , mmol).

[0111] By T Si-H / T 乙烯基 Calculated total Si-H group content (T Si-H ) and the total content of vinyl groups (T 乙烯基 ) can be as low as 0.0001, 0.001, 0.01, as high as 0.1, 1, 10, 100, 1000, or in any range defined between any two of the above values, such as between 0.001 and 0.1, 0.01 and 1, or 0.001 and 100. In an exemplary formulation, the total content of Si-H groups (T Si-H ) and the total content of vinyl groups (T 乙烯基 ) can be between 0.03 and 10.

[0112] 3. Thermally conductive filler

[0113] The first component and the second component of the thermogel contain one or more thermally conductive fillers. However, within the scope of the present disclosure, only one of the first component and the second component of the thermogel contains one or more thermally conductive fillers. Additionally, within the scope of the present disclosure, neither the first component nor the second component of the thermogel contains one or more thermally conductive fillers.

[0114] In an exemplary embodiment, both the first component and the second component contain bimodal aluminum filler, wherein a primary filler and a secondary filler are provided. The primary filler acts as an extender and serves to provide a component matrix for the components, while the secondary filler has a filling / uniformity function, wherein the gaps within the matrix formed by the primary filler are filled.

[0115] Exemplary thermally conductive fillers include metals, alloys, non-metals, metal oxides and ceramics, and combinations thereof. Metals include, but are not limited to, aluminum, copper, silver, zinc, nickel, tin, indium and lead. Non-metals include, but are not limited to, carbon, graphite, carbon nanotubes, carbon fibers, graphene, boron nitride and silicon nitride. Metal oxides or ceramics include, but are not limited to, aluminum oxide (aluminum oxide), aluminum nitride, boron nitride, zinc oxide and tin oxide.

[0116] The thermogel may contain the mixed thermally conductive filler in a total amount as low as 75 wt%, 77 wt%, 80 wt%, as high as 90 wt%, 92 wt%, 95 wt%, or in any range defined between any two of the above values, such as 75 wt% to 95 wt%, or 77 wt% to 92 wt%, or 80 wt% to 90 wt%, based on the total weight of the thermogel.

[0117] The average particle size (D) of the exemplary thermally conductive filler as measured by a laser diffraction analyzer according to ASTM B822 is 50 : Mass median diameter (MMD) or mass average particle size or log-normal distribution mass median diameter) can be as low as 5 microns, 10 microns, 20 microns, up to 40 microns, 60 microns, 80 microns, or in any range defined between any two of the above values.

[0118] In an exemplary embodiment, the first component and / or the second component of the thermal gel may include a first thermally conductive filler and a second thermally conductive filler, wherein the first thermally conductive filler is a plurality of metal particles having a particle size of 70 microns, and the second thermally conductive filler is a plurality of metal particles having a particle size of 5 microns. In a more specific embodiment, the ratio of the first thermally conductive filler to the second thermally conductive filler may be as low as 1:5, 1:4, 1:3, 1:2, as high as 1:1, 1.5:1, 2:1, 3:1, 4:1, 5:1, or in any range defined between any two of the above values, such as 1:5 to 5:1, 1:1 to 3:1, or 1.5:1 to 3:1.

[0119] 4. Additives (colorants)

[0120] The thermogel includes a colorant to distinguish the two components, such as organic and inorganic pigments and organic dyes. It is within the scope of the present disclosure that only one of the first component and the second component of the thermogel includes a colorant or other additive. It is also within the scope of the present disclosure that both the first component and the second component of the thermogel include a colorant or other additive. In addition, it is within the scope of the present disclosure that neither the first component nor the second component of the thermogel includes a colorant or other additive.

[0121] Exemplary organic pigments include: benzimidazolone, such as blue-toned benzimidazolone pigment Novoperm Carmine HF3C from Clariant International Ltd, Muttenz Switzerland. Exemplary inorganic pigments include carbon black and iron-based compounds. Exemplary iron-based compounds include iron oxide compounds such as α-Fe2O3, α-Fe2O3·H2O, Fe3O4, and combinations thereof. Exemplary organic dyes include: benzo[kl]thioxanthene-3,4-diimide, N-octadecyl-(8CI); benzothioxanthene-3,4-dicarboxylic acid-N-stearylimide.

[0122] In some exemplary embodiments, the colorant is an inorganic pigment selected from: α-Fe2O3; α-Fe2O3·H2O; and Fe3O4.

[0123] In some exemplary embodiments, the colorant is an organic pigment. In a more specific embodiment, the colorant is an organic substance selected from formula (I)-(XVI).

[0124] In a more specific embodiment, the colorant is an organic pigment of formula (I), also known as Pigment Red 176, and having CAS number 12225-06-8.

[0125]

[0126] In a more specific embodiment, the colorant is an organic pigment of formula (II), also known as calcium bis[4-[[1-[[(2-methylphenyl)amino]carbonyl]-2-oxopropyl]azo]-3-nitrobenzenesulfonate, and having CAS number 12286-66-7.

[0127]

[0128] In a more specific embodiment, the colorant is an organic pigment of formula (III), also known as 4,4'-[(3,3'-dichloro[1,1'-diphenyl]-4,4'-diyl)bis(azo)]bis[4,5-dihydro-5-oxo-1-phenyl-1h-pyrazole-3-carboxylic acid diethyl ester], and having CAS number 6358-87-8.

[0129]

[0130] In a more specific embodiment, the colorant is an organic pigment of formula (IV), also known as 2,2'-[(3,3'-dichloro[1,1'-diphenyl]-4,4'-diyl)bis(azo)]bis[N-(2,4-dimethylphenyl)-3-oxo-butyramide, and having CAS number 5102-83-0.

[0131]

[0132] In a more specific embodiment, the colorant is an organic pigment of formula (V), also known as (29H,31H-phthalocyaninato (2-)-N29,N30,N31,N32) copper, and having CAS number 147-14-8.

[0133]

[0134] In a more specific embodiment, the colorant is an organic pigment of formula (VI), also known as brilliant green phthalocyanine, and having CAS number 1328-53-6.

[0135]

[0136] In a more specific embodiment, the colorant is an organic pigment of formula (VII), also known as 9,19-dichloro-5,15-diethyl-5,15-dihydro-diindolo[2,3-c:2',3'-n]triphenoldioxazine, and having CAS number 6358-30-1.

[0137]

[0138] In a more specific embodiment, the colorant is an organic pigment of formula (VIII), also known as 5,12-dihydroquinone[2,3-b]acridine-7,14-dione; 5,12-dihydroquinone[2,3-b]acridine-7,14-dione, and having CAS number 1047-16-1.

[0139]

[0140] In a more specific embodiment, the colorant is an organic pigment of formula (IX), also known as 2,9-bis(3,5-dimethylphenyl)anthraquino[2,1,9-def:6,5,10-d'e'f']diisoquinoline-1,3,8,10(2h,9h)-tetraone, and having CAS number 4948-15-6.

[0141]

[0142] In a more specific embodiment, the colorant is an organic pigment of formula (X), also known as 4,4'-diamino-[1,1'-dianthracene]-9,9',10,10'-tetraone or Pigment Red 177, and having CAS number 4051-63-2.

[0143]

[0144] In a more specific embodiment, the colorant is an organic pigment of formula (XI), also known as 3,3'-[(2-methyl-1,3-phenylene)diimino]bis[4,5,6,7-tetrachloro-1H-isoindol-1-one], and having CAS number 5045-40-9.

[0145]

[0146] In a more specific embodiment, the colorant is an organic pigment of formula (XII), also known as calcium bis[4-[[1-[[(2-chlorophenyl)amino]carbonyl]-2-oxopropyl]azo]-3-nitrobenzenesulfonate], and having CAS number 71832-85-4.

[0147]

[0148] In a more specific embodiment, the colorant is an organic pigment of (XIII), also known as 3,4,5,6-tetrachloro-N-[2-(4,5,6,7-tetrachloro-2,3-dihydro-1,3-dioxo-1H-inden-2-yl)-8-quinolyl]phthalimide, and having CAS number 30125-47-4.

[0149]

[0150] In a more specific embodiment, the colorant is an organic pigment of formula (XIV), also known as [1,3-dihydro-5,6-bis[[(2-hydroxy-1-naphthyl)methylene]amino]-2H-benzimidazol-2-one acid (2-)-N5,N6,O5,O6]nickel, and having CAS number 42844-93-9.

[0151]

[0152] In a more specific embodiment, the colorant is an organic pigment of formula (XV), also referred to as Pigment Red 279, and has CAS No. 832743-59-6, wherein each R is independently selected from hydrogen, alkyl, aryl and halogen. In an even more specific embodiment, each R is independently selected from hydrogen, C1-C6 alkyl, phenyl and halogen. In another more specific embodiment, each R is chlorine, and even more specifically, each R is 7-chlorine.

[0153]

[0154] In a more specific embodiment, the colorant is an organic pigment of formula (XVI), also known as pyrimido[5,4-g]pteridine-2,4,6,8-tetraamine, 4-methylbenzenesulfonate, base hydrolyzed, and having CAS number 346709-25-9.

[0155]

[0156] In a more specific embodiment, the colorant is α-Fe2O3, such as iron red purchased from BAI YAN Company (BAIYAN). In another more specific embodiment, the colorant is α-Fe2O3·H2O, such as iron yellow purchased from BAI YAN Company (BAI YAN). In another more specific embodiment, the colorant is Fe3O4, such as iron blue purchased from BAI YAN Company (BAI YAN). In another more specific embodiment, the colorant is a pigment of formula (I), which has a chemical formula C 32 H 24 N6O5, such as Novoperm Carmine HF3C, available from Clariant International Ltd, Muttenz Switzerland.

[0157] In some exemplary embodiments, the thermogel includes a colorant in an amount as low as 0.001 wt%, 0.005 wt%, 0.01 wt%, as high as 0.015 wt%, 0.02 wt%, 0.025 wt%, 0.03 wt%, 0.05 wt%, or in any range defined between any two of the foregoing values, such as 0.001 wt% to 0.05 wt% or 0.005 wt% to 0.02 wt%, based on 100 wt% of the thermogel without the colorant.

[0158] B. Methods of Forming Thermal Gels

[0159] See also Figure 1, a method 100 for preparing a first component of a thermogel is shown. At step 102, a reaction vessel is opened, and silicone oil, an inhibitor, and a catalyst are weighed and added to the reaction vessel to form a mixture. The mixture is stirred for a period of time. Exemplary stirring rates may be as low as 20 revolutions per minute (rpm), 25 rpm, 30 rpm or less, as high as 35 rpm, 37 rpm, 40 rpm, or within any range defined between any two of the above values. Exemplary time periods for stirring rates are as little as 1 minute, 3 minutes, 5 minutes, and as much as 6 minutes, 8 minutes, 10 minutes, or within any range defined between any two of the above values. In an exemplary embodiment, the mixture is stirred for 5 minutes at a rate less than 30 rpm.

[0160] Then method 100 proceeds to step 104, in which the first thermally conductive filler and pigment are added to the reaction vessel. The resulting mixture in the reaction vessel is then stirred for a period of time. An exemplary stirring rate can be as low as 5 revs / min (rpm), 7rpm, below 9rpm, as high as 10rpm, 12rpm, 15rpm, or in any range defined between any two of the above values. An exemplary time period of the stirring rate is as little as 1 minute, 3 minutes, 5 minutes, as much as 6 minutes, 8 minutes, 10 minutes, or in any range defined between any two of the above values. In an exemplary embodiment, the mixture is stirred for 5 minutes at a rate lower than 10rpm.

[0161] Then method 100 proceeds to step 106, in which a second thermally conductive filler is added to the reaction vessel, and the resulting mixture is stirred at a first rate in a first time period, and then stirred at a second rate in a second time period. Exemplary stirring rates may be as low as 5 revs / min (rpm), 10rpm, 20rpm, 30rpm or less, as high as 40rpm, 50rpm, 60rpm, 70rpm, or in any range defined between any two of the above values. Exemplary time periods of stirring rates are as little as 5 minutes, 10 minutes, 20 minutes, 30 minutes, as much as 40 minutes, 50 minutes, 60 minutes, 70 minutes, or in any range defined between any two of the above values. In an exemplary embodiment, the mixture is stirred at 10rpm for 10 minutes, followed by stirring at 54rpm for 1 hour.

[0162] Then, method 100 advances to step 108, in which the mixture is placed under vacuum in the reaction vessel while continuing to stir for a period of time. Exemplary stir speeds may be as low as 40 revs / min (rpm), 45rpm, below 50rpm, as high as 55rpm, 60rpm, 65rpm, 70rpm, or in any range defined between any two values ​​above. The exemplary time period of stir speed is as little as 10 minutes, 15 minutes, 20 minutes, as much as 30 minutes, 40 minutes, 50 minutes, or in any range defined between any two values ​​above. In an exemplary embodiment, the mixture is placed under vacuum and stirred at 54rpm for 30 minutes.

[0163] Then, the method 100 proceeds to step 110, in which the vacuum is stopped and the contents of the reaction vessel are transferred to an evacuator, where a vacuum is applied to remove air from the resulting paste. The vacuum is then stopped and the resulting paste is compressed into a syringe.

[0164] See also Figure 2 , a method 200 for preparing a second component of a thermogel is shown. At step 202, a reaction vessel is opened, and silicone oil and cross-linked silicone oil are weighed and added to the reaction vessel to form a mixture. The mixture is stirred for a period of time. Exemplary stirring rates may be as low as 20 revolutions per minute (rpm), 25 rpm, 30 rpm or less, as high as 35 rpm, 37 rpm, 40 rpm, or within any range defined between any two of the above values. Exemplary time periods for stirring rates are as little as 1 minute, 3 minutes, 5 minutes, and as much as 6 minutes, 8 minutes, 10 minutes, or within any range defined between any two of the above values. In an exemplary embodiment, the mixture is stirred for 5 minutes at a rate less than 30 rpm.

[0165] Then method 200 proceeds to step 204, in which the first thermally conductive filler is added to the reaction vessel. The resulting mixture in the reaction vessel is then stirred for a period of time. An exemplary stirring rate can be as low as 5 revs / min (rpm), 7rpm, below 9rpm, as high as 10rpm, 12rpm, 15rpm, or in any range defined between any two of the above values. An exemplary time period of the stirring rate is as little as 1 minute, 3 minutes, 5 minutes, as much as 6 minutes, 8 minutes, 10 minutes, or in any range defined between any two of the above values. In an exemplary embodiment, the mixture is stirred for 5 minutes at a rate lower than 10rpm.

[0166] Then method 200 proceeds to step 206, in which a second thermally conductive filler is added to the reaction vessel, and the resulting mixture is stirred at a first rate in a first time period, and then stirred at a second rate in a second time period. Exemplary stirring rates may be as low as 5 revs / min (rpm), 10rpm, 20rpm, 30rpm or less, as high as 40rpm, 50rpm, 60rpm, 70rpm, or in any range defined between any two of the above values. Exemplary time periods of stirring rates are as little as 5 minutes, 10 minutes, 20 minutes, 30 minutes, as much as 40 minutes, 50 minutes, 60 minutes, 70 minutes, or in any range defined between any two of the above values. In an exemplary embodiment, the mixture is stirred at 10rpm for 10 minutes, followed by stirring at 54rpm for 1 hour.

[0167] Then, method 200 advances to step 208, in which the mixture is placed under vacuum in the reaction vessel while continuing to stir for a period of time. Exemplary stir speeds may be as low as 40 revs / min (rpm), 45rpm, below 50rpm, as high as 55rpm, 60rpm, 65rpm, 70rpm, or in any range defined between any two values ​​above. The exemplary time period of stir speed is as little as 10 minutes, 15 minutes, 20 minutes, as much as 30 minutes, 40 minutes, 50 minutes, or in any range defined between any two values ​​above. In an exemplary embodiment, the mixture is placed under vacuum and stirred at 54rpm for 30 minutes.

[0168] The method 200 then proceeds to step 210, where the vacuum is stopped and the contents of the reaction vessel are transferred to an evacuator where a vacuum is applied to remove air from the resulting paste. The vacuum is then stopped and the resulting paste is compressed into a syringe where the components will mix.

[0169] See now Figure 3 , a method 300 for preparing a thermogel is provided. At step 302, a first component and a second component are prepared according to methods 100 and 200, respectively. Then, at step 304, the first component and the second component are mixed together in a ratio (first component: second component) as low as 0.5:1, 0.75:1, 1:1, as high as 1.5:1, 1.75:1, 2:1, or in any range defined between any two of the above values. Too large or too small a ratio (first component: second component) may cause operational inconvenience when used, because the weight change of the smaller volume component may cause a large change in the target weight ratio of the inhibitor, catalyst, cross-linked silicone oil and / or other lower load components. In an exemplary embodiment, the first component and the second component are mixed in a 1:1 ratio by a static mixer.

[0170] After the first component and the second component are mixed, the resulting mixture is then applied to a surface, as indicated at step 306. The mixture may be applied by an automatic dispenser or a manual dispenser, such as a syringe.

[0171] Figure 6 Shows the application of Figures 1 to 3 Method 600 of preparing thermal gel 608. As shown in step 610, printed circuit board (PCB) 602 includes chips 604, 606. Within the scope of the present disclosure, a greater or lesser number of chips may be provided on PCB 602. In step 620, thermal gel 608 is applied to PCB 602 and chips 604, 606 via manual dispensing or an automatic dispensing machine, as described above. Thermal gel 608 is applied so that thermal gel 608 covers the upper surfaces of chips 604, 606. Once thermal gel 608 is applied, while thermal gel 608 is curing, heat sink 612 is applied to thermal gel 608, as shown in step 630. Step 640 shows the final structure of the device when thermal gel 608 is cured to form thermally conductive composite material 609.

[0172] When rework of the thermally conductive composite material 609 is required, the thermally conductive composite material 609 can be removed from the device as shown in method 600. To remove the thermal gel 608 from the device (starting from step 640), the heat sink 612 is removed from the thermally conductive composite material 609, as shown in step 650. Then, as shown in step 660, the thermally conductive composite material 609 is removed (e.g., peeled off, Figure 5A ) to restore the device to its original state. As discussed in more detail herein, the thermally conductive composite material 609 is removed without residue on the PCB 602 and the chips 604, 606.

[0173] C. Characteristics of thermal gel

[0174] The thermogel of the present disclosure can be mixed at a ratio of about 1:1 between the first component and the second component. Advantageously, such a ratio makes preparation / mixing easy to form the thermogel. In addition, the mixing ratio allows for easy and accurate mixing of the components before the time point of application. For example, when the mixing ratio of the first component to the second component is 1:1, the thermogel can be prepared more easily in a batch process compared to a different mixing ratio.

[0175] The thermal gel obtained by methods 100, 200 and 300 can be automatically dispensed. If the thermal gel needs to be reworked or reapplied to a surface, the thermal gel will cure in place and can also be peeled off or easily removed. Therefore, the easy removability of the thermal gel can reduce cleaning time when the thermal gel needs to be reworked or reapplied.

[0176] In addition, as previously mentioned, the thermal gel can be cured in situ. After assembly, the thermal gel can begin to cure in about 2 hours and be fully cured after 24 hours to 48 hours. The curing time depends on the temperature of the surrounding environment. For example, electronic components operating at a temperature of about 80°C will result in a different curing time for the thermal gel compared to electronic components operating at a different temperature.

[0177] The thermal conductivity of the thermal gel of the present disclosure is as low as 1 W / mK, 1.5 W / mK or 2 W / mK, or as high as 2.5 W / mK, 3 W / mK or 4 W / mK, or in any range defined between any two of the above values, such as between 1 W / mK and 4 W / mK, 1.5 W / mK to 3 W / mK or 2 W / mK to 2.5 W / mK. An exemplary thermal conductivity test method standard is ASTM D5470. In an exemplary embodiment, the thermal interface material as described above has a thermal conductivity of about 2.8 W / mK.

[0178] Example

[0179] Comparison of Comparative Example 1, Comparative Example 2 and Example 1

[0180] Thermogels of Example 1 and Comparative Example 1 were prepared according to the formulations shown in Table 1 and described below. Thermogel of Comparative Example 2 was Gel 30, commercially available from Parker-Chomerics.

[0181]

[0182] Table 1

[0183] The thermogel of Example 1 is a two-component system. The primary silicone oil is polydimethylsiloxane having a vinyl group, and the primary silicone oil has a kinematic viscosity of 2000 cSt. The cross-linked silicone oil of the second component of the thermogel of Example 1 is a copolymer of methylhydrogensiloxane-dimethylsiloxane; the cross-linked silicone oil has a kinematic viscosity of 500 cSt. The total content of Si-H groups (T Si-H ) and the total content of vinyl groups (T 乙烯基 ) is 0.07. The first component and the second component are prepared according to methods 100 and 200, respectively. The first component and the second component are then mixed in a ratio of 1:1 by a static mixer, and the thermal gel of Example 1 is applied to the surface. The thermal conductivity of the obtained thermal gel of Example 1 is 3 W / mK.

[0184] The thermogel of Comparative Example 1 was prepared as a one-component system. The primary silicone oil was polydimethylsiloxane having a vinyl group; the primary silicone oil had a kinematic viscosity of 2000 cSt. The crosslinked silicone oil of the thermogel of Comparative Example 1 was a copolymer of methylhydrogensiloxane-dimethylsiloxane; the crosslinked silicone oil had a kinematic viscosity of 500 cSt. The total content of Si-H groups (T Si-H ) and the total content of vinyl groups (T 乙烯基 The thermogel of Comparative Example 2 was prepared as a one-component system and was generally based on silicone oil containing a metal oxide (alumina) filler.

[0185] Then the thermal gel of Example 1 is printed onto the heat sink 201 in a 1 mm thick sheet. Figure 5A As shown. Figure 5A As shown, after curing, the sheet of Example 1 is easily removed from the heat sink 201. In addition, the thermal gel of Example 1 is applied to the heat sink 203 in a dot pattern. The dot pattern of Example 1 is also compressed on the non-contact side by the copper plate 205. Figure 5B As shown, after curing, the thermal gel of Example 1 can be easily peeled off from the two surfaces 203, 205.

[0186] In contrast, Figure 4A As shown, the thermal gel of Comparative Example 1 is applied to the substrate 101, and as Figure 4B and Figure 4C As shown, the applied thermal gel of Comparative Example 1 cannot be easily removed and spread on the substrate 101, while that of Example 1 can be easily removed.

[0187] In addition, if Figure 4D As shown, the thermal gel of Comparative Example 2 is applied to the substrate 101, and as Figure 4E and Figure 4F As shown, the applied thermal gel of Comparative Example 1 cannot be easily removed and spread on the substrate 101, while that of Example 1 can be easily removed.

[0188] Although the present invention has been described as having an exemplary design, the present invention may be further modified within the spirit and scope of the present disclosure. Therefore, this application is intended to cover any variation, use or adaptation of the present invention using its general principles. In addition, this application is intended to cover such deviations from the present disclosure within the known or customary practice of the field to which the present invention belongs, and it falls within the scope of the appended claims.

Claims

1. A thermal gel comprising: A first component, the first component comprising: Primary silicone oil; Inhibitors; Catalysts; and at least one thermally conductive filler; A second component, the second component comprising: Primary silicone oil; Cross-linked silicone oil; as well as at least one thermally conductive filler; wherein the primary silicone oil of the first component is vinyl silicone oil, the primary silicone oil of the second component is vinyl silicone oil, and the cross-linked second silicone oil of the second component is hydrogen-containing silicone oil; and wherein the thermal gel can be peeled off from a substrate on which the thermal gel is applied; wherein the thermally conductive filler comprises a first filler having a first particle size and a second filler having a second particle size, the first particle size being different from the second particle size, and wherein the total content of the thermally conductive filler in the thermal gel is 90 wt % to 95 wt %; wherein the weight ratio between the first component and the second component is 0.5:1 to 2:1; wherein the thermal gel cures in situ at room temperature; wherein the ratio of the total content of Si-H groups of the cross-linked silicone oil to the total content of vinyl groups of the primary silicone oil is 0.03 to 10; and The concentration of the catalyst in the thermal gel is greater than 100 ppm.

2. The thermal gel according to claim 1, wherein the at least one thermally conductive filler of the first component and the second component each has an average particle size of 5 microns to 80 microns.

3. The thermogel according to claim 1, wherein the primary silicone oils of the first component and the second component each have a kinematic viscosity greater than 1000 cSt.

4. The thermogel according to claim 1, wherein the viscosity of the first component is at least 100 Pa.s and the viscosity of the second component is at least 100 Pa.s.

5. The thermogel of claim 1, wherein the thermal conductivity of the thermogel is at least 2 W / mK.

6. The thermogel of claim 1, wherein the catalyst is a platinum catalyst having a weight loading of at least 200 ppm in the first component.

Citation Information

Cited By

  • Long-life high-thermal-conductivity two-component gel as well as preparation method and application thereof