Silicon dioxide matting powder as well as preparation method and application thereof
The preparation of silica matting powder through the dual-template agent method and microwave heating technology solves the problems of complex process and high cost in the existing technology, realizes efficient and environmentally friendly matting powder production, and improves performance in UV coatings.
Patent Information
- Application Number
- CN202410921212.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
AI Technical Summary
The existing preparation methods of silica matting powder have problems such as long process flow, large energy consumption and high production costs, and poor product structural performance, making it difficult to meet complex performance indicator requirements.
The dual-template agent method is used to prepare silica matting powder with microwave heating, and the pore size and particle size are adjusted through calcium carbonate microspheres and soft template agents, and the silica gel is rapidly aged by microwave reaction, reducing production costs and improving reaction efficiency.
Preparation of silica matting powder with specific specific surface area, pore volume and particle size improves production efficiency, reduces costs, and improves curing speed and mechanical properties in UV cured coatings without the need for toxic volatile organic solvents , has environmental advantages.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of matting powder, and in particular relates to a silicon dioxide matting powder and a preparation method and application thereof. Background Art
[0002] Matting powder is a general term for materials that can absorb light, reduce light reflection on the surface of an object, and make the surface appear matte. Generally speaking, matting powder can be divided into two categories: organic matting powder and inorganic matting powder. Among them, organic matting powder mainly includes polymer materials such as paraffin, polyvinyl chloride and polymethyl methacrylate, while inorganic matting powder mainly includes materials such as silicon dioxide, diatomaceous earth, talcum powder, light calcium carbonate and kaolin. Silicon dioxide has become the most popular matting powder material because its refractive index is similar to that of most resins used in the coating industry and it has good gloss adjustment ability. However, the silica used as matting agent usually has strict requirements on performance indicators such as particle size, pore volume and specific surface area (Fan Xinhua, Zhang Yi, Pei Yali. Effect of particle size on the application performance of silica matting agent [J]. Modern Coatings and Finishing, 2009, 12 (9), 41-42.); therefore, this also has corresponding strict requirements on the preparation method of silica matting agent. The silica matting agent synthesized by the gas phase method used in the early days has been rarely used due to its harsh reaction conditions, high energy consumption and high production cost. At present, the methods for preparing silica matting powder are mainly divided into two categories: gel method and precipitation method. Among them, the advantage of gel method is that the prepared silica product has the characteristics of good structure, large specific surface area, large pore volume and narrow pore size distribution, but the disadvantage is that the process flow is relatively long and the post-processing energy consumption is relatively high, resulting in high production cost; while the advantage of precipitation method is that the process flow is relatively simple and the cost is relatively low, but the disadvantage is that the obtained product has poor structural performance, small specific surface area, small pore volume and wide pore size distribution (Kong Qinggang, Qian Haiyan, Sun Xingju, Dong Ting, Liu Kai, Zhang Xiangyu, Li Jun, Gao Guizhi. Synthesis and Characterization of Silica Matting Powder [J]. China Powder Technology, 2012, 18 (2), 50-54.). In general, the above two commonly used matting powder preparation methods still have a lot of room for improvement.
[0003] In addition, in addition to being widely used in traditional fields such as coatings, paints and coatings, matting agents have also been widely used in the field of UV curing materials (Zhang Yi, Zhang Zhouhe, Li Chunshan. Research on silica matting agents for UV coatings [J]. Shanghai Coatings, 2014, 52(2), 4-6.).
[0004] In summary, it is meaningful to improve the preparation method of silicon dioxide matting powder and explore and develop the application of the prepared matting powder. In view of this, this patent application is specially proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a silicon dioxide matting powder and a preparation method and application thereof.
[0006] In order to achieve the above object, the solution of the present invention is:
[0007] A method for preparing a silicon dioxide matting powder comprises the following steps:
[0008] (1) adding a template into a mixed solvent, and then adding an alkaline solution to prepare a mixed solution;
[0009] (2) adding calcium carbonate microspheres to the mixed solution obtained in step (1), and after uniform dispersion, adding an alkaline solution to the resulting mixture to adjust the pH value of the system to obtain a dispersion containing calcium carbonate microspheres;
[0010] (3) adding organic silicate to the dispersion containing calcium carbonate microspheres obtained in step (2), stirring evenly to obtain silica gel; then transferring the obtained silica gel to a microwave reaction tank for microwave reaction to age the silica gel;
[0011] (4) The product obtained in step (3) is cooled and filtered, the solid obtained is washed with ethanol / water until neutral and then dried, and the dried solid is made into powder and then calcined.
[0012] Furthermore, the template agent described in step (1) is one of sodium dodecyl sulfonate, dodecyltrimethylammonium chloride or dodecyltrimethylammonium bromide.
[0013] Furthermore, the mixed solvent described in step (1) is a mixture of ethanol and water; and the alkaline solution is one of an ammonia solution, a sodium hydroxide solution or a potassium hydroxide solution.
[0014] Furthermore, the alkaline solution in step (2) is one of a sodium hydroxide solution or a potassium hydroxide solution; and the pH value range is 9-12.
[0015] Furthermore, the organic silicate described in step (3) is one of ethyl orthosilicate or isopropyl orthosilicate.
[0016] Furthermore, the microwave reaction conditions in step (3) are as follows: microwave power is 250-300 W, microwave reaction temperature is 80-100° C., and microwave reaction time is 1-2 h.
[0017] Furthermore, the calcination conditions in step (4) are: calcination temperature is 800-1100° C., and calcination time is 6-10 h.
[0018] The matting powder prepared by the above preparation method is composed of silicon dioxide powder; the specific surface area of the matting powder is 150 to 300 m 2 / g, the pore volume is 1.0~2.2mL / g, and the average particle size is 1~15μm.
[0019] The application of the aforementioned silica matting powder in UV curing coatings.
[0020] Compared with the existing methods, the principles and gain effects of the present invention are as follows:
[0021] 1. The present invention prepares silica matting powder by gel method combined with dual template, wherein the calcium carbonate microspheres used are hard templates, and the pore size of the synthesized silica can be regulated by adjusting the particle size and dosage of the calcium carbonate microspheres used, and the selected soft template dodecyltrimethylammonium bromide can also adjust the particle size of the synthesized silica, so that the silica matting powder with a specific specific surface area, pore volume and particle size can be prepared by the dual template method.
[0022] 2. The preparation method of the silica matting powder provided by the present invention uses microwave heating to quickly age the silica gel. Compared with the traditional heating method, the use of microwave heating can improve the reaction kinetics so that the gel can be quickly and evenly heated during the aging process, thereby increasing the reaction rate and greatly shortening the time required for the synthesis of the silica matting powder. This not only reduces the production time cost of the matting powder, but also has the advantages of energy saving and environmental protection.
[0023] 3. The silica matting powder provided by the present invention can be successfully used to prepare UV curing coatings, mainly by utilizing the silica matting powder's ability to absorb ultraviolet light to improve the curing speed of the resulting coating; adding silica matting powder can also effectively improve the mechanical properties of the prepared coating. In addition, the preparation method of UV curing coatings provided by the present invention does not use any toxic volatile organic solvents throughout the process, and has the advantage of being green and environmentally friendly. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with the embodiments. It should also be understood that the following embodiments are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. The specific quality, reaction time and temperature, process parameters, etc. in the examples are only examples within the appropriate ranges. Some non-essential improvements and adjustments made by those skilled in the art according to the above content of the present invention all belong to the scope of protection of the present invention.
[0025] Unless otherwise specified, all reagents used were commercial reagents and were not further purified before use. The specific surface area and pore volume tests were performed using a 3H-2000PS2 specific surface pore size detector from Best Instruments; the particle size test was performed using a Beckman Coulter LS13 320XR laser diffraction particle size analyzer.
[0026] Embodiment 1:
[0027] The preparation method of silicon dioxide matting powder specifically comprises the following steps:
[0028] (1) adding 2 g of the template agent hexadecyltrimethylammonium bromide to a mixed solvent consisting of 600 mL of anhydrous ethanol and 100 mL of deionized water, and then adding 18 mL of an ammonia solution having a mass concentration of 25% to prepare a mixed solution;
[0029] (2) adding 4 g of calcium carbonate microspheres (particle size range 10-20 μm) to the mixed solution obtained in step (1), and after uniform dispersion, adding NaOH solution (1 mol / L) to the resulting mixture to adjust the pH value of the system to 9.0 to obtain a dispersion containing calcium carbonate microspheres;
[0030] (3) adding 2.1 g of tetraethyl orthosilicate to the dispersion containing calcium carbonate microspheres obtained in step (2), stirring evenly to obtain silica gel; then transferring the obtained silica gel to a microwave reaction tank for microwave reaction to age the silica gel, the microwave power being 300 W, the reaction temperature being 80° C., and the microwave reaction time being 2 h;
[0031] (4) The product obtained in step (3) was cooled and filtered, and the obtained solid was washed with ethanol / water until it was neutral (the pH test paper was used to check whether the washed solution was neutral) and then dried. The dried solid was made into powder and then placed in a muffle furnace and roasted at 950° C. for 8 hours. The obtained white powder was the silica matting powder, and the obtained silica matting powder was recorded as XG-1. The obtained silica matting powder was characterized, and the test results of specific surface area and pore volume were 221 cm 2 / g and 1.51cm 3 / g; The results of particle size analysis test: the average particle size is 5.45μm.
[0032] Example 2
[0033] The preparation of silica matting powder refers to Example 1, except that step (4) is changed to the following step: the product obtained in step (3) is cooled and filtered, the obtained solid is washed with ethanol / water until it is neutral (the pH test paper is used to check whether the washed solution is neutral) and then dried, the dried solid is made into powder and then transferred into a dielectric barrier discharge (DBD) device for low-temperature plasma treatment to remove the template agent, and the treatment is carried out in an oxygen atmosphere at a temperature of 450°C, a voltage of 220V and a current of 3A for 4 hours, and the silica matting powder is obtained by natural cooling to room temperature. The obtained silica matting powder is recorded as XG-2. The obtained silica matting powder is characterized, and the test results of specific surface area and pore volume are 218cm 2 / g and 1.50cm 3 / g; The results of particle size analysis test: the average particle size is 5.41μm.
[0034] Example 3
[0035] The preparation of silica matting powder was carried out in accordance with Example 1, except that the amount of template agent hexadecyltrimethylammonium bromide in step (1) was changed to 4 g, and other conditions were the same. The obtained silica matting powder was recorded as XG-3. The obtained silica matting powder was characterized, and the test results of specific surface area and pore volume were 257 cm 2 / g and 1.53cm 3 / g; The results of particle size analysis test: the average particle size is 8.52μm.
[0036] Example 4
[0037] The preparation of silica matting powder was carried out in accordance with Example 1, except that the composition of the mixed solvent in step (1) was changed to 400 mL of anhydrous ethanol and 300 mL of deionized water. The other conditions were the same, and the obtained silica matting powder was recorded as XG-4. The obtained silica matting powder was characterized, and the test results of specific surface area and pore volume were 162 cm 2 / g and 1.22cm 3 / g; The results of particle size analysis test: the average particle size is 4.55μm.
[0038] Example 5
[0039] The preparation of silica matting powder was carried out in accordance with Example 1, except that the particle size of the calcium carbonate microspheres used in step (2) was adjusted to 30-40 μm and the amount was 4 g; other conditions were the same, and the obtained silica matting powder was recorded as XG-5. The obtained silica matting powder was characterized, and the test results of specific surface area and pore volume were 271 cm 2 / g and 1.61cm 3 / g; the results of particle size analysis test: the average particle size is 9.75μm.
[0040] Example 6
[0041] The preparation of silica matting powder was carried out in accordance with Example 1, except that the amount of calcium carbonate microspheres used in step (2) was adjusted to 8 g; other conditions were the same, and the obtained silica matting powder was recorded as XG-6. The obtained silica matting powder was characterized, and the test results of specific surface area and pore volume were 292 cm 2 / g and 1.66cm 3 / g; The results of particle size analysis test: the average particle size is 11.58μm.
[0042] Example 7
[0043] The preparation of silica matting powder was carried out in accordance with Example 1, except that the amount of calcium carbonate microspheres used in step (2) was adjusted to 2 g; other conditions were the same, and the obtained silica matting powder was recorded as XG-7. The obtained silica matting powder was characterized, and the test results of specific surface area and pore volume were 194 cm 2 / g and 1.41cm 3 / g; The results of particle size analysis test: the average particle size is 3.66μm.
[0044] Example 8
[0045] The preparation of silica matting powder was carried out in accordance with Example 1, except that the amount of template agent hexadecyltrimethylammonium bromide in step (1) was changed to 0 g, and other conditions were the same. The obtained silica matting powder was recorded as XG-8. The obtained silica matting powder was characterized, and the test results of specific surface area and pore volume were 106 cm 2 / g and 1.13cm 3 / g; The results of particle size analysis test: the average particle size is 14.52μm.
[0046] Example 9
[0047] The preparation of silica matting powder was carried out in accordance with Example 1, except that the amount of calcium carbonate microspheres used in step (2) was adjusted to 0 g; other conditions were the same, and the obtained silica matting powder was recorded as XG-9. The obtained silica matting powder was characterized, and the test results of specific surface area and pore volume were 114 cm 2 / g and 1.21cm 3 / g; The results of particle size analysis test: the average particle size is 15.66μm.
[0048] Example 10
[0049] The steps for applying silica matting powder in UV curing coatings are as follows:
[0050] (1) Add 6 g of silica matting powder XG-1 to 45 g of tripropylene glycol diacrylate and stir evenly to prepare a dispersion containing silica matting powder;
[0051] (2) Add 45 g of polyurethane acrylate, 2 g of 2-hydroxy-2-methyl-1-phenylpropanone, 0.5 g of silicone oil, 0.5 g of CI-2212 defoamer, and 1 g of zinc oxide particles to the dispersion containing silica matting powder prepared in step (1), stir and pre-disperse until there is no solid powder in the system, and then filter with a 300-mesh gauze to obtain the UV-curable coating; the obtained UV-curable coating is recorded as NPGDA-PU-ZnO-XG-1.
[0052] The curing time test method of the prepared UV curing coating is as follows:
[0053] Treatment of substrate: Cut the tinplate sheet into a test plate with a size of 50mm×120mm×0.3mm, wipe the surface clean with alcohol and dry it under an infrared lamp, and evenly apply the prepared UV curing coating on the tinplate test plate with a scraper, with 0.2ml of coating applied each time.
[0054] Curing of coating: Irradiate the tinplate test plate coated with coating with ultraviolet light, and press the stopwatch to start timing; wherein, the ultraviolet light source used is UV-LED light source, and the wavelength of the light source used is 395nm (optional wavelengths are 365nm, 385nm, 395nm and 405nm). This application uses the time required for complete curing as the curing time; the finger-picking method is used to indicate whether it is completely cured, that is, lightly scratch the cured film layer with a fingernail, and complete curing is indicated by no shedding or scratching. The test results are shown in Table 1.
[0055] The prepared UV curing coating NPGDA-PU-ZnO-XG-1 coating was subjected to performance tests; the hardness, adhesion, water resistance and salt spray corrosion resistance of the coating were measured according to the corresponding national standards, as follows: the hardness was measured using the pencil hardness method according to the national standard GB-6739-86; the peel strength was measured according to the national standard GB / T7122-1996; the resistance to distilled water (40°C immersion) / h was measured according to the national standard GB / T5209-85, and the resistance to 3% NaCl (40°C) / h was measured according to the national standard GB / T1763-79. The matte property was tested using a 60° gloss meter (expressed as gloss), and the results are shown in Table 1.
[0056] The antibacterial properties of the prepared UV-curing coatings were tested by the film method according to the implementation standard QB / T 2591-2003 (QB / T2591-2003, Test methods and antibacterial effects of antibacterial plastics [S]. Beijing: National Development and Reform Commission of the People's Republic of China, 2003.), and the antibacterial rate of the antibacterial plastics after contact with the test bacteria for 24 hours was investigated. The total number of colonies was determined according to GB / T 4789.2-2016 (GB / T 4789.2-2016, Determination of the total number of colonies in food microbiology [S]. Beijing: State Food and Drug Administration, 2016.), and the antibacterial rate was calculated according to the following formula:
[0057] R%=(BA) / B×100%
[0058] Wherein: R: antibacterial rate, %; A: average number of recovered colonies of NPGDA-PU-ZnO-XG-1 coating samples after culturing for 24 hours; B: average number of recovered colonies of blank control samples after culturing for 24 hours, the blank control sample is a coating made of pure PU and curing agent polyamide resin (mass ratio of 1:1) according to the same method; the results are shown in Table 1.
[0059] Embodiment 11-18:
[0060] The preparation of the UV curing coating is described in reference to Example 10, except that the silica matting powder XG-1 used in step (1) is replaced with XG-2, XG-3, XG-4, XG-5, XG-6, XG-7, XG-8 and XG-9 in sequence; the remaining steps are the same as in Example 10, and the preparation and performance characterization of the obtained coating are the same as in Example 10; the results are shown in Table 1.
[0061] Table 1 Effect of different silica matting powder on the performance of UV curing coatings
[0062] Example Curing time hardness Peel strength Water resistance Salt tolerance Glossiness Antibacterial rate 10 44s 5H 9.41 144h 148h 72.1% 91.0% 11 42s 5H 9.40 144h 148h 72.4% 91.2% 12 34s 5H 9.42 144h 148h 48.3% 91.1% 13 40s 5H 9.41 144h 148h 71.6% 91.1% 14 27s 5H 9.40 144h 148h 28.9% 90.9% 15 24s 5H 9.40 144h 148h 22.5% 91.0% 16 55s 5H 9.41 144h 148h 84.1% 91.3% 17 NA NA NA NA NA NA NA 18 NA NA NA NA NA NA NA
[0063] Note: NA means that the particle size of the matting powder is too large to be made into paint; the antibacterial rate refers to the antibacterial rate against Staphylococcus aureus; water resistance and salt resistance both refer to the time without change;
[0064] Embodiment 19-21:
[0065] The preparation of UV curing coating is based on Example 10, except that the zinc oxide particles used in step (2) are replaced with titanium dioxide particles, magnesium oxide particles and aluminum oxide particles in sequence, and the remaining steps are the same as in Example 10. The preparation and performance characterization of the obtained coating are the same as in Example 10; the results are shown in Table 2.
[0066] Embodiment 22:
[0067] The preparation of the UV curing coating is based on Example 10, except that the silica matting powder XG-1 used in step (1) is replaced by XG-6, and the zinc oxide particles used in step (2) are replaced by a mixed powder consisting of magnesium oxide particles and zinc oxide particles, wherein the amount of magnesium oxide particles is 0.6 g and the amount of zinc oxide particles is 0.4 g; the remaining steps are the same as in Example 10, and the preparation and performance characterization of the obtained coating are the same as in Example 10; the results are shown in Table 2.
[0068] Embodiment 23-25:
[0069] The preparation of the UV curing coating is described in reference to Example 10, except that the silica matting powder XG-1 used in step (1) is replaced by XG-6, and the amount of XG-6 is changed to 0 g, 2 g and 10 g respectively; the zinc oxide particles used in step (2) are replaced by a mixed powder composed of magnesium oxide particles and zinc oxide particles, wherein the amount of magnesium oxide particles is 0.6 g and the amount of zinc oxide particles is 0.4 g; the remaining steps are the same as in Example 10, and the preparation and performance characterization of the obtained coating are the same as in Example 10; the results are shown in Table 2.
[0070] Table 2 Effect of different oxide particles on the performance of UV curing coatings
[0071] Example Curing time hardness Peel strength Water resistance Salt tolerance Glossiness Antibacterial rate 19 52s 5H 9.46 144h 144h 82.5% 11.0% 20 42s 6H 9.71 192h 192h 71.8% 40.5% 21 43s 6H 9.60 168h 168h 71.3% 11.7% 22 23s 6H 9.67 192h 192h 22.9% 89.4% 23 84s 4H 9.32 192h 172h 89.2% 88.3% 24 31s 6H 9.62 192h 192h 36.7% 88.6% 25 20s 6H 9.68 192h 192h 18.4% 90.1%
[0072] Note: The antibacterial rate refers to the antibacterial rate against Staphylococcus aureus; water resistance and salt resistance both refer to the time without change.
Claims
1. A method for preparing a silicon dioxide matting powder, characterized in that: The specific steps include: (1) adding a template into a mixed solvent, and then adding an alkaline solution to prepare a mixed solution; (2) adding calcium carbonate microspheres to the mixed solution obtained in step (1), and after uniform dispersion, adding an alkaline solution to the resulting mixture to adjust the pH value of the system to obtain a dispersion containing calcium carbonate microspheres; (3) adding organic silicate to the dispersion containing calcium carbonate microspheres obtained in step (2), stirring evenly to obtain silica gel; then transferring the obtained silica gel to a microwave reaction tank for microwave reaction to age the silica gel; (4) The product obtained in step (3) is cooled and filtered, the solid obtained is washed with ethanol / water until neutral and then dried, and the dried solid is made into powder and then calcined.
2. The method for preparing the silicon dioxide matting powder according to claim 1, characterized in that: The template agent described in step (1) is one of sodium dodecyl sulfonate, dodecyltrimethylammonium chloride or dodecyltrimethylammonium bromide.
3. The method for preparing the silicon dioxide matting powder according to claim 1, characterized in that: The mixed solvent described in step (1) is a mixture of ethanol and water; the alkaline solution is one of ammonia solution, sodium hydroxide solution or potassium hydroxide solution.
4. The method for preparing the silicon dioxide matting powder according to claim 1, characterized in that: The alkaline solution in step (2) is one of a sodium hydroxide solution or a potassium hydroxide solution; and the pH value range is 9-12.
5. The method for preparing the silicon dioxide matting powder according to claim 1, characterized in that: The organic silicate described in step (3) is one of ethyl orthosilicate or isopropyl orthosilicate.
6. The method for preparing the silicon dioxide matting powder according to claim 1, characterized in that: The microwave reaction conditions in step (3) are as follows: microwave power is 250-300 W, microwave reaction temperature is 80-100° C., and microwave reaction time is 1-2 h.
7. The method for preparing the silicon dioxide matting powder according to claim 1, characterized in that: The calcination conditions described in step (4) are: calcination temperature is 800-1100° C., and calcination time is 6-10 h.
8. The matting powder prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The matting powder is composed of silicon dioxide powder; the specific surface area of the matting powder is 150 to 300 m 2 / g, the pore volume is 1.0~2.2mL / g, and the average particle size is 1~15μm.
9. A method for preparing the silicon dioxide matting powder according to claims 1 to 7 or use of the matting powder according to claim 8 in UV curing coatings.