High-transparency scratch-resistant antistatic coating and preparation method thereof
By combining silsesquioxane monomers containing fluoride ions with functional monomers, the problem of integrating high transparency, scratch resistance, and antistatic functions on touch screen surfaces has been solved, enabling simplified preparation and the application of multifunctional coatings suitable for touch screens and optical products.
Patent Information
- Application Number
- CN202310482795.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-03
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-03
AI Technical Summary
Existing technologies struggle to effectively integrate high transparency, scratch resistance, and antistatic properties on touchscreen surfaces. Traditional multi-layer structures are complex and costly, making it difficult to meet the application requirements of flexible wearable devices.
By combining silsesquioxane monomers containing fluoride ions with functional monomers and catalysts, and through rational structural design, the resistivity and hardness of the coating are adjusted to form a highly transparent, scratch-resistant, and antistatic coating.
It achieves simplified preparation of highly transparent, scratch-resistant, and antistatic coatings, and has multiple functions such as rapid electrostatic release, antibacterial properties, and dynamic scratch repair, making it suitable for touch screens and other optical products.
Smart Images

Figure CN118895075A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of advanced coatings and their preparation, and specifically relates to a highly transparent, scratch-resistant, multifunctional antistatic coating and a preparation method thereof. Background Art
[0002] With the advent of the Internet of Things era, touch screens are the main way of human-computer interaction, and their application scenarios are expanding. In the 3C (computer, communication, consumer electronics) market, capacitive touch screens have become mainstream due to their high sensitivity, support for multi-touch, and excellent anti-interference. However, in actual use, frequent contact and friction between the human body and clothing and the screen of electronic products will generate static electricity, which may cause problems such as false touches, freezes, and freezes during use of the touch screen. At the same time, excessive accumulated static electricity may damage important electronic components during rapid release, resulting in screen noise or even permanent black spots. Therefore, it is very necessary to design a layer of antistatic, highly transparent coating material on the surface of the touch screen product for the normal use of the touch screen. In addition, in order to prevent the surface of the touch screen from being scratched by foreign objects, the coating also needs to have a high hardness. In specific application scenarios, the coating must also have functions such as anti-fingerprint, antibacterial, dynamic scratch repair, high refractive index and flexibility, so as to solve problems such as rough touch and insensitive touch caused by fingerprint dust, bacteria breeding, scratches and impacts during use, thereby improving the user experience.
[0003] Most commercial touch screens currently use low-resistivity ITO (indium tin oxide) as the antistatic layer material of the touch screen. However, the strict requirements and complex processes of the vapor deposition or sputtering deposition methods used in the processing of the ITO layer, as well as the brittleness of ITO itself, make its practical application, especially in future foldable and flexible wearable devices, extremely limited. In addition, traditional multifunctional coatings integrate single-functional coating materials by accumulating them. For example, in the touch screen, the multilayer structure composed of the ITO layer, the hardening layer, the anti-fingerprint layer and other functional layers can simultaneously achieve antistatic, scratch resistance, anti-fingerprint and other necessary functions. This method is not only complex in process, but also increases the difficulty and cost of production. It is also difficult to regulate the interface compatibility of the multilayer structure and the balance of multiple functions, which greatly increases the complexity and difficulty of coating preparation. In addition, although there are academically highly transparent and antistatic (surface resistivity 1.2×10 12 Ω / sq) coatings (ACS Appl. Mater. Interfaces 2021, 13, 10301-10312), but it is still difficult to integrate high transparency, scratch resistance and antistatic functions at the same time, and it is even more difficult to integrate more functions. Therefore, if only one layer of coating with various properties is applied to the substrate, the production process can be simplified, greatly reducing the cost and difficulty. Summary of the invention
[0004] The current coating process is difficult to break through the shackles of integrating multiple functions into a small amount or even a single coating, mainly because there is a lack of simple and efficient methods to regulate the balance between the resistivity and hardness of transparent materials. Therefore, how to achieve an effective combination of resistivity and multi-functions through reasonable structural design and special building units has become the key to the multifunctionalization of highly transparent antistatic coatings.
[0005] In view of the above shortcomings, the present invention provides a highly transparent, scratch-resistant and antistatic coating, the light transmittance of the obtained coating is greater than 98% (550nm); the surface pencil hardness is greater than 9H, and no scratches are produced after rubbing with steel wool for more than 1000 times; the surface resistivity is about 10 8 ~10 9 Ω / sq, fast static discharge rate.
[0006] The technical solution of the present invention:
[0007] The first technical problem to be solved by the present invention is to provide a highly transparent and scratch-resistant antistatic coating, wherein the raw materials of the antistatic coating include a silsesquioxane monomer containing fluoride ions, a functional monomer and a catalyst; wherein the functional monomer is a crosslinking agent or an anti-crystallization agent.
[0008] Furthermore, the fluorine-containing silsesquioxane monomer is divided into two categories according to whether it contains reactive groups, and its structure is at least one of the following structural formulas:
[0009]
[0010] in, or k + At least one of the following; At least one of the reactive groups;
[0011] or At least one of the non-reactive groups.
[0012] Preferably, the R is vinyl Styrene Phenyl or trifluoropropyl
[0013] Preferably, the X + Tetrabutylammonium
[0014] Furthermore, the functional monomer accounts for 5 to 20% of the molar amount of the silsesquioxane monomer containing fluoride ions.
[0015] Furthermore, the catalyst accounts for 0.5-5% of the molar amount of the silsesquioxane monomer containing fluoride ions.
[0016] Furthermore, when the R group of the silsesquioxane monomer containing fluorine ions is a reactive group, the functional monomer is selected from a multifunctional crosslinking agent.
[0017] Furthermore, the multifunctional crosslinking agent includes at least one of multifunctional olefins, multifunctional thiols, multifunctional epoxides, multifunctional silanes or multifunctional siloxanes.
[0018] Preferably, the multifunctional olefin is selected from: a cross-linking agent in which the total number of vinyl groups / acrylate groups / methacrylate groups in a single molecule is greater than 1, such as neopentyl glycol diacrylate, trimethylolpropane triacrylate, etc.;
[0019] The multifunctional thiol is selected from: a cross-linking agent having a single molecule thiol group number greater than 1, such as tris(3-mercaptopropionic acid) trimethylolpropane ester, tetrakis(3-mercaptopropionic acid) pentaerythritol ester, etc.;
[0020] The multifunctional epoxide is selected from: a cross-linking agent having a single molecule epoxy group number greater than 1, such as 1,2,5,6-diepoxyhexane, 4-vinyl-1-cyclohexene diepoxide, etc.;
[0021] The multifunctional silane or siloxane includes: linear, cyclic, random network, ladder siloxane, and its general structural formula is Where R1 or Reactive groups such as The caged silsesquioxane T wherein the peripheral groups are vinyl, styryl, mercaptopropyl, acrylate and methacrylate n (n=8, 10, 12) etc.
[0022] Furthermore, when the R group of the silsesquioxane monomer containing fluorine ions is a non-reactive group, the functional monomer is selected from anticrystallization agents.
[0023] Furthermore, the anti-crystallization agent includes at least one of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, hexaethylcyclotrisiloxane, octaethylcyclotetrasiloxane, trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane, hexaphenylcyclotrisiloxane, octaphenylcyclotetrasiloxane, trifluoropropylmethylcyclotrisiloxane, trivinyltrimethylcyclotrisiloxane, tetravinyltetramethylcyclotetrasiloxane, etc.
[0024] Further, the catalyst comprises:
[0025] The catalyst used in combination with the crosslinking agent is at least one of azobisisobutyronitrile, azobisisobutyramidine hydrochloride, azobisisopropylimidazoline hydrochloride, dibenzoyl peroxide, tert-butyl perbenzoate, methyl ethyl ketone peroxide or pyridine;
[0026] The catalyst used in combination with the anti-crystallization agent is at least one of tetramethylammonium hydroxide, tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride, tetrabutylammonium fluoride and the like.
[0027] Furthermore, when the R group of the fluorine-containing silsesquioxane monomer is a reactive group, the reactions that can occur between it and the crosslinking agent include: mercapto-olefin reaction, free radical polymerization reaction, ring-opening reaction and hydrolysis condensation reaction of siloxane.
[0028] Furthermore, when the R group of the fluorine-containing silsesquioxane monomer is a non-reactive group, it can undergo a silicon-oxygen bond rearrangement reaction with an anti-crystallization agent.
[0029] Preferably, when R of the fluorine-containing silsesquioxane monomer is a vinyl group or a styrene group, the crosslinking agent is selected from the group consisting of multifunctional olefins and multifunctional epoxides.
[0030] Preferably, when R of the silsesquioxane monomer containing fluorine ions is trifluoropropyl or phenyl, the anti-crystallization agent is octamethylcyclotetrasiloxane or tetramethyltetraphenylcyclotetrasiloxane.
[0031] Furthermore, the fluoride-containing silsesquioxane monomer is prepared by the following preparation method: a POSS precursor and an anhydrous ion pair donor are added to a solvent I at a molar ratio of 1:0.5 to 1.2, and stirred for 16 to 24 hours, and the turbid suspension becomes translucent after standing, and the suspension is concentrated and filtered, and the solvent is removed under vacuum, and the fluoride-containing silsesquioxane monomer is obtained after drying;
[0032] Wherein, the POSS precursor is divided into two categories according to whether it contains reactive groups, and its structure is at least one of the following structural formulas:
[0033]
[0034] in
[0035] At least one of the reactive groups
[0036] or: At least one of the non-reactive groups.
[0037] Furthermore, in the method for preparing the fluoride-containing silsesquioxane monomer, the ion pair donor includes any one of tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride, tetrabutylammonium fluoride or potassium fluoride.
[0038] Furthermore, in the above-mentioned method for preparing the fluoride-containing silsesquioxane monomer, the solvent I is at least one of tetrahydrofuran, chloroform, toluene, acetone, dichloromethane, xylene, methanol, ethanol, ethylene glycol, ethyl acetate, dioxane, dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide.
[0039] The second technical problem to be solved by the present invention is to provide a method for preparing the above-mentioned highly transparent and scratch-resistant antistatic coating, wherein the preparation method comprises: firstly mixing the raw materials to obtain a coating composition, and then uniformly coating the coating composition on the surface of the substrate to form the antistatic coating.
[0040] Furthermore, the method for preparing the coating composition from the raw materials is one of the following methods:
[0041] Method 1: adding a fluoride-containing silsesquioxane monomer and a functional monomer into solvent II and stirring until dissolved, and then adding a catalyst to prepare a coating composition; wherein the functional monomer is a crosslinking agent;
[0042] Method 2: adding fluoride-containing silsesquioxane monomers, functional monomers and catalysts into solvent II and stirring until dissolved, washing and concentrating with solvent III to obtain a coating composition; wherein the functional monomer is an anti-crystallization agent.
[0043] Furthermore, the solvent II is at least one of tetrahydrofuran, chloroform, toluene, acetone, dichloromethane, xylene, methanol, ethanol, ethylene glycol, ethyl acetate, dioxane, dimethyl sulfoxide, N,N-dimethylformamide, and N,N-dimethylacetamide; the solvent III is at least one of methanol, ethanol, acetonitrile, toluene, xylene, acetone, dioxane, and deionized water.
[0044] Furthermore, the material of the substrate is selected from at least one of glass, polyethylene terephthalate, polyimide, polycarbonate or polymethyl methacrylate.
[0045] Furthermore, the coating composition is uniformly coated on the substrate by any of drop coating, spin coating, rod coating, blade coating or spray coating.
[0046] Furthermore, the method of uniformly coating the coating composition on the surface of a substrate to form the antistatic coating is: uniformly coating the coating composition on the substrate, and after the solvent evaporates, heat treatment and washing are performed to obtain the antistatic coating.
[0047] Furthermore, the heat treatment refers to curing at 50 to 200° C. for 1 second to 120 minutes.
[0048] Furthermore, the thickness of the obtained antistatic coating is 5 nm to 500 μm, preferably 100 nm to 300 μm.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] Since the present invention selects an ion pair donor that has a specific effect on siloxane, it can effectively solve the difficulties and conflicts brought about by the multilayer structure used in traditional functional coatings to achieve multifunctional integration for the balance of overall performance, and further give it more performance through the selection of appropriate functional monomers.
[0051] Since the coating provided by the present invention uses a silsesquioxane monomer containing fluoride ions, the silsesquioxane is combined with an ion pair donor, so the resistivity of such coating is simply and efficiently adjusted. More importantly, under the action of the ion pair donor, it can also be endowed with antibacterial and dynamic scratch repair functions.
[0052] Since the coating provided by the present invention introduces special functional monomers, it can be endowed with unique antistatic properties while ensuring high transparency. Different types of functional monomers can be selected to achieve functional customization of highly transparent and scratch-resistant antistatic coatings, such as anti-oil, anti-fingerprint, flexibility, high refractive index, etc., to promote the diversified development of the touch display field.
[0053] Since the functional monomers used in the coating provided by the present invention are of various types, the cross-linked network can be constructed or rearranged in various ways by selecting functional monomers of different types, structures and functionalities for silsesquioxane monomers containing fluoride ions; and by changing the relative content of the functional monomers, the mechanical properties of the coating can be effectively regulated in a wider range to meet the application requirements in various scenarios.
[0054] Since the silsesquioxane monomer containing fluoride ions used in the coating provided by the present invention is composed of an inorganic silicon-oxygen core and an organic group outside the core, it brings the characteristics of nanometer size and organic-inorganic hybrid structure, and can give the coating excellent optical and mechanical properties at the molecular scale and through reasonable structural design.
[0055] Since the raw materials used in the functional coating provided by the present invention are all commercially available, the monomers are easy to prepare, and the coating can be obtained by simply mixing various raw materials, coating and curing. This is simple, easy, time-saving and easy to prepare on a large scale.
[0056] At the same time, the present invention also has strong scalability, and the coating can also be applied to the surface of optical products such as computer screens, optical lenses, and precision optical components. While meeting the functions of protection, it can effectively prevent dust adsorbed by static electricity on the surface from affecting normal use. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 The T8V8 (T8V8@F) prepared from three different sizes of vinyl POSS as precursors in Examples 1 to 3 of the present invention - ), T 10 V 10 (T 10 V 10 @F - ) and T 12 V 12 (T 12 V 12 @F - ) infrared spectrum; 3100-2800cm -1 The alkyl peak appears at 1120 cm -1 The nearby Si-O-Si peak proves that the silsesquioxane monomer containing fluoride ions was successfully prepared.
[0058] Figure 2 Schematic diagram of preparing a highly transparent and scratch-resistant functional customized antistatic coating according to an embodiment of the present invention; first, a silsesquioxane monomer containing fluoride ions, a cross-linking agent or an anti-crystallization agent, a catalyst and a solvent are mixed to form a coating, and the target coating can be obtained after coating and curing.
[0059] Figure 3 For ordinary glass cover ( Figure 3 A) and the highly transparent and scratch-resistant functional customized antistatic coating prepared by the present invention ( Figure 3 B, taking Example 8 as an example), in the electrostatic dissipation experiment, the surface static charge generated by the electrostatic gun is still not completely dissipated after 30 minutes, while the coating prepared by the present invention can dissipate the static charge in a very short time, proving that the coating has an excellent antistatic effect.
[0060] Figure 4 The UV-visible light transmittance of the highly transparent and scratch-resistant customized antistatic coating prepared in Examples 8 to 13 of the present invention; Figure 4 It can be seen that the transmittance of the coatings in Examples 8 to 13 of the present invention is greater than 98% (wavelength is 550 nm), which proves that the coatings prepared by the present invention have high transmittance.
[0061] Figure 5 A is a scratch resistance test device, the steel wool used is #0000 grade, and the calculated average vertical pressure is about 27.9 kPa; Figure 5B and 5D are SEM electron microscope images and optical microscope images of PET after only one wear; Figure 5 C and 5E are SEM electron microscope images and optical microscope images of Example 8 of the present invention after being scratched 1000 times.
[0062] Figure 6 The antibacterial experimental effect of the highly transparent and scratch-resistant customized antistatic coating prepared in Example 8 of the present invention shows that Escherichia coli and Staphylococcus aureus on the surface of the glass cover can grow normally, while there is almost no bacterial growth on the surface of the coating of Example 8; Figure 6 It can be seen that the functionalized coating prepared in Example 8 of the present invention has an excellent antibacterial effect.
[0063] Figure 7 The dynamic repair experiment effect of the highly transparent and scratch-resistant customized antistatic coating prepared in Example 8 of the present invention is shown. The figure shows the scratches on the coating surface of Example 8 before and after water vapor treatment at 50°C and 90% humidity; Figure 7 It can be seen that the scratches on the coating disappeared after the water vapor treatment, proving that this type of coating has excellent dynamic scratch repair performance.
[0064] Figure 8 A bending test was conducted on the double-layer composite material of the highly transparent and scratch-resistant functional customized antistatic coating and PET film prepared in Example 10 of the present invention. The coating prepared in Example 10 still did not show any cracks when the bending radius of curvature was 1 mm, indicating that the customized coating material in Example 10 of the present invention has excellent flexibility.
[0065] Fig. 9 The refractive index of the highly transparent and scratch-resistant customized antistatic coating prepared in Example 12 of the present invention; Fig. 9 It can be seen that the refractive index of the coating prepared in Example 12 is greater than 1.68 (589 nm), indicating that the coating material customized in Example 12 of the present invention has a higher refractive index.
[0066] Fig.10 A is the water contact angle of the highly transparent and scratch-resistant customized antistatic coating prepared in Example 13 of the present invention; Fig.10 B is the anti-oil effect demonstration; Fig.10 It can be seen that: the water contact angle of the coating is greater than 105°; the marker marks on the glass cover are not easy to remove, while the marks on the coating surface are easy to clean, indicating that the coating customized in Example 13 of the present invention has excellent hydrophobic and oil-resistant properties. DETAILED DESCRIPTION
[0067] The present invention uses silsesquioxane monomers containing fluorine ions, wherein the silsesquioxane structure brings excellent characteristics of nano size and organic-inorganic hybrid structure; the silsesquioxane is combined with an ionic pair donor to adjust the resistivity of the coating, and can also give it antibacterial, dynamic scratch repair and other functions; the introduction of functional monomers breaks the regularity of the overall network, avoids its crystallization, achieves high transparency, creates conditions for the practical application of the coating, and provides the coating with more selectable properties. The combination of multiple functional components ultimately produces a highly transparent, scratch-resistant, antistatic multifunctional coating.
[0068] The present invention is further described below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and are not to be construed as limiting the scope of protection of the present invention. Those skilled in the art may make some non-essential improvements and adjustments to the present invention based on the above-mentioned contents of the present invention.
[0069] The present invention provides a method for preparing a highly transparent and scratch-resistant customized antistatic coating, the preparation process steps and conditions of the method are as follows:
[0070] (1) Preparation of silsesquioxane monomers containing fluoride ions:
[0071] The POSS precursor and the anhydrous ion pair donor are added to the solvent I at a molar ratio of 1:0.5-1.2, and stirred for 16-24 hours. The turbid suspension becomes translucent after standing. The suspension is concentrated and filtered, and the solvent is removed under vacuum. After drying, a silsesquioxane monomer containing fluoride ions is obtained.
[0072] (2) Preparation of coating composition:
[0073] Method 1: adding a fluoride-containing silsesquioxane monomer and a crosslinking agent accounting for 5 to 20% of the molar amount of the fluoride-containing silsesquioxane monomer to solvent II and stirring until dissolved, and then adding a catalyst accounting for 0.5 to 5% of the molar amount of the fluoride-containing silsesquioxane monomer to obtain a coating composition;
[0074] Method 2: adding a fluoride-containing silsesquioxane monomer, an anti-crystallization agent accounting for 5-20% of the molar amount of the fluoride-containing silsesquioxane monomer, and a catalyst in a molar amount of 0.5-5% to a solvent II, stirring until dissolved, washing and concentrating with a solvent III to obtain a coating composition;
[0075] (3) The obtained coating composition is uniformly coated on the surface of the substrate by any one of drop coating, spin coating, rod coating, scraping coating and spraying; the coating thickness is 5 nm to 500 μm, preferably 100 nm to 300 μm; after heat treatment (50 to 200° C.), the surface is cleaned with solvent IV to obtain the highly transparent and scratch-resistant functional customized antistatic coating.
[0076] It is worth noting that 1) the ratio of the precursor of the fluoride-containing silsesquioxane monomer and the ion pair donor in the following examples, and the ratio of the fluoride-containing silsesquioxane monomer, the functional monomer and the catalyst are all molar ratios; 2) the ultraviolet-visible light transmittance of the highly transparent and scratch-resistant functional customized antistatic coating obtained in the following examples was tested by UV-3600 of Shimadzu Corporation of Japan; the pencil hardness was tested by H501 pencil hardness tester of Elecometer of the United Kingdom; the surface resistivity was tested by RTS-8 four-probe tester; the flexibility was tested by a spiral micrometer; and the refractive index was tested by Metricon MODEL 2010 / M prism coupler of the United States.
[0077] Example 1 Preparation of silsesquioxane monomer containing fluoride ions
[0078] Octavidin caged silsesquioxane (T8V8, 5 mmol) was added to anhydrous tetrahydrofuran and stirred at room temperature until the monomer was completely dissolved. Then, tetrabutylammonium fluoride trihydrate (TBAF, 5 mmol) was dissolved in 50 mL of anhydrous tetrahydrofuran. The two solutions were mixed and stirred at room temperature for 16 hours to obtain a turbid suspension, which became translucent after standing for a period of time. The solvent was removed in vacuo and dried to obtain the final product, T8V8 containing fluoride ions (T8V8@F - ) molecules with a yield of 79%.
[0079] Example 2 Preparation of silsesquioxane monomer containing fluoride ions
[0080] Decavidin cage silsesquioxane (T 10 V 10 , 5mmol) was added to anhydrous tetrahydrofuran and stirred at room temperature until the monomer was completely dissolved, then tetrabutylammonium fluoride trihydrate (TBAF, 5mmol) was dissolved in 50mL anhydrous tetrahydrofuran, and then the two solutions were mixed and stirred at room temperature for 16 hours to obtain a turbid suspension, which became translucent after standing for a period of time, and the solvent was removed in vacuo, and the final product, T containing fluoride ions, was obtained after drying. 10 V 10 (T 10 V 10 @F - ) molecules with a yield of 72%.
[0081] Example 3 Preparation of silsesquioxane monomer containing fluoride ions
[0082] Dodecavinyl cage silsesquioxane (T 12 V 12, 5mmol) was added to anhydrous tetrahydrofuran and stirred at room temperature until the monomer was completely dissolved, then tetrabutylammonium fluoride trihydrate (TBAF, 5mmol) was dissolved in 50mL anhydrous tetrahydrofuran, and then the two solutions were mixed and stirred at room temperature for 16 hours to obtain a turbid suspension, which became translucent after standing for a period of time, and the solvent was removed in vacuo, and the final product, T containing fluoride ions, was obtained after drying. 12 V 12 (T 12 V 12 @F - ) molecules with a yield of 64%.
[0083] Example 4 Preparation of fluoride-containing silsesquioxane monomers
[0084] Octavidin caged silsesquioxane (T8V8, 5 mmol) was added to anhydrous tetrahydrofuran and stirred at room temperature until the monomer was completely dissolved. Then, tetrabutylammonium fluoride trihydrate (TBAF, 4 mmol) was dissolved in 50 mL of anhydrous tetrahydrofuran. The two solutions were mixed and stirred at room temperature for 16 hours to obtain a turbid suspension, which became translucent after standing for a period of time. The solvent was removed in vacuo and dried to obtain the final product, T8V8 containing fluoride ions (T8V8@F - ) molecules with a yield of 66%.
[0085] Example 5 Preparation of silsesquioxane monomer containing fluoride ions
[0086] Octavidin caged silsesquioxane (T8V8, 5 mmol) was added to anhydrous tetrahydrofuran and stirred at room temperature until the monomer was completely dissolved. Then, tetrabutylammonium fluoride trihydrate (TBAF, 6 mmol) was dissolved in 50 mL of anhydrous tetrahydrofuran. The two solutions were mixed and stirred at room temperature for 16 hours to obtain a turbid suspension, which became translucent after standing for a period of time. The solvent was removed in vacuo and dried to obtain the final product, T8V8 containing fluoride ions (T8V8@F - ) molecules with a yield of 70%.
[0087] Example 6 Preparation of silsesquioxane monomer containing fluoride ions
[0088] Octavidinyl caged silsesquioxane (SPOSS, 5 mmol) was added to anhydrous tetrahydrofuran and stirred at room temperature until the monomer was completely dissolved. Then, tetrabutylammonium fluoride trihydrate (TBAF, 5 mmol) was dissolved in 50 mL of anhydrous tetrahydrofuran. The two solutions were mixed and stirred at room temperature for 16 hours to obtain a turbid suspension, which became translucent after standing for a period of time. The solvent was removed in vacuo and dried to obtain the final product, SPOSS (SPOSS@F - ) molecules with a yield of 82%.
[0089] Example 7 Preparation of silsesquioxane monomer containing fluoride ions
[0090] Octatrifluoropropyl caged silsesquioxane (FPOSS, 5 mmol) was added to anhydrous tetrahydrofuran and stirred at room temperature until the monomer was completely dissolved. Then, tetrabutylammonium fluoride trihydrate (TBAF, 5 mmol) equivalent to FPOSS was dissolved in 50 mL of anhydrous tetrahydrofuran. The two solutions were mixed and stirred at room temperature for 16 hours to obtain a turbid suspension, which became translucent after standing for a period of time. The solvent was removed in vacuo and dried to obtain the final product - FPOSS with tetrabutylammonium as the peripheral cation and fluoride ion as the internal cation (FPOSS@F - ) molecules with a yield of 71%.
[0091] Example 8 Preparation of coating
[0092] The T8V8@F in Example 1 - (0.6mmol) and trimethylolpropane triacrylate (0.1mmol) were added into 20mL tetrahydrofuran and stirred to dissolve at room temperature, and free radical catalyst AIBN (0.03mmol) was added and stirred for five minutes; then the solution was dropwise coated on the substrate, and after the solvent evaporated, it was cured at 70°C for 6 hours, and the coating material was obtained after rinsing with ethanol.
[0093] Example 9
[0094] The T in Example 2 10 V 10 @F - (0.6mmol) and trimethylolpropane triacrylate (0.1mmol) were added into 20mL tetrahydrofuran and stirred to dissolve at room temperature, and free radical catalyst AIBN (0.03mmol) was added and stirred for five minutes; then the solution was dropwise coated on the substrate, and after the solvent evaporated, it was cured at 70°C for 6 hours, and the coating material was obtained after rinsing with ethanol.
[0095] Example 10
[0096] The T8V8@F in Example 1 - (0.6mmol) and neopentyl glycol diacrylate (0.12mmol) were added into 20mL tetrahydrofuran and stirred to dissolve at room temperature, free radical catalyst AIBN (0.03mmol) was added and stirred for five minutes; then the solution was dropwise coated on the substrate, and after the solvent evaporated, it was cured at 70°C for 6 hours, and the coating material was obtained after rinsing with ethanol.
[0097] Embodiment 11
[0098] The SPOSS@F in Example 6 -(0.6mmol) and octamethylcyclotetrasiloxane (0.1mmol) were added to 20mL of tetrahydrofuran and stirred at room temperature to dissolve, and a catalyst tetrabutylammonium fluoride (0.03mmol) was added and stirred for five minutes, and the mixture was washed and concentrated in acetonitrile; the solution was then dropwise coated on the substrate, and after the solvent evaporated, it was cured at 70°C for 6 hours, and the coating material was obtained by washing with ethanol.
[0099] Example 12
[0100] The SPOSS@F in Example 6 - (0.6mmol) and tetramethyltetraphenylcyclotetrasiloxane (0.1mmol) were added to 20mL of tetrahydrofuran and dissolved under stirring at room temperature, and a catalyst of tetrabutylammonium fluoride (0.03mmol) was added and stirred for five minutes, and the mixture was washed and concentrated in acetonitrile; the solution was then drop-coated on the substrate, and after the solvent evaporated, it was cured at 50°C for 5h, and the coating material was obtained after rinsing with ethanol.
[0101] Example 13
[0102] The FPOSS@F in Example 7 - (0.6mmol) and trifluoropropylmethylcyclotrisiloxane (0.1mmol) were added to 20mL of tetrahydrofuran and dissolved under stirring at room temperature, and a catalyst tetrabutylammonium fluoride (0.03mmol) was added and stirred for five minutes, and the mixture was washed and concentrated in acetonitrile; the solution was then drop-coated on the substrate, and after the solvent evaporated, it was cured at 50°C for 5h, and the coating material was obtained by washing with ethanol.
[0103] Comparative Example 1
[0104] The T8V8@F in Example 1 - (0.6mmol) was added with 20mL tetrahydrofuran and stirred at room temperature to dissolve, and free radical catalyst AIBN (0.03mmol) was added and stirred for five minutes; the solution was then dropwise coated on the substrate, and after the solvent evaporated, it was cured at 70°C for 6 hours, and the coating material was obtained after rinsing with ethanol.
[0105] Comparative Example 2
[0106] The SPOSS@F in Example 6 - (0.6mmol) was added with 20mL of tetrahydrofuran and dissolved under stirring at room temperature, and a catalyst of tetrabutylammonium fluoride (0.03mmol) was added, stirred for five minutes, and washed and concentrated in acetonitrile; the solution was then dropwise coated on the substrate, and after the solvent evaporated, it was cured at 50°C for 5h, and the coating material was obtained after rinsing with ethanol.
[0107] Table 2 summarizes the effective modulus, hardness, H / E of Examples 8 to 13 of the present invention. *Value, pencil hardness, transmittance, surface resistivity, tribostatic voltage, scratch repair ability, antibacterial ability, anti-oil ability, anti-fingerprint ability, bending curvature radius and 1000 times steel wool scratch test. Among them, the effective modulus and hardness obtained by the nanoindentation experiment, Examples 8 to 13 of the present invention all have high hardness, while Example 10 of the present invention has a low effective modulus, H / E * The value is 0.17, which has excellent flexibility; in the pencil hardness test, the pencil hardness of the coatings in Examples 8 to 12 of the present invention is greater than 9H, and that in Example 13 of the present invention is 8H, and these coatings have excellent scratch resistance; in the transmittance test, the transmittance of the coatings in Examples 8 to 13 of the present invention at a wavelength of 550nm is greater than 98%, and all have high transmittance; the surface resistivity of the coatings in Examples 10 to 13 of the present invention is greater than 10 8 ~10 9 Ω / sq range, having excellent antistatic performance; the surface static voltage measured by rubbing the coating surface with a copper rod 200 times, the absolute value of the instantaneous surface static voltage of the coatings of Examples 9-13 of the present invention is less than 50V, indicating that Examples 9-13 of the present invention have excellent antistatic effects, among which the static voltage of Example 8 of the present invention is greater than 50V, and the static voltage of Example 13 of the present invention is negative. In Comparative Examples 1-2, the obtained coating will precipitate white crystals during curing, with poor transparency, and is not suitable for practical applications.
[0108] Table 1 Raw materials of Examples 8 to 13
[0109]
[0110] Table 2 Performance results of the coatings obtained in Examples 8 to 13
[0111]
Claims
1. A highly transparent, scratch-resistant, antistatic coating. It is characterized in that The raw materials of the antistatic coating include: silsesquioxane monomer containing fluorine ions, functional monomer and catalyst; wherein the functional monomer is a crosslinking agent or an anti-crystallization agent.
2. A highly transparent, scratch-resistant antistatic coating according to claim 1, It is characterized in that The silsesquioxane monomer containing fluoride ions is selected from at least one of the substances represented by the following structural formulas: in, or at least one of the following; at least one of the reactive groups; or: At least one of the non-reactive groups.
3. A highly transparent, scratch-resistant antistatic coating according to claim 2, It is characterized in that The R is The X + for 4. A highly transparent, scratch-resistant antistatic coating according to any one of claims 1 to 3, It is characterized in that The functional monomer accounts for 5 to 20% of the molar amount of the silsesquioxane monomer containing fluoride ions; or: The catalyst accounts for 0.5-5% of the molar amount of the silsesquioxane monomer containing fluoride ions.
5. A highly transparent, scratch-resistant antistatic coating according to any one of claims 1 to 4, It is characterized in that When R of the silsesquioxane monomer containing fluorine ions is a reactive group, the functional monomer is a multifunctional crosslinking agent; or: When R of the silsesquioxane monomer containing fluoride ions is a non-reactive group, the functional monomer is an anti-crystallization agent; Further, the catalyst is selected from: When the functional monomer is a multifunctional crosslinking agent, the catalyst is at least one of azobisisobutyronitrile, azobisisobutyramidine hydrochloride, azobisisopropylimidazoline hydrochloride, dibenzoyl peroxide, tert-butyl perbenzoate, methyl ethyl ketone peroxide or pyridine; When the functional monomer is an anti-crystallization agent, the catalyst is at least one of tetramethylammonium hydroxide, tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride, tetrabutylammonium fluoride and the like.
6. A highly transparent, scratch-resistant antistatic coating according to claim 5, It is characterized in that The multifunctional crosslinking agent includes: at least one of multifunctional olefins, multifunctional thiols, multifunctional epoxides, multifunctional silanes or multifunctional siloxanes; or: The anti-crystallization agent comprises at least one of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, hexaethylcyclotrisiloxane, octaethylcyclotetrasiloxane, trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane, hexaphenylcyclotrisiloxane, octaphenylcyclotetrasiloxane, trifluoropropylmethylcyclotrisiloxane, trivinyltrimethylcyclotrisiloxane and tetravinyltetramethylcyclotetrasiloxane; Further, the multifunctional olefin is selected from: neopentyl glycol diacrylate or trimethylolpropane triacrylate; The multifunctional thiol is selected from: tris(3-mercaptopropionic acid) trimethylolpropane ester or pentaerythritol tetrakis(3-mercaptopropionic acid); The multifunctional epoxide is selected from: 1,2,5,6-diepoxyhexane or 4-vinyl-1-cyclohexene diepoxide; The multifunctional silane or siloxane includes: linear, cyclic, random network, ladder siloxane, and its general structural formula is: Where R 1 or Reactive groups, or One of the non-reactive groups, and a caged silsesquioxane T having a peripheral group of vinyl, styrene, mercaptopropyl, acrylate and methacrylate n , n=8, 10 or 12.
7. A highly transparent, scratch-resistant antistatic coating according to claim 6, It is characterized in that When R of the fluorine-ion-containing silsesquioxane monomer is a vinyl group or a styrene group, the crosslinking agent is selected from the group consisting of multifunctional olefins and multifunctional epoxides. When R of the silsesquioxane monomer containing fluorine ions is trifluoropropyl or phenyl, the anti-crystallization agent is octamethylcyclotetrasiloxane or tetramethyltetraphenylcyclotetrasiloxane.
8. A highly transparent, scratch-resistant antistatic coating according to any one of claims 1 to 7, It is characterized in that The fluoride-containing silsesquioxane monomer is prepared by the following preparation method: a POSS precursor and an ion pair donor are added to a solvent I at a molar ratio of 1:0.5-1.2, and stirred for 16-24 hours to obtain a suspension, wherein the turbid suspension becomes translucent after standing, and then the suspension is concentrated and filtered, and the solvent is removed under vacuum, and finally dried to obtain the fluoride-containing silsesquioxane monomer; Wherein, the POSS precursor is selected from at least one substance shown in the following structural formula: in At least one of the reactive groups, or: at least one of the non-reactive groups; Further, the ion pair donor is selected from any one of tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride, tetrabutylammonium fluoride or potassium fluoride; Furthermore, the solvent I is at least one of tetrahydrofuran, chloroform, toluene, acetone, dichloromethane, xylene, methanol, ethanol, ethylene glycol, ethyl acetate, dioxane, dimethyl sulfoxide, N,N-dimethylformamide or N,N-dimethylacetamide.
9. A method for preparing the highly transparent, scratch-resistant antistatic coating according to any one of claims 1 to 8, It is characterized in that The preparation method comprises the following steps: firstly, mixing various raw materials to obtain a coating composition, and then uniformly coating the coating composition on the surface of a substrate to form the antistatic coating.
10. The method for preparing the highly transparent and scratch-resistant antistatic coating according to claim 9, It is characterized in that The method for preparing the coating composition from the raw materials is one of the following methods: Method 1: adding a fluoride-containing silsesquioxane monomer and a functional monomer into solvent II and stirring until dissolved, and then adding a catalyst to prepare a coating composition; wherein the functional monomer is a crosslinking agent; Method 2: adding fluoride-containing silsesquioxane monomers, functional monomers and catalysts into solvent II and stirring until dissolved, washing and concentrating with solvent III to obtain a coating composition; wherein the functional monomer is an anti-crystallization agent; Further, the solvent II is at least one of tetrahydrofuran, chloroform, toluene, acetone, dichloromethane, xylene, methanol, ethanol, ethylene glycol, ethyl acetate, dioxane, dimethyl sulfoxide, N,N-dimethylformamide, and N,N-dimethylacetamide; the solvent III is at least one of methanol, ethanol, acetonitrile, toluene, xylene, acetone, dioxane, and deionized water; Further, the material of the substrate is selected from at least one of glass, polyethylene terephthalate, polyimide, polycarbonate or polymethyl methacrylate; Furthermore, the coating composition is uniformly coated on the substrate by any of drop coating, spin coating, rod coating, blade coating or spray coating; Furthermore, the method of uniformly coating the coating composition on the surface of a substrate to form the antistatic coating is as follows: uniformly coating the coating composition on the substrate, and after the solvent evaporates, heat-treating and washing to obtain the antistatic coating; Further, the heat treatment refers to: heating and curing at 50 to 200° C. for 1 second to 120 minutes; Furthermore, the thickness of the antistatic coating is 5 nm to 500 μm, preferably 100 nm to 300 μm.
Citation Information
Patent Citations
Coating composite and usage thereof
CN101565573A
Polymer composite material with high dielectric constant and low dielectric loss and preparation method thereof
CN111187461A
High-transparency flexible scratch-resistant coating, functionalized coating and preparation method of high-transparency flexible scratch-resistant coating
CN114479665A
Transparent self-healing omniphobic coatings
EP3167964A1
Properties tailoring in silsesquioxanes
WO2010062695A2
Cited By
Coating composition, antistatic protective coating and preparation method
CN119307180A