Spray-seeding material for mine repair and construction method of spray-seeding material

By using mine repair spray-piercing materials composed of composite fibers and optimized water retention agents, the problem of spray-piercing materials falling under heavy rain and high slopes in the prior art is solved, and soil moisture content and plant coverage are improved, thus achieving more Good mine repair effect.

CN118895148APending Publication Date: 2024-11-05BEIJING JINYU ENERGY-SAVING MATERIALS & TECH +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411022492.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing mine repair spray materials are prone to falling off when rainstorms or slopes exceed 75°, resulting in poor mine repair results.

Method used

Spray-sowed materials consisting of composite fibers, grass fibers, binders, water retention agents, compound fertilizers and seeds, where composite fibers include wood fibers, rock wool fibers and grass soil. By optimizing the preparation method of water retention agent and the mass ratio of fibers , improve soil moisture content and plant coverage, and propose a construction method to spray spray-pierce materials after cleaning the slope and cover non-woven fabrics or coconut silk blankets.

Benefits of technology

It is not easy to fall under heavy rain and high slope conditions, which significantly improves the mine restoration effect, soil moisture content and plant coverage, ensuring the effect of mine restoration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of soil remediation materials, and provides a spray-seeding material for mine remediation and a construction method thereof. The spray-seeding material for mine remediation comprises the following components in parts by mass: 80-100 parts of composite fibers, 40-60 parts of grass fibers, 10-15 parts of a binder, 7-11 parts of a water-retaining agent, 6-10 parts of a compound fertilizer, 8-12 parts of seeds and 20-30 parts of water, the composite fibers comprise wood fibers, rock wool fibers and turfy soil. Through the technical scheme, the problem of poor repairing effect of a mine repairing material in related technologies is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of soil remediation materials, and in particular to a spraying material for mine remediation and a construction method thereof. Background Art

[0002] Mine restoration spraying is an ecological restoration technology that uses spraying materials to repair damaged mines. Mine restoration spraying materials mainly include spraying substrates, water retaining agents, adhesives, grass seeds, etc., which can effectively restore the mine environment, promote vegetation growth, and achieve ecological environment restoration and protection.

[0003] The existing mine restoration material is soil, which is sprayed onto the mountain through soil and grass seeds. The problems are: ① It is easy to fall when encountering heavy rain; ② It is easy to fall when the slope exceeds 75°; resulting in poor mine restoration effect. Summary of the invention

[0004] The present invention provides a spraying material for mine restoration and a construction method thereof, which solves the problem of poor restoration effect of mine restoration materials in the related art.

[0005] The technical solution of the present invention is as follows: A spraying material for mine restoration, comprising the following components in parts by weight: 80-100 parts of composite fiber, 40-60 parts of grass fiber, 10-15 parts of binder, 7-11 parts of water retaining agent, 6-10 parts of compound fertilizer, 8-12 parts of seeds and 20-30 parts of water; The composite fibers include wood fibers, rock wool fibers and peat soil.

[0006] As a further technical solution, the seeds include one or more of tall fescue, ryegrass, bluegrass, Elymus salsa, alfalfa, Robinia pseudoacacia, Amorpha fruticosa, Cosmos, and Lespedeza.

[0007] As a further technical solution, the mass ratio of the wood fiber, rock wool fiber and peat soil is 30:40:30~40:20:20.

[0008] As a further technical solution, the mass ratio of the wood fiber, rock wool fiber and peat soil is 35:29:36.

[0009] The present invention limits the mass ratio of wood fiber, rock wool fiber and peat soil to 35:29:36, thereby further improving the soil moisture content and plant coverage.

[0010] As a further technical solution, the water retaining agent includes fly ash, polylactic acid and polyacrylamide.

[0011] The invention limits the water retaining agent to fly ash, polylactic acid and polyacrylamide, thereby further improving the soil moisture content and plant coverage.

[0012] As a further technical solution, the mass of the polylactic acid and polyacrylamide is greater than the mass of the fly ash.

[0013] The mass of the polylactic acid and polyacrylamide in the invention is greater than the mass of the fly ash, and the soil moisture content and plant coverage are further improved.

[0014] As a further technical solution, the mass ratio of the polylactic acid and polyacrylamide to the fly ash is 6:3~7:2.

[0015] The invention limits the mass ratio of polylactic acid and polyacrylamide to fly ash to 6:3-7:2, thereby further improving the soil moisture content and plant coverage.

[0016] As a further technical solution, the mass ratio of the polylactic acid to the polyacrylamide is 2:5 to 3:4.

[0017] The present invention limits the mass ratio of polylactic acid to polyacrylamide to 2:5-3:4, thereby further improving the soil moisture content and plant coverage.

[0018] As a further technical solution, the preparation method of the water retaining agent includes the following steps: dissolving polyacrylamide in water, adding fly ash for ultrasonication, drying, transferring to a dichloromethane solution of polylactic acid, mixing evenly, and drying to obtain the water retaining agent.

[0019] In the present invention, the preparation method of the water retaining agent is optimized to coat the surface of the fly ash with polyacrylamide first and then with polylactic acid, thereby further improving the soil moisture content and plant coverage.

[0020] As a further technical solution, the preparation method of the composite fiber includes the following steps: mixing wood fiber, rock wool fiber and peat soil evenly, and crushing them to obtain composite fiber.

[0021] The invention also proposes a construction method of the spraying material for mine restoration, which comprises the following steps: after cleaning the mine slope, spraying the spraying material, covering with non-woven fabric or coconut fiber blanket, and performing maintenance.

[0022] The working principle and beneficial effects of the present invention are: The present invention provides a spraying material for mine repair, comprising composite fiber, grass fiber, adhesive, water retaining agent, compound fertilizer, seeds and water; wherein the composite fiber comprises wood fiber, rock wool fiber and peat soil, and the combination of the three improves the soil moisture content and plant coverage rate. In addition, the spraying material for mine repair provided by the present invention is not easy to fall off in the event of heavy rain, and is not easy to fall off when the slope exceeds 75°, and the mine repair effect is good. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In the following examples and comparative examples: The binder is carboxymethyl cellulose; The compound fertilizer is a general agricultural compound fertilizer, and its nitrogen, phosphorus and potassium element specifications are 15-15-15; The seeds are tall fescue seeds, ryegrass seeds and bluegrass seeds in a mass ratio of 1:1:3; Polyacrylamide is non-ionic polyacrylamide with a weight average molecular weight of 8 million; The polylactic acid is PLA 4043D; The fly ash is first-grade fly ash.

[0025] Example 1 S1, 30 parts of wood fiber, 40 parts of rock wool fiber and 30 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of fly ash water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0026] Example 2 S1, 30 parts of wood fiber, 40 parts of rock wool fiber and 30 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2. Evenly mix 80 parts of composite fiber, 40 parts of grass fiber, 10 parts of binder, 7 parts of fly ash water retaining agent, 6 parts of compound fertilizer, 8 parts of seeds and 20 parts of water to obtain a spraying material.

[0027] Example 3 S1, 30 parts of wood fiber, 40 parts of rock wool fiber and 30 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2. Evenly mix 90 parts of composite fiber, 60 parts of grass fiber, 15 parts of binder, 11 parts of fly ash water retaining agent, 10 parts of compound fertilizer, 12 parts of seeds and 30 parts of water to obtain a spraying material.

[0028] Example 4 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of fly ash water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0029] Example 5 S1, 40 parts of wood fiber, 20 parts of rock wool fiber and 20 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of fly ash water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0030] Example 6 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 2 parts of polyacrylamide in 40 parts of water, adding 5 parts of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 2 parts of polylactic acid in 40 parts of dichloromethane, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0031] Example 7 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 2.5 parts of polyacrylamide in 40 parts of water, adding 4 parts of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 2.5 parts of polylactic acid in 40 parts of dichloromethane, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0032] Example 8 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 3 parts of polyacrylamide in 40 parts of water, adding 3 parts of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 3 parts of polylactic acid in 40 parts of dichloromethane, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0033] Example 9 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 3.5 parts of polyacrylamide in 40 parts of water, adding 2 parts of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 3.5 parts of polylactic acid in 40 parts of dichloromethane, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0034] Example 10 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 4 parts of polyacrylamide in 40 parts of water, adding 1 part of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 4 parts of polylactic acid in 40 parts of dichloromethane, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0035] Embodiment 11 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 4 parts of polyacrylamide in 40 parts of water, adding 2 parts of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 3 parts of polylactic acid in 40 parts of dichloromethane, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0036] Example 12 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 5 parts of polyacrylamide in 40 parts of water, adding 2 parts of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 2 parts of polylactic acid in 40 parts of dichloromethane, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0037] Example 13 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 6 parts of polyacrylamide in 40 parts of water, adding 2 parts of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 1 part of polylactic acid in 40 parts of dichloromethane, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0038] Embodiment 14 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 2 parts of polylactic acid in 40 parts of dichloromethane, adding 2 parts of fly ash and ultrasonicating for 30 minutes, and drying to obtain pre-modified fly ash; S3, dissolving 5 parts of polyacrylamide in 40 parts of water, adding pre-modified fly ash, stirring at 300 rpm for 400 min, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0039] Embodiment 15 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 2 parts of polylactic acid, 2 parts of fly ash, 5 parts of polyacrylamide, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0040] Example 16 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 7 parts of polylactic acid in 40 parts of dichloromethane, adding 2 parts of fly ash, ultrasonicating for 30 minutes, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0041] Embodiment 17 S1, 35 parts of wood fiber, 29 parts of rock wool fiber and 36 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2, dissolving 7 parts of polyacrylamide in 40 parts of water, adding 2 parts of fly ash, ultrasonicating for 30 minutes, and drying to obtain a water retaining agent; S4. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0042] Comparative Example 1 S1, 70 parts of wood fiber and 30 parts of peat soil are mixed evenly, and crushed to obtain composite fiber; S2. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of fly ash water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0043] Comparative Example 2 S1. Mix 70 parts of rock wool fiber and 30 parts of peat soil evenly, and crush them to obtain composite fibers; S2. Evenly mix 100 parts of composite fiber, 50 parts of grass fiber, 13 parts of binder, 9 parts of fly ash water retaining agent, 8 parts of compound fertilizer, 10 parts of seeds and 25 parts of water to obtain a spraying material.

[0044] After cleaning the slope of the mine with a slope of 75°, the spraying materials obtained in Examples 1 to 17 and Comparative Examples 1 to 2 were sprayed respectively to obtain a spraying surface with a thickness of 10 cm, covered with non-woven fabrics, and maintained. The area of ​​each treatment area was 5 mu, and each treatment area was repeated 5 times, and the average value of the 5 repeated tests was recorded as the final data. Rainwater erosion was simulated by artificial rainfall, the diameter of the raindrops was 3 mm, the rainfall was 100 mm / h, the rainfall time was 1 hour, and rainfall was once every 1 day. After 3 rainfalls, the soil moisture content and 30d plant coverage were recorded, and the results are shown in Table 1.

[0045] Table 1 Soil moisture content and 30d plant coverage

[0046] It can be seen from Table 1 that after the spraying material provided by the present invention is used, the soil moisture content is above 26% and the 30d plant coverage rate is above 70.0%.

[0047] Compared with Comparative Examples 1-2, Example 1 adds wood fiber, rock wool fiber and peat soil, Comparative Example 1 uses wood fiber and peat soil, and Comparative Example 2 uses rock wool fiber and peat soil. The soil moisture content and 30d plant coverage rate of the spraying material obtained in Example 1 after use are higher than those of Comparative Examples 1-2, indicating that wood fiber, rock wool fiber and peat soil as composite fibers can increase soil moisture content and plant coverage rate.

[0048] The soil moisture content and 30d plant coverage rate of the spraying material obtained in Example 4 after use are higher than those in Example 1 and Example 5, indicating that the mass ratio of wood fiber, rock wool fiber and peat soil is 35:29:36, which can further improve the soil moisture content and plant coverage rate.

[0049] The soil moisture content and 30d plant coverage rate of the spraying materials obtained in Examples 6 to 17 after use are higher than those in Example 4, indicating that using fly ash, polylactic acid and polyacrylamide as water retaining agents can further improve soil moisture content and plant coverage rate than using fly ash as a water retaining agent.

[0050] The soil moisture content and 30d plant coverage rate of the spraying materials obtained in Examples 7 to 17 after use are higher than those in Example 6, indicating that the quality of polylactic acid and polyacrylamide is greater than the quality of fly ash, which can further improve the soil moisture content and plant coverage rate.

[0051] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A spraying material for mine restoration, It is characterized in that The invention comprises the following components in parts by weight: 80-100 parts of composite fiber, 40-60 parts of grass fiber, 10-15 parts of binder, 7-11 parts of water retaining agent, 6-10 parts of compound fertilizer, 8-12 parts of seeds and 20-30 parts of water; The composite fibers include wood fibers, rock wool fibers and peat soil.

2. A spraying material for mine repair according to claim 1, It is characterized in that The mass ratio of the wood fiber, rock wool fiber and peat soil is 30:40:30-40:20:

20.

3. A spraying material for mine restoration according to claim 1, It is characterized in that The mass ratio of the wood fiber, rock wool fiber and peat soil is 35:29:

36.

4. The spraying material for mine restoration according to claim 1, It is characterized in that The water retaining agent comprises fly ash, polylactic acid and polyacrylamide.

5. A spraying material for mine restoration according to claim 4, It is characterized in that The mass of the polylactic acid and polyacrylamide is greater than the mass of the fly ash.

6. A spraying material for mine restoration according to claim 5, It is characterized in that The mass ratio of the polylactic acid and polyacrylamide to the fly ash is 6:3-7:

2.

7. A spraying material for mine restoration according to claim 6, It is characterized in that The mass ratio of the polylactic acid to the polyacrylamide is 2:5 to 3:

4.

8. The spraying material for mine restoration according to claim 4, It is characterized in that The preparation method of the water retaining agent comprises the following steps: dissolving polyacrylamide in water, adding fly ash for ultrasonication, drying, transferring to a dichloromethane solution of polylactic acid, mixing evenly, and drying to obtain the water retaining agent.

9. The spraying material for mine restoration according to claim 1, It is characterized in that The preparation method of the composite fiber comprises the following steps: mixing wood fiber, rock wool fiber and peat soil evenly, and crushing them to obtain the composite fiber.

10. The method for constructing a mine repair spraying material according to any one of claims 1 to 9, It is characterized in that The following steps are involved: After cleaning the mine slope, spray the seeding material and cover it with non-woven fabric or coconut fiber blanket for maintenance.