Buried test piece measuring cathode and method thereof

The method of measuring cathode through buried test pieces, including self-corrosion test pieces, cathode polarization test pieces and reference electrode, solves the problem of corrosion rate detection of oil and gas pipelines in the soil environment, and realizes accurate evaluation of pipeline corrosion conditions and Effective detection of cathode protection system reduces the risk of pipeline corrosion and extends service life.

CN118895510APending Publication Date: 2024-11-05SHENYANG INST OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410946187.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art cannot effectively and accurately detect the corrosion rate of oil and gas pipelines in the soil environment and the effect of cathode protection system, making it difficult to prevent the pipeline from failing prematurely.

Method used

The method of measuring the cathode by using buried test pieces, including self-corrosion test pieces, cathode polarization test pieces and reference electrode. By setting the test pieces in the soil and electrically connecting them, the corrosion rate of the pipeline and the performance of the cathode protection system are measured. Combined with power failure testing and potential fluctuation analysis, accurately assess the corrosion status of the pipeline.

Benefits of technology

Accurate measurement of the corrosion rate of oil and gas pipelines, timely discover and deal with the shortcomings of the cathode protection system, reduce the risk of pipeline corrosion, extend the service life of the pipeline, and reduce the detection cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895510A_ABST
    Figure CN118895510A_ABST
Patent Text Reader

Abstract

The invention provides a buried test piece measuring cathode and a method thereof, and relates to the technical field of pipeline detection.The buried test piece measuring cathode comprises a to-be-detected pipeline located in soil, a self-corrosion test piece, a cathode protection polarization test piece, a reference electrode and a switch, the self-corrosion test piece and the cathode protection polarization test piece are symmetrically arranged in the soil and located on the two sides of the outer diameter of the pipeline, and the wide faces of the self-corrosion test piece and the cathode protection polarization test piece are parallel to the pipeline; the exposed surface is buried back to the pipeline, the self-corrosion test piece and the cathode protection polarization test piece are connected with the pipeline and are connected in series with the electrical switch so that the self-corrosion test piece and the cathode protection polarization test piece can be disconnected from the pipeline, and the reference electrode is arranged on the ground and is connected with the switch; the method comprises the following steps: (1) burying a test piece; (2) taking out the test piece for treatment; according to the buried test piece measuring cathode and the method thereof, the operation is simple and convenient, the cost is low, complex equipment and a large amount of human input are not needed, the cost is relatively low, the corrosion rate of an oil and gas pipeline can be accurately measured, and pipeline corrosion is effectively prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of pipeline detection, and in particular to a buried test piece measuring cathode and a method thereof. Background Art

[0002] Oil and gas gathering and transportation facilities and pipelines usually use anti-corrosion measures to provide certain protection for materials and extend the service life of equipment and pipelines. However, various natural factors, environmental factors and human factors during the operation of equipment and pipelines can cause the failure of protective measures, thereby directly exposing materials to corrosive media, causing equipment and pipelines to fail prematurely during their service life.

[0003] Stray current mainly refers to the current that does not move in the prescribed path. It exists in the soil and has no connection with the equipment system that needs to be protected. This stray current in the soil will enter the pipeline through a part of the pipeline where the anti-corrosion layer is relatively weak, and after moving a certain distance in the pipeline, it will leave from a part of the pipeline where the anti-corrosion layer is relatively weak and return to the soil. Corrosion will occur where these currents leave the pipeline, which is why it is called stray current corrosion. And according to the source of the interference source, it can be divided into DC stray current, AC DC current and ground current; DC stray current mainly comes from DC electrified railways, DC electrolysis systems, DC welding systems, high-voltage DC transmission lines, and other pipelines with external cathodic protection systems; AC stray current mainly comes from AC electrified railways, high-voltage AC transmission lines, etc.

[0004] Therefore, after oil and gas facilities and pipelines are put into operation, they must be inspected during their service. Inspection is the basis for reliable safety evaluation of long-distance oil and gas pipelines, and is an important means to prevent failure of long-distance oil and gas pipelines and reduce pipeline risks. Cathodic protection and stray current detection research is one of the important contents of oil and gas pipeline inspection;

[0005] The current scheme cannot effectively and accurately obtain the corrosion rate when performing cathodic protection and stray current detection to carry out corrosion protection work to prevent pipeline corrosion. Therefore, based on the detection of cathodic protection and stray current, we propose a buried test piece cathode measurement method. Summary of the invention

[0006] The object of the present invention is to provide a buried test piece measuring cathode and method thereof to solve the above-mentioned deficiencies in the technology.

[0007] In order to achieve the above-mentioned purpose, the present invention provides the following technical solutions: a buried test piece measuring cathode, comprising a pipeline to be tested located in the soil, a self-corrosion test piece, a cathode polarization test piece, a reference electrode and a switch, wherein the self-corrosion test piece and the cathode polarization test piece are symmetrically arranged on both sides of the outer diameter of the pipeline in the soil, and the wide surface is parallel to the pipeline, and the exposed surface is buried with the back of the pipeline, the self-corrosion test piece and the cathode polarization test piece are connected to the pipeline, and an electrical switch is connected in series so that the self-corrosion test piece and the cathode polarization test piece can be disconnected from the pipeline, and the reference electrode is placed on the ground and connected to the switch.

[0008] Furthermore, the central axis of the self-corrosion test piece and the cathode polarization test piece is at the same elevation as the center of the pipeline, and the net distance from the pipeline wall is 0.1 to 0.3 m.

[0009] Furthermore, according to the buried test piece measuring cathode according to claim 1, the cathode polarization maintaining test piece is connected to the pipeline by using a test pile, a quick connector, a coupler or an adapter.

[0010] Furthermore, the self-corrosion test piece and the cathode polarization test piece and the pipeline can be connected in series with a current interrupter.

[0011] Furthermore, the reference electrode is connected to a switch for collecting parameters of AC voltage and pipe-to-ground potential fluctuation values.

[0012] Furthermore, the self-corrosion test piece is a steel sheet made of No. 20 steel.

[0013] A method for measuring cathode of a buried test piece, the method comprising the following steps:

[0014] (I) The steps for burying the test piece are as follows:

[0015] 1) Cathodic protection stray current measurement

[0016] Test the interference of stray current along the entire pipeline, including dynamic and static stray current interference;

[0017] 2) Power off test

[0018] After the test piece is buried, the cathodic protection system is turned off to observe the changes in the natural corrosion potential of the pipeline;

[0019] 3) Steel sheet processing and burial

[0020] After the steel sheet is polished to a surface without marks, the surface is cleaned, and then its size is measured with a vernier caliper, and the steel sheet is placed in a container containing a solution to remove oil stains on the surface. After degreasing, it is washed with water and scrubbed with anhydrous ethanol. After being dried by a hair dryer, it is placed in a drying oven to dry, and then cooled to room temperature and weighed to a constant weight with a precision electronic analytical balance. The mass is taken and recorded as W0, and it is wrapped and buried on site;

[0021] (II) Sample removal and processing

[0022] The corrosion condition of the effective self-corrosion test piece was observed, the corrosion morphology of the self-corrosion test piece was recorded, the corrosion products on the surface of the self-corrosion test piece were retained for corrosion product analysis, the corrosion products on the surface of the steel piece were rinsed with deionized water and a steel brush was used to remove the corrosion products, and then the surface corrosion film was further removed with a film removal liquid. The above process was repeated many times until the steel piece was cleaned, and then the water was absorbed with filter paper and immersed in anhydrous ethanol for 5 minutes. After dehydration, it was taken out and placed in a vacuum dryer. After 24 hours, its mass was weighed with a precision electronic analytical balance and recorded as W1. Finally, the average corrosion rate was calculated according to the mass difference before and after corrosion and the corrosion time.

[0023] Furthermore, the cathodic protection stray current measurement is carried out in areas with obvious interference sources, such as transformer entry points, crossings between railways and highways, spot checks of sections parallel to railways and highways at close distances, crossings of high-voltage lines, areas where pipelines cross, etc. If preliminary tests find stray current interference, further 24-hour continuous testing will be carried out.

[0024] Further, the power-off test comprises the following steps:

[0025] Step 1: Before measuring, make sure the pipeline is in cathodic protection state;

[0026] Step 2: When measuring, place the probe end of the power-off tester on the moist soil above the pipeline, and ensure that the bottom of the probe is in good contact with the soil;

[0027] Step 3: Adjust the voltmeter to the appropriate range, read the data, record the pipe-to-ground potential value, temperature and polarity, and indicate the name of the potential value;

[0028] Step 4: Divide the soil layer from the soil surface directly above the pipeline to the top of the pipeline into five equal parts, and measure the potential of the pipeline relative to the copper / copper sulfate electrode at each soil layer.

[0029] Furthermore, the soil around the self-corrosion test piece and the cathodic polarization test piece is moistened with water and compacted so that the test piece is in close contact with the soil to ensure that it is fully polarized, and the solution is petroleum ether with a boiling range of 60-90°C.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. Through the buried test piece measurement cathode and its method, the corrosion rate of oil and gas pipelines in the soil environment can be accurately measured, providing reliable data support for pipeline corrosion protection.

[0032] 2. After measuring and analyzing the corrosion rate, the corrosion of the pipeline can be discovered in time, and then corresponding protective measures can be taken to avoid premature failure of the pipeline during its service life and ensure the safe and stable operation of the pipeline.

[0033] 3. At the same time, through the setting of self-corrosion test pieces and cathodic polarization test pieces, the protection effect of the cathodic protection system on the pipeline can be comprehensively evaluated, and the deficiencies of the cathodic protection system can be discovered and dealt with in time.

[0034] 4. Through cathodic protection stray current measurement and power-off test, the interference of stray current in the soil around the pipeline can be accurately detected, providing an important basis for pipeline safety assessment.

[0035] In summary, the buried test piece cathode measurement method and its operation are simple and low-cost, do not require complex equipment and a large amount of manpower investment, and have a relatively low cost. It can accurately measure the corrosion rate of oil and gas pipelines, effectively prevent pipeline corrosion, and improve the safety and service life of pipelines. It has important practical application value and is suitable for wide application in oil and gas pipeline inspection. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A schematic diagram of a buried test piece provided by the present invention for measuring the outer side of a cathode pipeline;

[0037] Figure 2 A schematic diagram of a buried test piece for measuring a cathode pipeline end provided by the present invention.

[0038] Legend: 1. Pipeline; 2. Self-corrosion test piece; 3. Cathodic polarization test piece; 4. Reference electrode; 5. Switch. DETAILED DESCRIPTION

[0039] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0040] To facilitate understanding of the present invention, the present invention will be described more comprehensively below with reference to related references, and several embodiments of the present invention are given. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.

[0041] It should be noted that when an element is referred to as being "fixed on" another element, it may be directly on the other element or there may also be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used in this article are for illustrative purposes only.

[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0043] Example 1

[0044] like Figure 1 and 2 As shown, the present invention provides a buried test piece measuring cathode, comprising a pipeline 1 to be detected in the soil, a self-corrosion test piece 2, a cathode polarization test piece 3, a reference electrode 4 and a switch 5;

[0045] The self-corrosion test piece 2 and the cathode polarization test piece 3 are symmetrically arranged on both sides of the outer diameter of the pipeline 1 in the soil, with the wide surface parallel to the pipeline 1 and the exposed surface buried with the back of the pipeline 1. The self-corrosion test piece 2 and the cathode polarization test piece 3 are connected to the pipeline 1, and an electrical switch 5 is connected in series to enable the self-corrosion test piece 2 and the cathode polarization test piece 3 to be disconnected from the pipeline 1. The reference electrode 4 is placed on the ground and connected to the switch 5. The reference electrode 4 is connected to the switch 5 and is used to collect AC voltage and pipe-to-ground potential fluctuation value parameters.

[0046] The central axis of the self-corrosion test piece 2 and the cathode polarization test piece 3 are at the same elevation as the center of the pipeline 1, and the net distance from the wall of the pipeline 1 is 0.1 to 0.3 m.

[0047] It should be added that the cathode-protected polarization test piece 3 is connected to the pipeline 1 using a test pile, a quick connector, a coupler or an adapter, and the self-corrosion test piece 2 and the cathode-protected polarization test piece 3 and the pipeline 1 can also be connected in series using a current interrupter, and the self-corrosion test piece 2 is made of a steel sheet made of No. 20 steel.

[0048] Embodiment 2, a method for measuring cathode by buried test piece, based on the above-mentioned method for measuring cathode by buried test piece:

[0049] (I) The steps for burying the test piece are as follows:

[0050] 1) Cathodic protection stray current measurement

[0051] The interference of stray current is tested along the entire pipeline 1, including dynamic and static stray current interference; cathodic protection stray current is measured in areas with obvious interference sources, such as transformer entry points, crossing railways and highways, spot checks of sections parallel to railways and highways at close distances, high-voltage line crossings, areas where pipelines cross, etc. If preliminary tests find stray current interference, further 24-hour continuous testing will be carried out;

[0052] By 1) choosing a suitable testing location:

[0053] 2) Power off test

[0054] After the test piece is buried, the cathodic protection system is turned off to observe the change of natural corrosion potential of pipeline 1;

[0055] The detailed steps of power-off test are as follows:

[0056] Step 1: Before measuring, confirm that pipeline 1 is in a cathodic protection state;

[0057] Step 2: During measurement, place the probe end of the power-off tester on the moist soil on the surface above the pipeline 1, and ensure that the bottom of the probe is in good contact with the soil;

[0058] Step 3: Adjust the voltmeter to the appropriate range, read the data, record the pipe-to-ground potential value, temperature and polarity, and indicate the name of the potential value;

[0059] Step 4: Divide the soil layer from the soil surface directly above the pipeline 1 to the top of the pipeline 1 into five equal parts, and measure the potential of the pipeline 1 relative to the copper / copper sulfate electrode at each soil layer.

[0060] 3) Steel sheet processing and burial

[0061] After the steel sheet is polished to a surface without marks, the surface is cleaned, and then its size is measured with a vernier caliper, and the steel sheet is placed in a container containing a solution to remove oil stains on the surface. After degreasing, it is washed with water and scrubbed with anhydrous ethanol. After being dried by a hair dryer, it is placed in a drying oven to dry, and then cooled to room temperature and weighed to a constant weight with a precision electronic analytical balance. The mass is taken and recorded as W0, and it is wrapped and buried on site;

[0062] Specifically, the solution is petroleum ether with a boiling range of 60-90°C;

[0063] (II) Sample removal and processing

[0064] The corrosion condition of the effective self-corrosion test piece 2 was observed, the corrosion morphology of the self-corrosion test piece 2 was recorded, the corrosion products on the surface of the self-corrosion test piece 2 were retained for corrosion product analysis, the corrosion products on the surface of the steel sheet were washed with deionized water and removed with a steel brush, and then the surface corrosion film was further removed with a film removal liquid, and the above process was repeated many times until the steel sheet was cleaned, and then the water was absorbed with filter paper and immersed in anhydrous ethanol for 5 minutes, and then taken out after dehydration and placed in a vacuum dryer, and its mass was weighed with a precision electronic analytical balance after 24 hours, recorded as W1, and finally the average corrosion rate was calculated according to the mass difference before and after corrosion and the corrosion time;

[0065] Among them, the average corrosion rate is calculated based on the mass difference (W0-W1) of the test piece before and after corrosion and the corrosion time. According to the corrosion rate data obtained from the test, the corrosion situation of the oil and gas pipeline is evaluated, and corresponding corrosion protection measures are formulated to extend the service life of the pipeline and ensure safe operation.

[0066] In the above process of (3) steel piece processing and burying and (ii) test piece removal processing;

[0067] The following test equipment and materials need to be prepared: including self-corrosion test pieces, cathodic polarization test pieces, reference electrodes, electrical switches, power-off testers, voltmeters, precision electronic analytical balances, vernier calipers, degreasing solutions (petroleum ether with a boiling range of 60-90°C), deionized water, film removal solution, anhydrous ethanol, drying oven, vacuum dryer, etc.

[0068] During the burial of the test pieces, the soil around the self-corrosion test piece 2 and the cathode polarization test piece is moistened with water and compacted to make the test piece in close contact with the soil to ensure that it is fully polarized.

[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A buried test piece measuring cathode, Features: The invention comprises a pipeline (1) to be tested located in soil, a self-corrosion test piece (2), a cathode polarization test piece (3), a reference electrode (4) and a switch (5); the self-corrosion test piece (2) and the cathode polarization test piece (3) are symmetrically arranged on both sides of the outer diameter of the pipeline (1) in the soil, with the wide surface parallel to the pipeline (1) and the exposed surface buried with the back of the pipeline (1); the self-corrosion test piece (2) and the cathode polarization test piece (3) are connected to the pipeline (1), and an electrical switch (5) is connected in series so that the self-corrosion test piece (2) and the cathode polarization test piece (3) can be disconnected from the pipeline (1); and the reference electrode (4) is placed on the ground and connected to the switch (5).

2. A buried test piece measuring cathode according to claim 1, Features: The central axes of the self-corrosion test piece (2) and the cathode polarization test piece (3) are at the same elevation as the center of the pipeline (1), and the net distance from the pipeline (1) wall is 0.1 to 0.3 m.

3. A buried test piece measuring cathode according to claim 1, Features: The cathode polarization-maintaining test piece (3) is connected to the pipeline (1) by using a test pile, a quick connector, a coupler or an adapter.

4. A buried test piece measuring cathode according to claim 1, Features: The self-corrosion test piece (2) and the cathode polarization test piece (3) can also be connected in series with the pipeline (1) using a current interrupter.

5. The buried test piece measuring cathode according to claim 1, Features: The reference electrode (4) is connected to a switch (5) and is used to collect parameters of AC voltage and pipe-to-ground potential fluctuation values.

6. A buried test piece measuring cathode according to claim 1, Features: The self-corrosion test piece (2) is a steel sheet made of No. 20 steel.

7. A method for measuring cathode of buried test piece, Features: Applied to the buried test piece measuring cathode as claimed in claims 1-6, the method comprises the following: (I) The steps for burying the test piece are as follows: 1) Cathodic protection stray current measurement Testing the interference of stray current along the entire pipeline (1), including dynamic and static stray current interference; 2) Power off test After the test piece is buried, the cathodic protection system is turned off to observe the change of the natural corrosion potential of the pipeline (1); 3) Steel sheet processing and burial After the steel sheet is polished to a surface without marks, the surface is cleaned, and then its size is measured with a vernier caliper, and the steel sheet is placed in a container containing a solution to remove oil stains on the surface. After degreasing, it is washed with water and scrubbed with anhydrous ethanol. After being dried by a hair dryer, it is placed in a drying oven to dry, and then cooled to room temperature and weighed to a constant weight with a precision electronic analytical balance. The mass is taken and recorded as W0, and it is wrapped and buried on site; (II) Sample removal and processing The corrosion condition of the effective self-corrosion test piece (2) is observed, the corrosion morphology of the self-corrosion test piece (2) is recorded, and the corrosion products on the surface of the self-corrosion test piece (2) are retained for corrosion product analysis. The corrosion products on the surface of the steel sheet are rinsed with deionized water and a steel brush is used to remove the corrosion products. Then, the surface corrosion film is further removed with a film removal liquid. The above process is repeated many times until the steel sheet is cleaned, and then the water is absorbed with filter paper and immersed in anhydrous ethanol for 5 minutes. After dehydration, it is taken out and placed in a vacuum dryer. After 24 hours, its mass is weighed with a precision electronic analytical balance and recorded as W1. Finally, the average corrosion rate is calculated according to the mass difference before and after corrosion and the corrosion time.

8. A method for measuring cathode of a buried test piece according to claim 7, Features: The cathodic protection stray current measurement is carried out in areas with obvious interference sources, such as transformer entry points, crossings between railways and highways, spot checks of sections parallel to railways and highways at close distances, crossings of high-voltage lines, areas where pipelines cross, etc. If preliminary tests find stray current interference, further 24-hour continuous testing will be carried out.

9. A method for measuring cathode of a buried test piece according to claim 7, Features: The power-off test comprises the following steps: Step 1: Before measuring, confirm that the pipeline (1) is in a cathodic protection state; Step 2: During measurement, place the probe end of the power-off tester on the moist soil on the surface above the pipeline (1), and ensure that the bottom of the probe is in good contact with the soil; Step 3: Adjust the voltmeter to the appropriate range, read the data, record the pipe-to-ground potential value, temperature and polarity, and indicate the name of the potential value; Step 4: Divide the soil layer from the soil surface directly above the pipeline (1) to the top of the pipeline (1) into five equal parts, and measure the potential of the pipeline (1) relative to the copper / copper sulfate electrode at each soil layer.

10. A method for measuring cathode of a buried test piece according to claim 7, Features: The soil around the self-corrosion test piece (2) and the cathodic polarization test piece is moistened with water and compacted so that the test piece is in close contact with the soil to ensure that it is fully polarized. The solution is petroleum ether with a boiling range of 60-90°C.

Citation Information

Patent Citations

  • Method and system for testing cathode protection of buried pipeline

    CN114774928A

  • Ground marking and cathode protection comprehensive intelligent monitoring system for oil and gas pipeline

    CN116770317A

  • Underground pipeline protection potential intelligent detection system and detection method

    CN118256921A

  • Corrosion preventive method for underground buried metallic pipe

    JP1993230677A