Preparation method of monatomic supported cobalt selenide oxygen evolution reaction catalyst
By preparing single-atom supported cobalt selenide catalysts on carbon cloth, the problem of decreased stability of transition metal selenides in the oxygen evolution reaction was solved, resulting in a catalyst with high activity and high stability, suitable for water electrolysis and battery applications.
Patent Information
- Application Number
- CN202411397011.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-05
AI Technical Summary
Existing transition metal selenides suffer from surface reconstruction during the oxygen evolution reaction, leading to decreased stability and making them unsuitable for industrial applications. Furthermore, existing catalysts such as iridium oxide and ruthenium oxide are costly and have low abundance, making them unsuitable for large-scale commercialization.
Single-atom-supported cobalt selenide catalysts were prepared on carbon cloth using hydrothermal, vapor deposition, and electrochemical deposition techniques to form a rough-surfaced nanoneedle structure. By adjusting the charge distribution of active sites and the metal-oxygen binding strength, the catalytic activity and stability were improved.
The prepared catalyst exhibits excellent oxygen evolution reaction performance and stability. The three-dimensional nanoneedle structure increases the active sites, provides good conductivity, is suitable for large-scale industrial applications, is inexpensive, and has catalytic activity exceeding that of commercial ruthenium oxide.
Smart Images

Figure CN118895533A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrocatalytic materials, and in particular to a method for preparing a single-atom-supported cobalt selenide oxygen evolution reaction catalyst. Background Art
[0002] The oxygen evolution reaction (OER) is a key process in a range of energy conversion technologies, including water electrolysis, metal-air batteries, and fuel cells. The efficiency and stability of the oxygen evolution reaction are crucial to advancing sustainable energy systems. To improve the efficiency and stability of OER, it is necessary to explore efficient and durable OER electrocatalysts. Currently, the best catalysts for OER activity are iridium oxide and ruthenium oxide, but they are expensive and have low abundance, which is not conducive to large-scale commercial applications.
[0003] Transition metal chalcogenides, especially selenides based on transition metals such as cobalt, nickel and iron, have attracted the interest of researchers due to their tunable electronic structure and relatively low cost. The rich d electrons, high polarizability and strong metallicity of selenium make the metal atoms bound to it more electrophilic, thereby increasing the affinity of selenide with oxygen, resulting in the reconstruction of the selenium surface into transition metal hydroxide oxides during the OER process, thereby improving the catalytic activity. However, this reconstruction will cause its OER stability to decrease rapidly and cannot meet the requirements of industrial applications. How to inhibit the surface remodeling of TMSe while maximizing its catalytic activity is an urgent problem to be solved. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst, which has high activity and high stability under industrial conditions.
[0005] A method for preparing a single-atom-loaded cobalt selenide oxygen evolution reaction catalyst comprises the following steps: using hydrothermal, vapor deposition, and electrochemical deposition techniques to prepare a single-atom-loaded cobalt selenide catalyst in situ grown on carbon cloth, the catalyst having a rough surface and a nano-needle shape. Specifically, the method comprises the following steps: (1) subjecting carbon cloth to ultrasonic treatment in a mixed solution of nitric acid and sulfuric acid; (2) dissolving cobalt nitrate, ammonium fluoride and urea in deionized water, and adding a piece of carbon cloth; (3) subjecting the above solution to a high-pressure closed reaction by a hydrothermal method to obtain a cobalt hydroxide catalyst in situ grown on the carbon cloth; (4) annealing the catalyst obtained in step (3) with selenium powder in an argon atmosphere to obtain a cobalt selenide catalyst in situ grown on the carbon cloth; (5) using the catalyst obtained in step (4) as a working electrode, a carbon rod as a counter electrode, Hg / HgO as a reference electrode, and a mixed solution of chemical A and sodium chloride as an electrolyte, and using an electrochemical workstation to perform electrochemical deposition on the working electrode to obtain a cobalt selenide catalyst in situ grown on the carbon cloth with a single atom load.
[0006] In the mixed solution of nitric acid and sulfuric acid in step (1), the molar ratio of nitric acid to sulfuric acid is 1:0.5 to 1:2.
[0007] In the step (2), the molar ratio of cobalt nitrate, ammonium fluoride and urea is 2:3:7 to 4:5:9.
[0008] The size of the carbon cloth added in step (2) is 1×0.5 cm 2 Up to 1×4 cm 2 .
[0009] The vessel used for the high-pressure closed reaction in step (3) is a stainless steel high-pressure reactor.
[0010] In the step (3), the heating temperature in the reactor is 100° C. to 150° C., and the heating time is 5 h to 8 h.
[0011] The content of selenium powder in the step (4) is 0.2 g to 0.5 g.
[0012] The annealing temperature in step (4) is 300°C to 500°C, and the annealing time is 0.5 h to 2 h.
[0013] The electrochemical workstation used for electrochemical deposition in step (5) is Shanghai Chenhua CHI660E, the mode is cyclic voltammetry, the voltage range is -2 V vs. Hg / HgO to 0 V vs. Hg / HgO, and the number of cycles is 2 to 6.
[0014] In the step (5), the chemical A is any one of silver nitrate, nickel nitrate, iron nitrate, copper nitrate, chromium nitrate and manganese nitrate.
[0015] In the step (5), the molar ratio of chemical A to sodium chloride in the mixed solution is 0.004 to 0.008.
[0016] In addition, the present invention also discloses a single-atom-loaded cobalt selenide oxygen evolution reaction catalyst.
[0017] The single-atom-supported cobalt selenide oxygen evolution reaction catalyst prepared in the present invention is prepared by any of the above-mentioned methods for preparing a single-atom-supported cobalt selenide oxygen evolution reaction catalyst, and the single-atom-supported cobalt selenide oxygen evolution reaction catalyst has a three-dimensional needle-like structure grown on a carbon cloth.
[0018] Compared with the prior art, the present invention has the following advantages.
[0019] (1) The single-atom-loaded cobalt selenide catalyst prepared by the preparation method of the present invention has excellent OER performance and stability; (2) Compared with catalysts with other morphologies, the catalyst prepared by the preparation method of the present invention has a three-dimensional nanoneedle structure, has a larger specific surface area, and increases the number of OER active sites. In addition, the nanoneedles are intertwined to form a huge network for electron conduction, which is beneficial to conductivity. In addition, the preparation method of the present invention has a simple process, low material cost, good repeatability, and can be prepared on a large scale to meet industrial applications. (3) The catalyst is a composite material, and the single-atom species in the catalyst can be precisely adjusted, thereby improving the activity of the active site and the stability of the catalyst, and effectively improving the OER performance of the catalyst. (4) The catalyst of the present invention adjusts the charge distribution of the active site by loading single atoms, enhances the bonding between metal and oxygen in the structure, and thus makes the catalyst highly active and stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is the X-ray diffraction pattern (XRD) of Ag-CoSe2 / CC prepared in Example 1.
[0021] Figure 2 This is a scanning electron microscopy image (SEM) of Ag-CoSe2 / CC prepared in Example 1.
[0022] Figure 3 OER performance of Ag-CoSe2 / CC prepared in Example 1 in 1M KOH electrolyte: a is the OER polarization curve; b is the Tafel slope; c is the double layer capacitance curve; d is the impedance diagram; e is the stability test diagram. DETAILED DESCRIPTION
[0023] The present invention uses RIGAKU SmartLab X-ray diffractometer to obtain XRD patterns. The instrument uses Cu Kα as the anode target, the X-ray power is 2 kW, and the scanning speed is 6° min -1 , the scanning range is 10°~80°; the SEM images were obtained using a FEI Quanta-450 FEG field emission scanning electron microscope; the OER test was performed using a Chenhua electrochemical workstation. The reference electrode is Hg / HgO, the counter electrode is a carbon rod, and the working electrode is a single-atom-loaded cobalt selenide catalyst. The test voltage range of the LSV polarization curve is 0 V vs. Hg / HgO to 0.8 V vs. Hg / HgO, and the scanning speed is 2 mV s -1 , IR compensation is 95 %. Tafel slope is obtained from LSV test curve. Input voltage for impedance is 0.45926 V vs. Hg / HgO. Stability test voltage is 1.4 V vs. Hg / HgO.
[0024] Embodiment 1:
[0025] (1) The carbon cloth was ultrasonically treated in a mixed solution of nitric acid and sulfuric acid in a molar ratio of 1:1, washed with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven at 60 °C for 6 h.
[0026] (2) Dissolve 3 mmol of cobalt nitrate, 4 mmol of ammonium fluoride, and 8 mmol of urea in 40 mL of deionized water and add a 1×1 cm 2 of carbon cloth.
[0027] (3) The solution in step (2) was transferred into a 50 mL autoclave with a Teflon-lined liner and kept at 120° C. for 6 h to obtain a cobalt hydroxide (Co(OH)2 / CC) catalyst in situ grown on carbon cloth.
[0028] (4) Add 0.4 g of selenium powder to the catalyst obtained in step (3) and anneal it in an argon atmosphere (400 ° C, 1 h) to obtain a cobalt selenide catalyst (CoSe2 / CC) grown in situ on carbon cloth.
[0029] (5) The cobalt selenide catalyst grown on the carbon cloth obtained in step (4) was used as a working electrode, a carbon rod was used as a counter electrode, Hg / HgO was used as a reference electrode, and a mixed solution of 0.3 mM silver nitrate and 0.05 M sodium chloride (100 mL) was used as an electrolyte. The working electrode was electrochemically deposited using cyclic voltammetry of an electrochemical workstation. The voltage range was set to -0.6 V vs. RHE to -0.2 V vs. RHE, and the number of cycles was 5. A cobalt selenide catalyst (Ag-CoSe2 / CC) with a silver single atom load in situ grown on carbon cloth was obtained.
[0030] Figure 1 The silver single atom supported cobalt selenide catalyst (Ag-CoSe2 / CC) prepared by the present invention is different from CoSe2 ( Figure 1 PDF#09-0234 in is the standard crystal card of CoSe2, which is consistent with the crystal structure, indicating that Ag is doped in the form of single atoms, without agglomerating into particles or forming other silver oxides, and the crystal structure of CoSe2 is maintained.
[0031] Figure 2 It shows that the silver single atom-supported cobalt selenide catalyst (Ag-CoSe2 / CC) prepared by the present invention has a vertically staggered nanoneedle structure.
[0032] The silver single atom-loaded cobalt selenide catalyst (Ag-CoSe2 / CC) prepared by the present invention was used as a working electrode, a carbon rod as a counter electrode, Hg / HgO as a reference electrode, and 1M KOH dissolved as an electrolyte to test the electrochemical oxygen evolution performance of Ag-CoSe2 / CC. The test results are as follows: Figure 3 a shows that the Ag-CoSe2 / CC catalyst of the present invention only needs a low overpotential of 167 mV to reach 10 mA cm -2 The current density of Ag-CoSe2 / CC catalyst of the present invention is only 28.9 mV dec. -1 , indicating that Ag-CoSe2 / CC has very fast oxygen evolution reaction kinetics. c is the double layer capacitance curve of Ag-CoSe2 / CC of the present invention, 16.4 mF cm -2 The high double-layer capacitance value of shows that Ag-CoSe2 / CC has a large electrochemically active surface area and multiple electrochemically active sites, which is beneficial to its oxygen evolution reaction activity. d shows that in the electrochemical impedance spectrum of the Ag-CoSe2 / CC catalyst of the present invention, the charge transfer resistance is only 3.65Ω, indicating that it has a small charge transfer resistance value, which is beneficial to the electron transfer between the electrolyte and the catalyst surface and enhances the conductivity. e shows that the Ag-CoSe2 / CC catalyst of the present invention has a high electrochemical activity at 100 mA cm -2 Under high current density, the performance remains almost unchanged after 500 h of continuous operation, and it has excellent oxygen evolution stability.
[0033] Compared with the prior art, the present invention improves the synthesis method of the catalyst. The method makes the catalyst grow uniformly, is simple to operate, improves the yield, has good repeatability, and effectively increases the specific surface area of the catalyst, providing abundant active sites that are conducive to electron transfer. In addition, the synthesis method also improves the catalytic activity of the cobalt selenide catalyst, making it higher than the level of commercial ruthenium oxide. The method is simple and convenient, suitable for large-scale production, and has significant green environmental benefits. It can be widely used in the fields of water electrolysis, hydrogen production, and batteries.
[0034] Although the above embodiments of the present invention are described in conjunction with the accompanying drawings, it should be noted that the present invention is not limited to the above specific embodiments or application fields. In addition, the above specific embodiments are only for illustrative purposes and are not restrictive. Individuals with a certain level of professional knowledge in this field can, inspired by this description, create many alternative forms without departing from the scope of protection claimed by the present invention, all of which are protected by the present invention.
Claims
1. A method for preparing a single-atom-supported cobalt selenide oxygen evolution reaction catalyst, comprising the following steps: selenizing cobalt hydroxide using selenium powder to obtain a cobalt selenide precursor; and loading single atoms on the precursor using an electrochemical deposition method to obtain a single-atom-supported cobalt selenide oxygen evolution reaction catalyst.
2. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 1, specifically comprising: The carbon cloth is ultrasonically treated in a mixed solution of nitric acid and sulfuric acid, then repeatedly washed with deionized water and anhydrous ethanol in sequence, and finally dried; the pretreated carbon cloth, cobalt nitrate, ammonium fluoride and urea are added to deionized water by a hydrothermal method, and a cobalt hydroxide catalyst is obtained after heating, washing and drying in a reactor; the cobalt hydroxide is annealed with selenium powder by a vapor deposition method to obtain a cobalt selenide catalyst; and the cobalt selenide catalyst is electrochemically deposited by an electrochemical deposition method using a mixed solution of chemical A and sodium chloride as an electrolyte to load single atoms.
3. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 2, characterized in that: In the mixed solution, the molar ratio of nitric acid to sulfuric acid is 1:0.5 to 1:
2.
4. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 2, characterized in that: The molar ratio of cobalt nitrate, ammonium fluoride and urea is 2:3:7 to 4:5:
9.
5. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 2, characterized in that: The size of the added carbon cloth is 1×0.5 cm 2 Up to 1×4 cm 2 .
6. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 2, characterized in that: The reactor is a stainless steel high-pressure reactor.
7. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 2, characterized in that: The heating temperature in the reactor is 100°C to 150°C, and the heating time is 5 h to 8 h.
8. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 2, characterized in that: When selenizing cobalt hydroxide by vapor deposition, 0.2 g to 0.5 g of selenium powder is added, the annealing temperature is 300° C. to 500° C., and the annealing time is 0.5 h to 2 h.
9. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 2, characterized in that: Chemical A is any one of silver nitrate, nickel nitrate, iron nitrate, copper nitrate, chromium nitrate, and manganese nitrate.
10. The method for preparing a single-atom supported cobalt selenide oxygen evolution reaction catalyst according to claim 2, characterized in that: The molar ratio of chemical A to sodium chloride in the mixed solution used for electrodeposition is 0.004 to 0.008.