Method for treating surface of titanium-based material
By using fluorine-containing alkaline electrolyte on the surface of titanium-based materials, the titanium hydride is removed and the protective layer is formed, and the complexity and hazards of removing titanium hydride in the prior art are solved, and the material is realized Improved performance and extended life.
Patent Information
- Application Number
- CN202410993440.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-05
AI Technical Summary
The prior art has problems such as cumbersome operation, restriction of structure, or the use of strong acids to cause harm when removing titanium hydrides on the surface of titanium-based materials, and lacks a simple, effective and safe removal method.
The alkaline electrolyte containing fluoride ions is used to electrolyze to generate a titanium-based material for removing titanium hydride, and then a protective layer is formed by anodizing, and a titanium dioxide protective film is generated in the form of a large voltage and a small current.
It realizes efficient removal of titanium hydride on the surface of titanium-based materials, extends the service life of the material, avoids harm to components, is easy to operate, and is not restricted by structure.
Smart Images

Figure CN118895544A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of titanium-based materials, and in particular relates to a method for treating the surface of a titanium-based material. Background Art
[0002] The excellent properties of pure titanium and titanium alloys make them widely used in chemical engineering, medicine, construction, aerospace and other engineering fields. However, with the advancement of technology, the service environment of components made of pure titanium or titanium alloys is becoming more and more complex.
[0003] From a thermodynamic point of view, the reaction between titanium and hydrogen is an exothermic reaction, that is, a spontaneous reaction. In a hydrogen environment, pure titanium or titanium alloy components will undergo a hydrogen absorption reaction, and the absorbed hydrogen atoms will form titanium hydride with titanium and distribute on the surface of the component. Titanium hydride significantly reduces the mechanical and chemical properties of the component and reduces its service life. In order to ensure the performance of the component, the titanium hydride on the surface of the component needs to be removed. The commonly used methods for removing titanium hydride on the surface of the component are currently high-temperature method, mechanical method and chemical method. The high-temperature method refers to heating the titanium component containing hydride to a high temperature in a certain environment to decompose the titanium hydride to achieve the purpose of removal, but the implementation conditions are harsh and the operation process is relatively cumbersome. The mechanical method refers to the use of mechanical friction to remove the surface titanium hydride, but this method is not applicable to pure titanium components with complex structures and narrow operating space. The chemical method is to use hydrofluoric acid or nitric acid to remove the titanium hydride on the surface by washing. This method is easy to operate and has no restrictions on the component structure, but the amount of surface removal is large and strong acid is required. For pure titanium components that are already in service, the method of using strong acid to remove a large amount of the surface layer will also cause certain harm to the components.
[0004] In view of the above situation, it is necessary to develop a method for removing titanium hydride from the surface of a component which is simple, effective and will not cause harm to the component. Summary of the invention
[0005] In view of this, the present invention provides a method for treating the surface of a titanium-based material. The treatment method provided by the present invention is simple and easy to operate, is not limited by the structure of the component, and will not cause harm to the titanium-based material component.
[0006] In order to solve the above technical problems, the present invention provides a method for treating the surface of a titanium-based material, comprising the following steps:
[0007] The titanium-based material containing titanium hydride on the surface is electrolyzed to obtain the titanium-based material except the titanium hydride; the electrolysis electrolyte is an alkaline electrolyte containing fluoride ions, the electrolysis voltage is 7 to 10V, and the current is 55 to 75A / dm 2 , electrolysis time is 5 to 45 seconds;
[0008] The titanium-based material without titanium hydride is anodized to obtain a titanium-based material with a protective layer on the surface; the voltage of the anodization is 15 to 20 V, and the current is 5 to 15 A / dm 2 , the oxidation time is 1 to 6 seconds.
[0009] Preferably, the electrolytic solution for electrolysis is a mixed aqueous solution of first sodium hydroxide and sodium fluoride.
[0010] Preferably, the molar concentration of sodium hydroxide in the first mixed aqueous solution of sodium hydroxide and sodium fluoride is 5 to 8 mol / L, and the molar concentration of sodium fluoride is 0.01 to 0.08 mol / L.
[0011] Preferably, the electrolysis process is accompanied by oscillation.
[0012] Preferably, the power of the oscillation is 3 to 50 kHz.
[0013] Preferably, the electrolyte for anodization includes a mixed aqueous solution of a second sodium hydroxide and sodium fluoride, a sodium carbonate solution, a sodium sulfate solution or a sodium nitrate solution.
[0014] Preferably, the molar concentration of sodium hydroxide in the second mixed aqueous solution of sodium hydroxide and sodium fluoride is 0.5-0.8 mol / L, and the molar concentration of sodium fluoride is 0.001-0.008 mol / L.
[0015] Preferably, the cathodes for electrolysis and anodic oxidation are inert electrodes respectively.
[0016] Preferably, the inert electrode comprises a platinum electrode, a carbon electrode or a stainless steel electrode.
[0017] Preferably, the titanium-based material includes a titanium component or a titanium alloy component.
[0018] The present invention provides a method for treating the surface of a titanium-based material, comprising the following steps: electrolyzing the titanium-based material containing titanium hydride on the surface to obtain the titanium-based material without titanium hydride; the electrolysis electrolyte is an alkaline electrolyte containing fluoride ions, the electrolysis voltage is 7 to 10V, and the current is 55 to 75A / dm 2 , the electrolysis time is 5 to 45 seconds; the titanium-based material without titanium hydride is anodized to obtain a titanium-based material with a protective layer on the surface; the voltage of the anodization is 15 to 20V, and the current is 5 to 15A / dm 2, the oxidation time is 1 to 6 seconds. In the present invention, titanium hydride reacts with hydroxide ions in the electrolyte under electrolysis conditions to generate amorphous titanium nanoparticles. Since fluorine ions in the electrolyte have a corrosive effect on titanium, they also inhibit the precipitation of Ti particles on the surface of the titanium matrix, thereby promoting the dispersion of titanium nanoparticles in the electrolyte. The present invention uses a high voltage and a small current form to perform anodization to oxidize the surface of the titanium-based material except for titanium hydride to generate a titanium dioxide protective film layer, thereby ensuring the performance of the titanium-based material and extending its service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is the XRD spectrum of the pure titanium component with titanium hydride on the surface to be treated in Example 1;
[0020] Figure 2 are optical micrographs of the pure titanium component before and after surface treatment in Example 1, wherein (a) is an optical micrograph of the pure titanium component before surface treatment, and (b) is an optical micrograph of the pure titanium component after surface treatment;
[0021] Figure 3 are optical micrographs of the pure titanium component before and after surface treatment in Example 2, wherein (a) is an optical micrograph of the pure titanium component before surface treatment, and (b) is an optical micrograph of the pure titanium component after surface treatment;
[0022] Figure 4 : are optical micrographs of the pure titanium component before and after surface treatment in Comparative Example 1, wherein (a) is an optical micrograph of the pure titanium component before surface treatment, and (b) is an optical micrograph of the pure titanium component after surface treatment;
[0023] Figure 5 These are optical microscope images of the pure titanium component before and after surface treatment in Comparative Example 2, wherein (a) is the optical microscope image of the pure titanium component before surface treatment, and (b) is the optical microscope image of the pure titanium component after surface treatment. DETAILED DESCRIPTION
[0024] The present invention provides a method for treating the surface of a titanium-based material, comprising the following steps:
[0025] The titanium-based material containing titanium hydride on the surface is electrolyzed to obtain the titanium-based material except the titanium hydride; the electrolysis electrolyte is an alkaline electrolyte containing fluoride ions, the electrolysis voltage is 7 to 10V, and the current is 55 to 75A / dm 2 , electrolysis time is 5 to 45 seconds;
[0026] The titanium-based material without titanium hydride is anodized to obtain a titanium-based material with a protective layer on the surface; the voltage of the anodization is 15 to 20 V, and the current is 5 to 15 A / dm 2 , the oxidation time is 1 to 6 seconds.
[0027] The present invention electrolyzes a titanium-based material containing titanium hydride on its surface to obtain a titanium-based material except for titanium hydride. In the present invention, the titanium-based material preferably includes a titanium component or a titanium alloy component, and more preferably a titanium component. In the present invention, the titanium component is preferably a component prepared from titanium metal. In the present invention, the titanium hydride is preferably TiH x , where x is preferably 1.5 or 2.
[0028] The present invention preferably uses a titanium-based material containing titanium hydride on the surface as the anode for electrolysis; the cathode for electrolysis is preferably an inert electrode; the inert electrode preferably includes a platinum electrode, a carbon electrode or a stainless steel electrode, and is more preferably a platinum electrode. In the present invention, the inert electrode is preferably a sheet electrode or a mesh electrode.
[0029] In the present invention, the electrolytic solution is an alkaline electrolyte containing fluoride ions, preferably a mixed aqueous solution of first sodium hydroxide and sodium fluoride. In the present invention, the molar concentration of sodium hydroxide in the mixed aqueous solution of the first sodium hydroxide and sodium fluoride is preferably 5-8 mol / L, more preferably 6-7 mol / L; the molar concentration of sodium fluoride in the mixed aqueous solution of the first sodium hydroxide and sodium fluoride is preferably 0.01-0.08 mol / L, more preferably 0.02-0.06 mol / L. In the present invention, the voltage of the electrolysis is 7-10V, preferably 8-10V; the current of the electrolysis is preferably 55-75A / dm 2 , more preferably 65 to 75 A / dm 2 The electrolysis time is preferably 5 to 45 seconds, more preferably 35 to 45 seconds; the electrolysis temperature is preferably 20 to 30° C., more preferably 23 to 25° C. The present invention uses low voltage and high current for electrolysis to quickly remove titanium hydride.
[0030] In the present invention, a chemical reaction as shown in Formula 1 occurs during the electrolysis process:
[0031] TiHx+xOH-→Ti+xH2O+xe - Formula 1.
[0032] In the present invention, the electrolysis process is preferably accompanied by oscillation, and the power of the oscillation is preferably 3 to 50 kHz, more preferably 30 to 50 kHz. Under the action of oscillation, the present invention can disperse the titanium particles generated by electrolysis into the electrolyte to avoid deposition on the surface of the titanium-based material.
[0033] After obtaining the titanium-hydride-free titanium-based material, the present invention performs anodization on the titanium-hydride-free titanium-based material to obtain a titanium-based material having a protective layer on the surface. The present invention preferably uses the titanium-hydride-free titanium-based material as the anode for anodization; the anodization cathode is preferably an inert electrode; the inert electrode preferably includes a platinum electrode, a carbon electrode or a stainless steel electrode, and is more preferably a platinum electrode.
[0034] In the present invention, the electrolyte for anodization preferably includes a mixed aqueous solution of a second sodium hydroxide and sodium fluoride, a sodium carbonate solution, a sodium sulfate solution or a sodium nitrate solution, and is more preferably a mixed aqueous solution of a second sodium hydroxide and sodium fluoride. In the present invention, the molar concentration of sodium hydroxide in the second mixed aqueous solution of sodium hydroxide and sodium fluoride is preferably 0.5-0.8 mol / L, and is more preferably 0.6-0.7 mol / L; the molar concentration of sodium fluoride in the second mixed aqueous solution of sodium hydroxide and sodium fluoride is preferably 0.001-0.008 mol / L, and is more preferably 0.002-0.006 mol / L. In the present invention, the voltage of the anodization is 15-20 V, and is preferably 16-18 V; the current of the anodization is 5-15 A / dm 2 , preferably 5 to 10 A / dm 2 or 10~15A / dm 2 The anodic oxidation time is 1 to 6 seconds, preferably 2 to 5 seconds; the anodic oxidation temperature is preferably 20 to 30° C., more preferably 23 to 25° C. The present invention adopts high voltage and low current to carry out anodic oxidation, which can accelerate the surface oxidation rate, achieve oxidation in a short time and avoid overoxidation.
[0035] The present invention generates a titanium dioxide protective film layer on the surface of the titanium-based material except titanium hydride through anodization. The present invention controls the thickness of the protective film layer by regulating the anodization time. When the anodization time is greater than 5s, the generated protective film layer will show color.
[0036] Due to TiH x The chemical activity of TiH is higher than that of TiO2. Under electrolytic conditions, x It preferentially reacts with OH- in the electrolyte to generate amorphous nano-sized Ti particles. Applying ultrasonic vibration in the electrolytic cell will disperse the generated nano-sized Ti particles into the electrolyte. Since F- has a corrosive effect on titanium, it will also inhibit the Ti particles from settling into the matrix. As time goes by, TiHx is gradually consumed, while TiO2 is consumed less. When TiH x After the removal is complete, the ultrasonic oscillation is stopped. In order to quickly oxidize the area where the titanium hydride has been removed, anodization is performed in the form of high voltage and low current to quickly oxidize the surface of the material to form an oxide film, thereby ensuring the performance of the material and extending its service life.
[0037] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0038] Since it is difficult to control the voltage and current to specific values during actual operation and they will fluctuate within a certain range, the values of the voltage and current in the embodiment are range values.
[0039] Example 1
[0040] The pure titanium component with titanium hydride on the surface to be treated is connected to a DC power supply as an anode, an inert electrode Pt sheet as a cathode, and a mixed solution of NaOH and NaF as an electrolyte, wherein the molar concentration of NaOH in the electrolyte is 7 mol / L and the molar concentration of NaF is 0.08 mol / L; the DC power supply is turned on, the voltage is adjusted to 8-10 V, and the current is adjusted to 65-75 A / dm 2 , electrolyzed at 25°C (accompanied by 45kHz oscillation) for 40s to obtain a pure titanium component except for titanium hydride;
[0041] The titanium hydride-free pure titanium component is used as the anode, the inert electrode Pt sheet is used as the cathode, and the mixed solution of NaOH and NaF is used as the electrolyte. The molar concentration of NaOH in the electrolyte is 0.7 mol / L, and the molar concentration of NaF is 0.008 mol / L. A DC power supply is connected, and the voltage is adjusted to 15-20 V and the current is 5-10 A / dm 2 , and anodized for 2s at 25°C to obtain a pure titanium component with a protective layer on the surface.
[0042] Example 2
[0043] The pure titanium component with titanium hydride on the surface to be treated is connected to a DC power supply as an anode, an inert electrode Pt sheet as a cathode, and a mixed solution of NaOH and NaF as an electrolyte, wherein the molar concentration of NaOH in the electrolyte is 8 mol / L and the molar concentration of NaF is 0.05 mol / L; the DC power supply is turned on, the voltage is adjusted to 8-10 V, and the current is adjusted to 65-75 A / dm 2 , electrolyzed at 25°C (accompanied by 40kHz oscillation) for 45s to obtain a pure titanium component except for titanium hydride;
[0044] The titanium hydride-free pure titanium component is used as the anode, the inert electrode Pt sheet is used as the cathode, and the mixed solution of NaOH and NaF is used as the electrolyte. The molar concentration of NaOH in the electrolyte is 0.8 mol / L, and the molar concentration of NaF is 0.005 mol / L. A DC power supply is connected, and the voltage is adjusted to 15-20 V and the current is 10-15 A / dm 2 , and anodized for 6s at 25°C to obtain a pure titanium component with a protective layer on the surface.
[0045] Comparative Example 1
[0046] The pure titanium component with titanium hydride on the surface to be treated is connected to a DC power supply as an anode, an inert electrode Pt sheet as a cathode, and a mixed solution of NaOH and NaF as an electrolyte, wherein the molar concentration of NaOH in the electrolyte is 6 mol / L and the molar concentration of NaF is 0.04 mol / L; the DC power supply is turned on, the voltage is adjusted to 4-5 V, and the current is adjusted to 30-40 A / dm 2 , electrolyzed at 25°C (accompanied by 45kHz oscillation) for 40s to obtain a treated pure titanium component.
[0047] Comparative Example 2
[0048] The pure titanium component with titanium hydride on the surface to be treated is connected to a DC power supply as an anode, an inert electrode Pt sheet as a cathode, and a mixed solution of NaOH and NaF as an electrolyte, wherein the molar concentration of NaOH in the electrolyte is 7 mol / L and the molar concentration of NaF is 0.06 mol / L; the DC power supply is turned on, the voltage is adjusted to 7-8 V, and the current is adjusted to 65-75 A / dm 2 , electrolyzed at 25°C (accompanied by 45kHz oscillation) for 40s to obtain a treated pure titanium component.
[0049] The surface of the pure titanium component to be treated in Example 1 containing titanium hydride is subjected to X-ray diffraction detection to obtain an XRD spectrum, as shown in FIG. Figure 1 As shown. Figure 1 It can be seen that the surface of the pure titanium component to be treated contains titanium hydride. 1.5 of titanium hydride.
[0050] The pure titanium components before and after the surface treatment in Examples 1 to 2 and Comparative Examples 1 to 2 were examined using an optical microscope to obtain optical microscope images, as shown in FIG. Figures 2 to 5 As shown, Figure 2 is the optical microscope image of Example 1, Figure 3 is the optical microscope image of Example 2, Figure 4 This is the optical microscope image of Comparative Example 1. Figure 5 2 are optical microscope images of comparative example 2; wherein (a) is an optical microscope image of a pure titanium component before surface treatment, and (b) is an optical microscope image of a pure titanium component after surface treatment.
[0051] Depend on Figure 2 It can be seen that the titanium hydride on the surface of the pure titanium component can be removed by electrolysis according to the conditions of Example 1, and the titanium hydride is basically removed; an oxide layer (thin thickness) is generated on the surface after anodization, and no color appears.
[0052] Depend on Figure 3It can be seen that the titanium hydride on the surface of the pure titanium component can be removed by electrolysis according to the conditions of Example 2, and it is basically completely removed; after anodization, a TiO2 oxide layer (thicker) is generated on the surface, and color appears locally.
[0053] Figure 4 From (a), it can be seen that the surface of the sample is titanium hydride but it does not completely cover the surface of the pure titanium component, and contains part of titanium dioxide (wherein the dark area is titanium hydride and the light area is the uncovered pure titanium component); Figure 4 It can be seen in (b) that the titanium hydride on the surface of the pure titanium component can be partially removed according to the conditions of Comparative Example 1, but due to the low voltage and large current, most of the titanium hydride on the surface of the pure titanium component is not removed, and the exposed titanium oxide layer becomes thicker and appears colored.
[0054] Depend on Figure 5 It can be seen that the titanium hydride on the surface of the pure titanium component can be removed by electrolysis according to the conditions of Comparative Example 2, but since no anodization is performed, no titanium dioxide coverage occurs.
[0055] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for treating the surface of a titanium-based material, It is characterized in that The following steps are involved: The titanium-based material containing titanium hydride on the surface is electrolyzed to obtain the titanium-based material except the titanium hydride; the electrolysis electrolyte is an alkaline electrolyte containing fluoride ions, the electrolysis voltage is 7 to 10V, and the current is 55 to 75A / dm 2 , electrolysis time is 5 to 45 seconds; The titanium-based material without titanium hydride is anodized to obtain a titanium-based material with a protective layer on the surface; the voltage of the anodization is 15 to 20 V, and the current is 5 to 15 A / dm 2 , the oxidation time is 1 to 6 seconds.
2. The method for treating the surface of a titanium-based material according to claim 1, It is characterized in that The electrolytic solution for electrolysis is a mixed aqueous solution of first sodium hydroxide and sodium fluoride.
3. The method for treating the surface of a titanium-based material according to claim 2, It is characterized in that The molar concentration of sodium hydroxide in the first mixed aqueous solution of sodium hydroxide and sodium fluoride is 5-8 mol / L, and the molar concentration of sodium fluoride is 0.01-0.08 mol / L.
4. The method for treating the surface of a titanium-based material according to claim 1, It is characterized in that The electrolysis process is accompanied by oscillation.
5. The method for treating the surface of a titanium-based material according to claim 4, It is characterized in that The power of the oscillation is 3 to 50 kHz.
6. The method for treating the surface of a titanium-based material according to claim 1, It is characterized in that The electrolyte for anodizing includes a mixed aqueous solution of a second sodium hydroxide and sodium fluoride, a sodium carbonate solution, a sodium sulfate solution or a sodium nitrate solution.
7. The method for treating the surface of a titanium-based material according to claim 6, It is characterized in that The molar concentration of sodium hydroxide in the second mixed aqueous solution of sodium hydroxide and sodium fluoride is 0.5-0.8 mol / L, and the molar concentration of sodium fluoride is 0.001-0.008 mol / L.
8. The method for treating the surface of a titanium-based material according to claim 1, It is characterized in that The cathodes for electrolysis and anodic oxidation are respectively inert electrodes.
9. The method for treating the surface of a titanium-based material according to claim 8, It is characterized in that The inert electrode includes a platinum electrode, a carbon electrode or a stainless steel electrode.
10. The method for treating the surface of a titanium-based material according to claim 1, It is characterized in that The titanium-based material includes a titanium component or a titanium alloy component.