Single crystal thin film wafer structure and preparation method
By adjusting the Euler angle and ion implantation conditions of the monocrystalline thin film wafer, and combining the use of amorphous and polycrystalline thin film layers, the problem of void defects in the bonding process was solved, thereby improving the bonding yield and the quality and reliability of components.
Patent Information
- Application Number
- CN202410955783.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-05
AI Technical Summary
Existing technologies are prone to void defects during the bonding process of heterogeneous thin film materials, resulting in low bonding yield and affecting the performance and reliability of semiconductor chips.
By employing a single-crystal thin-film wafer structure and adjusting the Euler angle and ion implantation conditions of the single-crystal thin-film layer, the single-crystal wafer first contacts the midpoint of the substrate layer during the bonding process and then gradually expands. Combined with the use of amorphous and polycrystalline thin-film layers, stress distribution and mechanical support are optimized.
It improves bonding yield, enhances the morphology of single-crystal thin-film wafer structures and the quality and reliability of related components, and ensures complete bonding without voids.
Smart Images

Figure CN118895559A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a single crystal thin film wafer structure and a preparation method thereof. Background Art
[0002] The integration technology of heterogeneous materials plays a significant role in enhancing the performance of semiconductor chips and improving their integration. In the semiconductor industry, achieving efficient integration of different materials is a key step in manufacturing advanced chips. At present, the conventional practice for producing wafers of heterogeneous thin film materials is to use bonding technology to transfer the required material layer to a silicon substrate or other types of substrates. Although this technology plays an important role in integrating different functional layers, defects such as holes may appear during the bonding process. These problems will reduce the yield of bonding, thus posing a challenge to the performance and reliability of the final product. Therefore, there is an urgent need for an improved single-crystal thin-film wafer structure to improve the bonding yield and enhance the performance of components based on single-crystal thin-film wafer structures. Summary of the invention
[0003] In order to solve the above technical problems, the present application proposes a single crystal thin film wafer structure and a preparation method.
[0004] On the one hand, an embodiment of the present application provides a single crystal thin film wafer structure, including:
[0005] substrate layer;
[0006] A single crystal thin film layer, wherein the single crystal thin film layer is located on the surface of the substrate layer;
[0007] The precession angle of the Euler angle of the single crystal thin film layer is 0, the nutation angle is θ±n*180°, the precession angle is 0, the value range of θ is -90°~-20°, and n is a positive integer;
[0008] Among them, the single crystal thin film layer is a single crystal wafer that has been ion implanted; when the single crystal wafer is ion implanted under the same conditions, the curvature change is a positive value; the curvature change of the single crystal wafer is inversely proportional to the θ value of the Euler angle of the single crystal wafer.
[0009] Furthermore, the single crystal thin film wafer structure also includes:
[0010] The amorphous thin film layer is arranged between the substrate layer and the single crystal thin film layer.
[0011] Furthermore, the single crystal thin film wafer structure also includes:
[0012] The polycrystalline thin film layer is arranged between the amorphous thin film layer and the substrate layer.
[0013] Furthermore, the same conditions include: the same implantation energy, the same implantation dose and the same ion species.
[0014] Furthermore, the implantation depth corresponding to the implantation energy is less than the thickness of the single crystal wafer.
[0015] Furthermore, the implantation depth corresponding to the implantation energy is less than the thickness of the single crystal wafer.
[0016] On the other hand, an embodiment of the present application further provides a method for preparing a single crystal thin film wafer structure, the method comprising:
[0017] Providing a substrate layer and a single crystal wafer;
[0018] Performing ion implantation on the single crystal wafer to form a single crystal wafer with a damaged layer;
[0019] bonding a single crystal wafer with a damaged layer to a substrate layer to obtain a bonding structure;
[0020] The bonded structure is processed to obtain a single crystal thin film wafer structure.
[0021] Furthermore, the bonding structure is processed as described above to obtain a single crystal thin film wafer structure, including:
[0022] Annealing the bonded structure to peel off the bonded structure along the damaged layer to obtain an initial single crystal thin film wafer structure;
[0023] The initial single crystal thin film wafer structure is subjected to post-annealing treatment and flattening treatment to obtain a single crystal thin film wafer structure.
[0024] Furthermore, the above-mentioned ion implantation into the single crystal wafer includes:
[0025] When ion implantation is performed on a single crystal wafer, when the conditions of the ion implantation are the same, the single crystal wafer bends, and the change in curvature is a positive value; the change in curvature of the single crystal wafer is inversely proportional to the θ value of the Euler angle of the single crystal wafer.
[0026] Furthermore, the above method also includes:
[0027] forming a polycrystalline thin film layer on a surface of the substrate layer;
[0028] An amorphous thin film layer is formed on a surface of the polycrystalline thin film layer away from the substrate layer.
[0029] By adopting the above technical solution, the single crystal thin film wafer structure provided by the present application has the following beneficial effects:
[0030] The present application discloses a single crystal thin film wafer structure and a preparation method thereof, wherein the single crystal thin film wafer structure comprises a substrate layer and a single crystal thin film layer, wherein the single crystal thin film layer is located on the surface of the substrate layer; the precession angle of the Euler angle of the single crystal thin film layer is 0, the nutation angle is θ±n*180°, the precession angle is 0, the value range of θ is -90°~-20°, and n is a positive integer; wherein the single crystal thin film layer is a single crystal wafer implanted with ions; when the single crystal wafer is implanted with the same ions under the same conditions, the curvature change is a positive value; the curvature change of the single crystal wafer is inversely proportional to the θ value of the Euler angle of the single crystal wafer. The present application realizes that the wafer contacts the middle point of the substrate layer first during the bonding process, thereby improving the bonding yield; at the same time, the curvature change of the wafer can be adjusted by adjusting the Euler angle of the single crystal thin film layer, thereby improving the wafer morphology, which is beneficial to improving the quality and reliability of related components based on the single crystal thin film wafer structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions and advantages in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 A schematic diagram of a single crystal thin film wafer structure provided in an embodiment of the present application;
[0033] Figure 2 A schematic diagram of the definition of Euler angles provided in an embodiment of the present application;
[0034] Figure 3 A schematic diagram of the structural changes of a single crystal wafer after ion implantation provided in an embodiment of the present application;
[0035] Figure 4 A relationship diagram between the curvature change of a single crystal wafer and the Euler angle of the single crystal wafer provided in an embodiment of the present application;
[0036] Figure 5 A schematic structural diagram of an optional single crystal thin film wafer structure provided in an embodiment of the present application;
[0037] Figure 6 A schematic diagram of a process for preparing a single crystal thin film wafer structure provided in an embodiment of the present application;
[0038] Figure 7 A schematic diagram of a method for preparing a single crystal thin film wafer structure provided in an embodiment of the present application;
[0039] Figure 8A schematic diagram of an optional method for preparing a single crystal thin film wafer structure provided in an embodiment of the present application;
[0040] Fig. 9 Schematic diagram of the preparation method of the polycrystalline thin film layer and the amorphous thin film layer provided in the embodiment of the present application.
[0041] The following is a supplementary description of the attached drawings:
[0042] 100 - substrate layer; 200 - single crystal thin film layer; 300 - polycrystalline thin film layer; 400 - amorphous thin film layer; 500 - damaged layer. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0044] It should be noted that the terms "first", "second", etc. in the specification and claims of the embodiment of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the embodiment of the present application described here can be implemented in an order other than those illustrated or described here. Thus, the features defined as "first" and "second" can expressly or implicitly include one or more of the features. In the description of the present embodiment, unless otherwise specified, the meaning of "multiple" is two or more. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or server comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0045] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the invention are approximations, the numerical values set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0046] When a numerical range is disclosed herein, the above range is deemed to be continuous and includes the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all sub-ranges included therein. For example, a specified range from "1 to 10" should be deemed to include any and all sub-ranges between a minimum of 1 and a maximum of 10. Exemplary sub-ranges of ranges 1 to 10 include, but are not limited to, 1 to 6.1, 3.5 to 7.8, 5.5 to 10, etc.
[0047] Please refer to Figure 1 , Figure 1 A schematic diagram of a single crystal thin film wafer structure provided in an embodiment of the present application. The present application discloses a single crystal thin film wafer structure, comprising: a substrate layer 100 and a single crystal thin film layer 200, wherein the single crystal thin film layer 200 is located on the surface of the substrate layer 100; the precession angle of the Euler angle of the single crystal thin film layer 200 is 0, the nutation angle is θ±n*180°, the precession angle is 0, the value range of θ is -90° to -20°, and n is a positive integer; wherein, when the single crystal wafer corresponding to the single crystal thin film layer 200 is ion-implanted under the same conditions, the curvature change is a positive value; the curvature change of the single crystal wafer is inversely proportional to the value of θ of the Euler angle of the single crystal wafer.
[0048] For example, the Euler angle refers to a set of three independent angular parameters used to determine the position of a fixed-point rotating rigid body, consisting of the nutation angle θ, the precession angle (i.e., the precession angle) α, and the rotation angle β, expressed as the Euler angle (α, θ, β). Figure 2 As shown in the figure, the angles of the Euler angles (α, θ, β) correspond to the angles of rotation around the coordinate axis ZXZ, where (0, θ, 0) is the rotation of the plate axis around the X axis by a certain angle; counterclockwise rotation is positive and clockwise rotation is negative. For example, (0, -36, 0) is the rotation of the plate 36° clockwise around the X axis.
[0049] Bow (BOW) refers to the deviation between the minimum and maximum values of the center point of the wafer surface from the reference plane when the wafer is not in close contact. The deviation includes concave and convex shapes. The concave bow is a negative value, and the convex bow is a positive value. It is generally expressed in microns (μm), and the general expression is: -15~15μm.
[0050] The precession angle of the Euler angle of the single crystal thin film layer 200 of the embodiment of the present application is 0, the nutation angle is θ±n*180°, the precession angle is 0, the value range of θ is -90° to -20°, and n is a positive integer; wherein the single crystal thin film layer 200 is a single crystal wafer that has been ion-implanted, and the structural changes of the single crystal wafer that has been ion-implanted in advance are as follows: Figure 3 shown.
[0051] like Figure 4 As shown, when the single crystal wafer corresponding to the single crystal thin film layer 200 is ion-implanted under the same conditions, the curvature change is positive; the curvature change of the single crystal wafer is inversely proportional to the θ value of the Euler angle of the single crystal wafer. That is, the Bow value change of the single crystal wafer decreases as the Euler angle of the single crystal wafer increases.
[0052] The single crystal thin film wafer structure is formed by bonding the ion-implanted single crystal wafer to the substrate layer 100. Figure 3 As shown, after the single crystal wafer is ion implanted, it presents a certain curvature. At this time, the single crystal wafer is bonded to the substrate layer 100. The middle point of the single crystal wafer and the substrate layer 100 first contacts and then gradually expands to the surrounding areas, thereby ensuring that the bonding is complete and free of holes, thereby improving the bonding yield.
[0053] It should be noted that the change in curvature of the single crystal wafer structure corresponding to the above single crystal film is inversely proportional to the value of the Euler angle θ of the single crystal film layer 200, and is applicable when the thickness of the single crystal wafer is the same.
[0054] Optionally, the material of the single crystal thin film layer 200 is at least one of lithium niobate and lithium tantalate.
[0055] Optionally, the material of the substrate layer 100 includes but is not limited to at least one of Si, sapphire, quartz, and SiC.
[0056] Optionally, the thickness of the single crystal thin film layer 200 is 300 nm-20000 nm.
[0057] The present application discloses a single crystal thin film wafer structure and a preparation method thereof, wherein the single crystal thin film wafer structure comprises a substrate layer 100 and a single crystal thin film layer 200, wherein the single crystal thin film layer 200 is located on the surface of the substrate layer 100; the precession angle of the Euler angle of the single crystal thin film layer 200 is 0, the nutation angle is θ±n*180°, the precession angle is 0, the value range of θ is -90° to -20°, and n is a positive integer; wherein the single crystal thin film layer 200 is a single crystal wafer that has been ion implanted; when the single crystal wafer is implanted with the same ions under the same conditions, the curvature change is a positive value; the curvature change of the single crystal wafer is inversely proportional to the θ value of the Euler angle of the single crystal wafer. The present application realizes that during the bonding process, the wafer first contacts the middle point of the substrate layer 100 and then gradually expands to the surrounding areas, thereby ensuring that the bonding is complete and free of holes, thereby improving the bonding yield; at the same time, the curvature of the wafer can be adjusted by adjusting the Euler angle of the single crystal thin film layer 200, thereby improving the wafer morphology, which is beneficial to improving the quality and reliability of related components based on the single crystal thin film wafer structure.
[0058] As an optional implementation, the single crystal thin film wafer structure further includes: an amorphous thin film layer 400 , wherein the amorphous thin film layer 400 is disposed between the substrate layer 100 and the single crystal thin film layer 200 .
[0059] As an optional implementation, the single crystal thin film wafer structure further includes: a polycrystalline thin film layer 300 , and the polycrystalline thin film layer 300 is disposed between the amorphous thin film layer 400 and the substrate layer 100 .
[0060] For example, Figure 5 As shown, in some application scenarios, the single crystal thin film wafer structure further includes: an amorphous thin film layer 400 and a polycrystalline thin film layer 300, the polycrystalline thin film layer 300 is arranged on the surface of the substrate layer 100, the amorphous thin film layer 400 is arranged on the surface of the polycrystalline thin film layer 300 away from the substrate layer 100, and then the single crystal thin film layer 200 is arranged on the surface of the amorphous thin film layer 400 away from the substrate layer 100. That is, the single crystal thin film wafer structure is respectively a single crystal thin film layer 200, an amorphous thin film layer 400, a polycrystalline thin film layer 300 and a substrate layer 100 from top to bottom.
[0061] Optionally, the material of the amorphous thin film layer 400 includes but is not limited to at least one of SiO2, SiN and the like.
[0062] Optionally, the thickness of the amorphous thin film layer 400 is 100-15000 nm.
[0063] Optionally, the functions of the amorphous film layer 400 include but are not limited to acting as a buffer layer to reduce the stress difference between the single crystal film layer 200 and the polycrystalline film layer 300 or the substrate layer 100, thereby preventing cracks or peeling due to mismatch in thermal expansion coefficients; the amorphous film layer can provide protection to prevent the single crystal film layer from chemical corrosion or physical damage; the amorphous film layer can affect the stress distribution of the entire structure through its own stress state, which helps to optimize performance; provide certain mechanical support to enhance the stability of the overall structure, etc.
[0064] Optionally, the material of the polycrystalline thin film layer 300 is a polycrystalline silicon layer.
[0065] Optionally, the thickness of the polycrystalline thin film layer 300 is 300-2000 nm.
[0066] Optionally, the polysilicon layer can provide additional mechanical support to enhance the stability and durability of the overall structure; polysilicon has a high thermal conductivity, which can help dissipate heat to a certain extent and has a positive effect on maintaining the thermal stability of the device; polysilicon can provide chemical stability, etc.
[0067] The embodiment of the present application discloses another structure of a single crystal thin film wafer structure, that is, the single crystal thin film wafer structure comprises a single crystal thin film layer 200, an amorphous thin film layer 400, a polycrystalline thin film layer 300 and a substrate from top to bottom. The amorphous thin film layer 400 provides buffering, protection, support and other functions, thereby improving the material stability of the single crystal thin film wafer structure, that is, ensuring the stability of the single crystal thin film wafer structure, and further improving the bonding yield.
[0068] As an optional implementation, the above same conditions include: the same implantation energy, the same implantation dose and the same ion species.
[0069] As an optional implementation, the above-mentioned ions are at least one of H ions and He ions.
[0070] As an optional implementation, the implantation depth corresponding to the implantation energy is less than the thickness of the single crystal wafer.
[0071] For example, the implantation energy refers to the maximum energy that the implanted ions reach in the wafer during the ion implantation process. The implantation depth refers to the depth to which the ions penetrate into the wafer material, while the thickness of a single crystal wafer refers to the physical thickness of the wafer.
[0072] The implantation depth corresponding to the implantation energy is less than the thickness of the single crystal wafer, which means that the depth of penetration of the ions in the wafer does not reach the bottom of the wafer.
[0073] It should be noted that, in practical applications, the specific conditions for ion implantation are not limited in this application and can be the same as those in the prior art.
[0074] In an embodiment of the present application, a single crystal wafer that has undergone ion implantation is bonded to a substrate layer 100. Since the curvature of the single crystal wafer that has undergone ion implantation changes to a positive value and the curvature can be regulated according to the value of its Euler angle, the controllability of the material is improved, the bonding yield is improved, and the morphology of the single crystal thin film wafer structure is improved, which is beneficial to improving the quality and reliability of related components based on the single crystal thin film wafer structure.
[0075] On the other hand, the present application provides a method for preparing a single crystal thin film wafer structure, such as Figure 6 As shown, the method includes:
[0076] S10: providing a substrate layer 100 and a single crystal wafer.
[0077] Optionally, the material of the single crystal wafer is at least one of lithium niobate and lithium tantalate.
[0078] Optionally, the material of the substrate layer 100 includes but is not limited to at least one of Si, sapphire, quartz, and SiC.
[0079] Optionally, the thickness of the single crystal wafer is 300nm-20000nm.
[0080] The precession angle of the Euler angle of the single crystal thin film layer 200 in the embodiment of the present application is 0, the nutation angle is θ±n*180°, the precession angle is 0, the value range of θ is -90° to -20°, and n is a positive integer.
[0081] It should be noted that, in practical applications, the method and conditions for obtaining the substrate layer 100 may be the same as those in the prior art, and this application does not impose any limitation thereto.
[0082] S30 : performing ion implantation on the single crystal wafer to form a single crystal wafer with a damaged layer 500 .
[0083] For example, Figure 7 As shown, ion implantation is performed on a single crystal wafer to form a damaged layer 500 formed after ion implantation in the single crystal wafer. Optionally, ion implantation refers to gas ion implantation, and the type of the implanted gas ions is at least one of hydrogen ions, helium ions, or argon ions. The depth of ion implantation is less than the thickness of the single crystal wafer.
[0084] After the single crystal wafer is ion implanted, the curvature changes to a positive value, and the curvature change is inversely proportional to the θ value of the Euler angle of the single crystal wafer. That is, the Bow value change of the single crystal wafer decreases as the Euler angle of the single crystal wafer increases.
[0085] S50: Bonding the single crystal wafer with the damaged layer 500 to the substrate layer 100 to obtain a bonding structure.
[0086] Alternatively, if Figure 7 As shown, the structure bonded to the single crystal wafer here may be the substrate layer 100; or Figure 8 The substrate layer 100 is shown with an amorphous thin film layer 400 and a polycrystalline thin film layer 300 deposited thereon.
[0087] In practical applications, the bonding method and conditions may be the same as those in the prior art, and this application does not impose any limitation thereto.
[0088] S70: Processing the bonded structure to obtain a single crystal thin film wafer structure.
[0089] Exemplarily, the method of processing the bonding structure includes but is not limited to annealing treatment, planarization treatment, etc.
[0090] The embodiment of the present application discloses a method for preparing a single crystal thin film wafer structure, which includes a substrate layer 100 and a single crystal thin film layer 200, wherein the single crystal thin film layer 200 is located on the surface of the substrate layer 100; the precession angle of the Euler angle of the single crystal thin film layer 200 is 0, the nutation angle is θ±n*180°, the precession angle is 0, the value range of θ is -90° to -20°, and n is a positive integer; when the single crystal wafer is implanted with different ions under the same conditions, the curvature change is a positive value; the curvature change of the single crystal wafer is inversely proportional to the θ value of the Euler angle of the single crystal wafer. The above method is used to achieve that during the bonding process, the wafer first contacts the middle point of the substrate layer 100 and then gradually expands to the surrounding areas, thereby ensuring that the bonding structure is complete and free of holes, thereby improving the bonding yield; at the same time, the curvature of the single crystal wafer can be adjusted by adjusting the Euler angle of the single crystal wafer, thereby improving the morphology of the single crystal wafer, which is beneficial to improving the quality and reliability of related components based on the single crystal thin film wafer structure.
[0091] As an optional implementation, Figure 7 As shown, in the above step S70, the bonding structure is processed to obtain a single crystal thin film wafer structure, including:
[0092] S71: performing annealing treatment on the bonding structure so as to peel off the bonding structure along the damaged layer 500 to obtain an initial single crystal thin film wafer structure.
[0093] It should be noted that the single crystal wafer separated here can be reused, and the annealing conditions are not limited in this application.
[0094] S72: performing post-annealing and planarization treatment on the initial single crystal thin film wafer structure to obtain a single crystal thin film wafer structure.
[0095] Optionally, the planarization process includes but is not limited to chemical mechanical polishing, etch back, etch-back, etc., preferably chemical mechanical polishing.
[0096] The embodiment of the present application processes the single crystal thin film layer 200 of the bonding structure through the above-mentioned method to obtain a single crystal thin film wafer structure, which makes the surface of the single crystal thin film wafer structure flatter and smoother, helps to ensure the morphology of the single crystal thin film wafer structure, and is beneficial to improving the quality and reliability of related components based on the single crystal thin film wafer structure.
[0097] As an optional implementation, ion implantation is performed on a single crystal wafer, including:
[0098] When ion implantation is performed on a single crystal wafer, when the conditions of the ion implantation are the same, the single crystal wafer bends, and the change in curvature is a positive value; the change in curvature of the single crystal wafer is inversely proportional to the θ value of the Euler angle of the single crystal wafer.
[0099] Optionally, the above-mentioned same conditions include: the same implantation energy, the same implantation dose and the same ion type, and the above-mentioned ions are at least one of H ions and He ions.
[0100] It should be noted that the change in curvature of the single crystal thin film wafer structure is inversely proportional to the value of θ of the Euler angle of the single crystal thin film layer 200 when the thickness of the single crystal thin film layer 200 is the same.
[0101] As an optional implementation, after the above step S10, as Fig. 9 As shown, the above method also includes:
[0102] S11 : forming a polycrystalline thin film layer 300 on the surface of the substrate layer 100 .
[0103] Optionally, the method of preparing the polycrystalline thin film layer 300 on the surface of the substrate layer 100 includes but is not limited to LPCVD, PECVD, etc.
[0104] Optionally, the material of the polycrystalline thin film layer 300 is a polycrystalline silicon layer.
[0105] Optionally, the thickness of the polycrystalline thin film layer 300 is 300-2000 nm.
[0106] Optionally, the polysilicon layer can provide additional mechanical support to enhance the stability and durability of the overall structure; polysilicon has a high thermal conductivity, which can help dissipate heat to a certain extent and has a positive effect on maintaining the thermal stability of the device; polysilicon can provide chemical stability, etc.
[0107] S12 : depositing an amorphous thin film layer 400 on a surface of the polycrystalline thin film layer 300 away from the substrate layer 100 .
[0108] Optionally, methods for depositing the polycrystalline thin film layer 300 on the surface of the amorphous thin film layer 400 away from the substrate layer 100 include but are not limited to low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition (PECVD), physical vapor deposition (PVD), thermal oxidation, etc.
[0109] Optionally, the material of the amorphous thin film layer 400 includes but is not limited to at least one of SiO2, SiN and the like.
[0110] Optionally, the thickness of the amorphous thin film layer 400 is 100-15000 nm.
[0111] Optionally, the functions of the amorphous thin film layer 400 include but are not limited to acting as a buffer layer to reduce the stress difference between the single crystal thin film layer 200 and the polycrystalline thin film layer 300 or the substrate layer 100, thereby preventing cracks or peeling due to mismatch in thermal expansion coefficients; the amorphous layer can provide protection to prevent the single crystal thin film layer from chemical corrosion or physical damage; the amorphous layer can affect the stress distribution of the entire structure through its own stress state, which helps to optimize the piezoelectric performance; provide certain mechanical support to enhance the stability of the overall structure, etc.
[0112] The embodiment of the present application discloses a method for preparing another structure of a single crystal thin film wafer structure, namely, a method for preparing an amorphous thin film layer 400 and a polycrystalline thin film layer 300 in a single crystal thin film wafer structure. The amorphous thin film layer 400 provides buffering, protection, support and other functions, and the polycrystalline thin film layer 300 ensures electrical conductivity, heat dissipation and chemical stability, thereby improving the material stability of the single crystal thin film wafer structure, that is, ensuring the stability of the single crystal thin film wafer structure, and further improving the bonding yield.
[0113] The above preparation method is described in detail below through specific examples.
[0114] Embodiment 1:
[0115] 1) providing a single crystal wafer, whose initial Bow value is 0, the Euler angle of the single crystal wafer is (0, -54°, 0), and providing a substrate layer 100;
[0116] 2) performing ion implantation on the above single crystal wafer, wherein the implanted ion species is H ion, the implantation energy is 120kev, the implantation dose is 6e16, and the Bow value of the single crystal wafer after implantation is 75um;
[0117] 3) Bonding the ion-implanted single crystal wafer and the substrate layer 100 to obtain a bonding structure; the substrate layer 100 is a single crystal silicon substrate, and a polycrystalline thin film layer 300 and an amorphous thin film layer 400 are prepared on the surface of the substrate layer 100; the polycrystalline thin film layer 300 is made of polycrystalline silicon with a thickness of 1 um, and the amorphous thin film layer 400 is made of SiO2 with a thickness of 0.5 um;
[0118] 4) Annealing the bonded structure to separate the single crystal wafer along the damaged layer 500 formed by the ion implantation to obtain an initial single crystal thin film wafer structure;
[0119] 5) Performing high temperature annealing and chemical mechanical polishing on the initial single crystal thin film wafer to obtain a single crystal thin film wafer structure.
[0120] Embodiment 2:
[0121] 1) providing a single crystal wafer, whose initial Bow value is 0, the Euler angle of the single crystal wafer is (0, -40°, 0), and providing a substrate layer 100;
[0122] 2) performing ion implantation on the above single crystal wafer, wherein the implanted ion species is H ion, the implantation energy is 120kev, the implantation dose is 6e16, and the Bow value of the single crystal wafer after implantation is 30um;
[0123] 3) Bonding the ion-implanted single crystal wafer and the substrate layer 100 to obtain a bonding structure; the substrate layer 100 is a single crystal silicon substrate, and a polycrystalline thin film layer 300 and an amorphous thin film layer 400 are prepared on the surface of the substrate layer 100; the polycrystalline thin film layer 300 is made of polycrystalline silicon with a thickness of 1 um, and the amorphous thin film layer 400 is made of SiO2 with a thickness of 0.5 um;
[0124] 4) Annealing the bonded structure to separate the single crystal wafer along the damaged layer 500 formed by the ion implantation to obtain an initial single crystal thin film wafer structure;
[0125] 5) Performing high temperature annealing and chemical mechanical polishing on the initial single crystal thin film wafer to obtain the single crystal thin film wafer structure.
[0126] The difference between Examples 1 and 2 is that the Euler angle of the single crystal wafer in Example 2 is greater than that in Example 1. Comparison between Example 1 and Example 2 reflects the material properties of the single crystal wafer: when ion implantation is performed on the single crystal wafer, when the conditions of the ion implantation are the same, the curvature change of the single crystal wafer is a positive value, and the curvature change of the single crystal wafer is inversely proportional to the θ value of the Euler angle of the single crystal wafer.
[0127] As can be seen from the above embodiments, the present invention uses ion implantation to make the single crystal wafer convex to one side of the bonding surface, so that the wafer starts to contact from the middle point during the bonding process and then gradually expands to the surrounding areas, thereby ensuring that the bonding structure is complete and free of holes, thereby improving the bonding yield. At the same time, the present invention can adjust the curvature of the wafer by selecting the size of the Euler angle of the single crystal wafer, thereby improving the wafer morphology, which is beneficial to improving the quality and reliability of related components based on the single crystal thin film wafer structure.
[0128] It should be noted that the above-mentioned sequence of the embodiments of the present application is for description only and does not represent the advantages and disadvantages of the embodiments. The above-mentioned specific embodiments of this specification are described. Other embodiments are within the scope of the attached claims. In some cases, the actions or steps recorded in the claims can be performed in an order different from that in the embodiments and still achieve the desired results. In addition, the processes depicted in the drawings do not necessarily require the specific order or continuous order shown to achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.
[0129] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0130] A person skilled in the art will understand that all or part of the steps to implement the above embodiments may be accomplished by hardware or by instructing the relevant hardware through a program, and the relevant program may be stored in a computer-readable storage medium, and the above-mentioned storage medium may be a read-only memory, a disk or an optical disk, etc.
[0131] In order to make the purpose, technical solution and advantages disclosed in the embodiments of the present application more clearly understood, the embodiments of the present application are further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the embodiments of the present application and are not used to limit the embodiments of the present application.
[0132] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A single crystal thin film wafer structure, characterized in that: include: A substrate layer (100); a single crystal thin film layer (200), the single crystal thin film layer (200) being located on the surface of the substrate layer (100); The precession angle of the Euler angle of the single crystal thin film layer (200) is 0, the nutation angle is θ±n*180°, the precession angle is 0, the value range of θ is -90° to -20°, and n is a positive integer; Wherein, when the single crystal wafer corresponding to the single crystal thin film layer (200) is subjected to ion implantation under the same conditions, the curvature change is a positive value; and the curvature change of the single crystal wafer is inversely proportional to the value of the Euler angle θ of the single crystal wafer.
2. The single crystal thin film wafer structure according to claim 1, characterized in that: The single crystal thin film wafer structure further comprises: An amorphous thin film layer (400), wherein the amorphous thin film layer (400) is disposed between the substrate layer (100) and the single crystal thin film layer (200).
3. The single crystal thin film wafer structure according to claim 2, characterized in that: The single crystal thin film wafer structure further comprises: A polycrystalline thin film layer (300), wherein the polycrystalline thin film layer (300) is disposed between the amorphous thin film layer (400) and the substrate layer (100).
4. The single crystal thin film wafer structure according to claim 1, characterized in that: The same conditions include: the same implantation energy, the same implantation dose and the same ion species.
5. The single crystal thin film wafer structure according to claim 1, characterized in that: The ions are at least one of H ions and He ions.
6. The single crystal thin film wafer structure according to claim 4, characterized in that: The implantation depth corresponding to the implantation energy is less than the thickness of the single crystal wafer.
7. A method for preparing a single crystal thin film wafer structure as claimed in claims 1 to 6, characterized in that: The method comprises: Providing a substrate layer (100) and a single crystal wafer; Performing ion implantation on the single crystal wafer to form a single crystal wafer with a damaged layer (500); Bonding the single crystal wafer with the damaged layer (500) to the substrate layer (100) to obtain a bonding structure; The bonding structure is processed to obtain a single crystal thin film wafer structure.
8. The method according to claim 7, characterized in that The step of processing the bonding structure to obtain a single crystal thin film wafer structure includes: Annealing the bonding structure so that the bonding structure is peeled off along the damaged layer (500) to obtain an initial single crystal thin film wafer structure; The initial single crystal thin film wafer structure is subjected to post-annealing treatment and planarization treatment to obtain the single crystal thin film wafer structure.
9. The method according to claim 7, characterized in that: The step of implanting ions into the single crystal wafer comprises: Ions are implanted into the single crystal wafer. When the conditions of the ion implantation are the same, the single crystal wafer bends, and the change in curvature is a positive value. The change in curvature of the single crystal wafer is inversely proportional to the value of θ of the Euler angle of the single crystal wafer.
10. The method according to claim 7, characterized in that The method further comprises: forming a polycrystalline thin film layer (300) on the surface of the substrate layer (100); An amorphous thin film layer (400) is formed on a surface of the polycrystalline thin film layer (300) away from the substrate layer (100).