Wool / cashmere / mohair covering yarn production process
Through fine raw material selection and process flow, combined with the use of different and wool emulsions, wool/cashmere/mohair core yarn with good strength and anti-flushing and pilling properties was successfully prepared, which solved the uniformity and consistent mixing of cashmere and mohair. The production of high-end textile materials has been realized.
Patent Information
- Application Number
- CN202410936421.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
How to mix cashmere and mohair into a core-encapsulated yarn with good uniformity, which not only utilizes the excellent appearance of cashmere and the high strength and pill resistance of mohair, but also solves the inconsistency between suede height and smoothness of hand, but also improves fibers elasticity and wear resistance.
Using specific raw material selection and process flow, including the preparation of worsted wool yarn, the wool mixing of cashmere and mohair, combing, striping, combed, striping and refueling, improve the smoothness of the fiber through the use of different wool emulsions and soft and made into wool/cashmere/mohair core yarn by the Sero core scribing process.
The prepared core-encapsulated yarn has good strength and anti-pilling properties, smoothness and softness, which improves the overall performance of the fiber and is suitable as a high-end textile material.
Abstract
Description
Technical Field
[0001] The invention relates to a production process of a wool / cashmere / mohair core-spun yarn, and belongs to the technical field of wool / cashmere / mohair core-spun yarn production. Background Art
[0002] With the rapid development of contemporary science and technology and the continuous improvement of people's living standards, people's demand for clothing tends to be comfortable and high-end. Wool, cashmere and mohair are all natural animal protein fibers.
[0003] Cashmere fiber is a rare special animal fiber. It is not only in small production (accounting for only 0.2% of the world's total animal fiber production), but also of excellent quality. It is priced by gram in transactions and is considered to be the "fiber gem" and "fiber queen". It is incomparable to all textile raw materials currently available to humans. Cashmere products have a delicate and plump appearance, soft and smooth feel, light and comfortable to wear, and good warmth retention. However, the length of the velvet is limited, and the finished product has poor elasticity; the height of the suede and the smoothness of the feel are affected by the washing process, making it difficult to maintain a consistent style and having poor elasticity.
[0004] The appearance of mohair fiber is similar to that of sheep wool. The scales are flat and wide, close to the hair shaft, and rarely overlap. Therefore, the fiber surface is smooth, with natural shiny color, silk-like luster, not easy to shrink, and difficult to felt. It has high strength, good resilience and wear resistance, dust and anti-fouling properties, not easy to pilling, and easy to clean and wash. The cortex of mohair is almost entirely composed of positive cortical cells, so the fiber rarely bends, and is more sensitive to some chemical agents than ordinary wool, and has better dyeability. The appearance of mohair is very similar to sheep wool, but not exactly the same. The scales are few and flat and close to the hair shaft, rarely overlap, and have a bamboo tube-like appearance, which makes the fiber surface smooth and produces a silk-like luster. Its fabric has the characteristics of glitter. The fiber is soft, has high fastness, good durability, does not felt, does not pill, and is easy to clean after being stained. Its magnificent appearance, high-grade feel and unique natural luster are unique among textile fibers.
[0005] The core-spun yarn prepared by mixing cashmere and mohair as the covering layer and wool worsted yarn as the core yarn can combine the advantages of cashmere and mohair. In addition, the length of mohair is quite different from that of cashmere, so how to mix cashmere and mohair to make a core-spun yarn with good uniformity has become a problem to be solved. Summary of the invention
[0006] The invention aims to provide a production process of wool / cashmere / mohair core-spun yarn, wherein the prepared core-spun yarn has good strength and anti-pilling properties.
[0007] To solve the above technical problems, the purpose of the present invention is achieved as follows:
[0008] The present invention relates to a wool / cashmere / mohair core-spun yarn production process, comprising the following steps:
[0009] S1. Raw material selection: wool, cashmere and mohair are selected; the wool is 70s-80s wool and 50-120mm in length; the cashmere has a fineness of 15.8μm-16.7μm and a length of 36mm-38mm; the mohair has a fineness of 40-60μm and a length of 100-150mm;
[0010] S2, preparation of core yarn: using wool to make worsted wool yarn, and twisting two worsted wool yarns to form a core yarn;
[0011] S3, preparation of cashmere wool strips: the cashmere fibers are subjected to the steps of wool kneading → wool combing → stripping → combing to obtain cashmere wool strips; the first wool kneading emulsion is sprayed during the wool kneading;
[0012] S4, preparation of mohair tops: the mohair is subjected to the steps of combing → combing into strips → first needle → second needle → combing → third needle → fourth needle to obtain the mohair tops; spraying the second combing emulsion during the combing;
[0013] S5, Blending: The first drawing is to blend the cashmere slivers and add oil to them; the mohair slivers are added with oil; the second drawing is to blend the cashmere slivers off the first drawing with the mohair slivers after adding oil; the slivers off the second drawing are drawn again, mixed and added with oil to finally obtain mixed slivers; the slivers after adding oil need to be left to stand for 20-24 hours before entering the next process;
[0014] S6, spinning: the mixed wool tops prepared in the previous step are made into cashmere / mohair blended roving;
[0015] S7, core-spun yarn preparation: two cashmere / mohair blended rovings and one core yarn are made into wool / cashmere / mohair core-spun yarn by Siro spinning core-spun process;
[0016] The first wool emulsion used in step S3 includes wool oil, antistatic agent and deionized water;
[0017] The second wool emulsion used in step S4 includes wool oil, antistatic agent, coconut oil diethanolamide, lauryl alcohol polyoxyethylene ether, methyl silicone oil and deionized water.
[0018] On the basis of the above scheme and as a preferred scheme of the above scheme: the crude oil includes quaternary ammonium salt of terminal amino hyperbranched compound, cross-linked hyperbranched water-based polyurethane acrylate, refined natural oil, epoxidized soybean oil, castor oil polyoxypropylene polyoxyethylene ether and deionized water.
[0019] On the basis of the above scheme and as a preferred scheme of the above scheme: the antistatic agent is octadecyl phosphate.
[0020] On the basis of the above scheme and as a preferred scheme of the above scheme: in step S5, the oil added to the cashmere wool tops is the first wool emulsion, and the oil added to the mohair wool tops is the second wool emulsion.
[0021] On the basis of the above scheme and as a preferred scheme of the above scheme: in step S5, the third wool emulsion is added to the wool strips obtained by mixing mohair and cashmere, and the third wool emulsion includes wool oil, antistatic agent, bonding agent, hydrogen peroxide, ferrous chloride and deionized water.
[0022] On the basis of the above scheme and as a preferred scheme of the above scheme: the encapsulating agent is at least one of fatty alcohol polyoxyethylene ether or fatty amine polyoxyethylene ether.
[0023] The beneficial effects of the present invention are as follows: the wool / cashmere / mohair core-spun yarn production process of the present invention uses coconut oil diethanolamide, lauryl alcohol polyoxyethylene ether, and methyl silicone oil in the hair oiling agent used when adding oil to mohair, which can improve the smoothness and softness of mohair fibers during combing and facilitate the combing of mohair. Oiling is also performed during blending and the yarn is left to stand for a certain period of time, so that the blending can proceed smoothly. DETAILED DESCRIPTION
[0024] The present invention is further described below in conjunction with specific embodiments.
[0025] Embodiment 1
[0026] The wool / cashmere / mohair core-spun yarn production process involved in this embodiment includes the following steps: S1 raw material selection, S2 core yarn preparation, S3 cashmere top preparation, S4 mohair top preparation, S5 blending, S6 roving, S7 core-spun yarn preparation.
[0027] In step S1, wool, cashmere and mohair are selected; the wool is 70s-80s wool and 50-120mm in length; the cashmere has a fineness of 15.8μm-16.7μm and a length of 36mm-38mm; the mohair has a fineness of 40-60μm and a length of 100-150mm.
[0028] In step S2, the core yarn is prepared by using wool to make worsted wool yarn, and two worsted wool yarns are twisted together to form the core yarn. The wool fiber is made into 60-count worsted wool yarn by using a worsted spinning system, and two 60-count worsted wool yarns are twisted together to form a 2 / 60-count ply yarn.
[0029] In step S3, the cashmere wool strips are prepared by kneading, combing, slivering and combing the cashmere fibers to obtain cashmere wool strips. The first kneading emulsion is sprayed during kneading, and the spraying amount of the first kneading emulsion accounts for 4-6% of the weight of the cashmere fibers, and is selected as 5% in this embodiment. The basis weight of the cashmere wool strips is 18.5-19.0 g / 5 m.
[0030] The first wool emulsion used in step S3 includes wool oil, antistatic agent and deionized water, wherein the wool oil is 15-30% by weight and the antistatic agent is 5-10% by weight. In this embodiment, the wool oil is 20% by weight, the antistatic agent is 5% by weight, and the balance is deionized water.
[0031] In step S4, the mohair wool top is prepared by kneading the mohair wool → combing into strips → first needle → second needle → combing → third needle → fourth needle, and the mohair wool top is obtained; the second kneading emulsion is sprayed during kneading, and the dosage of the second kneading emulsion is 6% of the weight of the mohair fiber. The weight of the mohair wool top is 18.5-19.0g / 5m.
[0032] The wool-adding auxiliary agent used in the wool-adding oil involved in step S4 comprises wool-adding oil, antistatic agent, coconut oil diethanolamide, lauryl alcohol polyoxyethylene ether, methyl silicone oil and deionized water. Wherein, by weight percentage, the wool-adding oil is 10-20%, the antistatic agent is 5-10%, the coconut oil diethanolamide is 2-5%, the lauryl alcohol polyoxyethylene ether is 1-3%, and the methyl silicone oil is 2-5%. Specifically in the present embodiment, in the second wool-adding emulsion, the wool-adding oil is 15%, the antistatic agent is 6%, the coconut oil diethanolamide is 3%, the lauryl alcohol polyoxyethylene ether is 2%, the methyl silicone oil is 3%, and the balance is deionized water.
[0033] Further, the used and crude oil comprise terminal amino hyperbranched compound quaternary ammonium salt, cross-linked hyperbranched waterborne polyurethane acrylate, refined natural oil, epoxidized soybean oil, castor oil polyoxypropylene polyoxyethylene ether and deionized water.Wherein by weight percentage, amino hyperbranched compound quaternary ammonium salt is 10-20%, cross-linked hyperbranched waterborne polyurethane acrylate is 8-12%, refined natural oil is 15-25%, epoxidized soybean oil is 15-25%, and castor oil polyoxypropylene polyoxyethylene ether is 8-12%.Specific to the present embodiment, in and crude oil, amino hyperbranched compound quaternary ammonium salt is 15%, cross-linked hyperbranched waterborne polyurethane acrylate is 10%, refined natural oil is 20%, epoxidized soybean oil is 20%, castor oil polyoxypropylene polyoxyethylene ether is 10%, and surplus is deionized water.
[0034] Furthermore, the antistatic agent used is octadecyl phosphate.
[0035] In step S5, the first drawing is to mix and oil the cashmere wool strips; the oil added to the cashmere wool strips is the first wool emulsion, and the amount is 1-3% of the weight of the cashmere wool strips. In this embodiment, 3% is selected. In the first drawing, the basis weight is 18.9g / 5m, 8 strands are drawn, and the drafting multiple in the back zone is 1.65; the bell mouth diameter is 3.2mm;
[0036] The mohair wool tops are oiled; the oil added to the mohair wool tops is the second wool oil emulsion, and the amount used accounts for 2-5% of the weight of the mohair wool tops. In this embodiment, 4% is selected.
[0037] The second drawing process is to mix the cashmere wool strips after the first drawing process with the mohair wool strips after oiling; the wool strips after the second drawing process are drawn again, mixed and oiled to finally obtain mixed wool strips; the wool strips after each oiling process need to be left to stand for 20-24 hours before entering the next process; the wool strips after the mohair and cashmere are mixed are added with the third wool emulsion, which includes wool oil, antistatic agent, cohesive agent, hydrogen peroxide, ferrous chloride and deionized water. The amount of the third wool emulsion accounts for 3% of the weight of the mixed wool strips. The hydrogen peroxide used reacts with the divalent iron ions in the ferrous chloride to generate oxygen free radicals and trivalent iron ions, which have good oxidizability, can treat the surface of mohair and cashmere fibers, can increase the roughness of the fiber surface, increase friction, and under the joint action of the cohesive agent, can improve the cohesive force between fibers, and the yarn formed is not easy to pilling.
[0038] In the second drawing process, the basis weight is 18.7g / 5m, 8 strands are drawn together, and the drafting multiple in the rear zone is 1.52; the bell mouth diameter is 3.0mm.
[0039] Furthermore, by weight percentage, the third and wool emulsion contains 25-35% of wool oil, 6-10% of antistatic agent, 4-6% of cohesive agent, 4-6% of hydrogen peroxide, and 2-5% of ferrous chloride. Specifically, in the third and wool emulsion of this embodiment, the wool oil is 30%, the antistatic agent is 8%, the cohesive agent is 5%, the hydrogen peroxide is 4%, the ferrous chloride is 3% and the balance is deionized water.
[0040] Furthermore, the cohesive agent is at least one of fatty alcohol polyoxyethylene ether and fatty amine polyoxyethylene ether. In this embodiment, fatty alcohol polyoxyethylene ether and fatty amine polyoxyethylene ether are mixed in a weight ratio of 1:1.
[0041] S6, roving: the mixed wool tops prepared in the previous step are made into cashmere / mohair blended roving.
[0042] S7. Preparation of core-spun yarn: Two cashmere / mohair blended rovings and one core yarn are made into wool / cashmere / mohair core-spun yarn by siro spinning core-spun process; the fineness of the prepared wool / cashmere / mohair core-spun yarn is 5.5 count.
[0043] The wool / cashmere / mohair core-spun yarn prepared in this embodiment was knitted into a fabric according to a warp knitting plain needle structure, and the anti-pilling performance was tested, and the test result was level 4.
[0044] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A wool / cashmere / mohair core-spun yarn production process, characterized in that: The steps include: S1. Raw material selection: wool, cashmere and mohair are selected; the wool is 70s-80s wool and 50-120mm in length; the cashmere has a fineness of 15.8μm-16.7μm and a length of 36mm-38mm; the mohair has a fineness of 40-60μm and a length of 100-150mm; S2, preparation of core yarn: using wool to make worsted wool yarn, and twisting two worsted wool yarns to form a core yarn; S3, preparation of cashmere wool strips: the cashmere fibers are subjected to the steps of wool kneading → wool combing → stripping → combing to obtain cashmere wool strips; the first wool kneading emulsion is sprayed during the wool kneading; S4, preparation of mohair tops: the mohair is subjected to the steps of combing → combing into strips → first needle → second needle → combing → third needle → fourth needle to obtain the mohair tops; spraying the second combing emulsion during the combing; S5, Blending: The first drawing is to blend the cashmere slivers and add oil to them; the mohair slivers are added with oil; the second drawing is to blend the cashmere slivers off the first drawing with the mohair slivers after adding oil; the slivers off the second drawing are drawn again, mixed and added with oil to finally obtain mixed slivers; the slivers after adding oil need to be left to stand for 20-24 hours before entering the next process; S6, spinning: the mixed wool tops prepared in the previous step are made into cashmere / mohair blended roving; S7, core-spun yarn preparation: two cashmere / mohair blended rovings and one core yarn are made into wool / cashmere / mohair core-spun yarn by Siro spinning core-spun process; The first wool emulsion used in step S3 includes wool oil, antistatic agent and deionized water; The second wool emulsion used in step S4 includes wool oil, antistatic agent, coconut oil diethanolamide, lauryl alcohol polyoxyethylene ether, methyl silicone oil and deionized water.
2. A wool / cashmere / mohair core-spun yarn production process according to claim 1, characterized in that: The crude oil comprises quaternary ammonium salt of terminal amino hyperbranched compound, cross-linked hyperbranched waterborne polyurethane acrylate, refined natural oil, epoxy soybean oil, castor oil polyoxypropylene polyoxyethylene ether and deionized water.
3. A wool / cashmere / mohair core-spun yarn production process according to claim 1, characterized in that: The antistatic agent is octadecyl phosphate.
4. A wool / cashmere / mohair core-spun yarn production process according to claim 1, characterized in that: In step S5, the oil added to the cashmere wool top is the first wool emulsion, and the oil added to the mohair wool top is the second wool emulsion.
5. A wool / cashmere / mohair core-spun yarn production process according to claim 1, characterized in that: In step S5, the third wool emulsion is added to the wool strips obtained by mixing mohair and cashmere. The third wool emulsion comprises wool oil, antistatic agent, bonding agent, hydrogen peroxide, ferrous chloride and deionized water.
6. A wool / cashmere / mohair core-spun yarn production process according to claim 5, characterized in that: The cohesive agent is at least one of fatty alcohol polyoxyethylene ether or fatty amine polyoxyethylene ether.
Citation Information
Patent Citations
Method for producing dyeing-free camel hair and yak wool blended fabric
CN101413167A
Mohair blended stocking yarn and technique for processing same
CN101469473A
Wool oil for production of fibers
CN102704264A
Cashmere fiber core-spun composite yarn and preparation method thereof
CN102936775A
Mohair blended yarn
CN104357986A
Cited By
Antibacterial mildew-proof wood wax oil and preparation method thereof
CN120888233A