Wear-resistant fabric with heating function and preparation method thereof
Through the combination of rush/cotton blended yarn and far infrared fiber, combined with degumming and soft processing technology, the problem of improving wear resistance and warmth performance of down jacket fabrics is solved, and wear resistance with high strength and excellent far infrared heating performance is achieved Fabric improves the durability and comfort of the down jacket.
Patent Information
- Application Number
- CN202411034487.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-05
AI Technical Summary
When existing down jacket fabrics improve wear resistance and warmth, the coating is easily damaged, affecting breathable and moisture permeability and wear comfort, and the fiber selection is not enough to meet the requirements of high strength and durability.
Using rush/cotton blended yarn as warp yarn, far infrared fiber as weft yarn, fiber strength is enhanced by degumming, soft treatment and cyclic heat treatment, and made of polyurethane slices, far infrared ceramic powder, antistatic agents and other materials with heating Functional wear-resistant fabric.
It achieves high strength of the fabric, excellent far-infrared heating performance and good wear resistance, and improves the service life and wear comfort of the down jacket.
Smart Images

Figure BDA0004970711530000051 
Figure BDA0004970711530000061 
Figure BDA0004970711530000062
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fabric preparation, and in particular relates to a wear-resistant fabric with a heating function and a preparation method thereof. Background Art
[0002] Functional fabrics refer to fabrics with certain special properties and uses. Functional fabrics on the market are mainly clothing fabrics. With the continuous expansion of the wearing environment of down jackets, there are some new requirements for the performance of down jacket fabrics. They are not only limited to the improvement of warmth retention performance, but also require functionality such as wear resistance and high strength, so as to meet the requirements of durability of down jackets.
[0003] In order to enhance the wear resistance of fabrics, the existing process will coat a wear-resistant functional coating on the surface of the fabrics, but the coating is easily damaged by wearing, and correspondingly affects its air permeability, moisture permeability and wearing comfort. Therefore, the improvement of fabric performance can also be based on the selection of fibers. To this end, in response to the above-mentioned problems, the present invention provides a wear-resistant fabric with a heating function and a preparation method thereof. Summary of the invention
[0004] In order to solve the above problems, the primary purpose of the present invention is to provide a wear-resistant fabric with heating function and a preparation method thereof.
[0005] The specific technical solutions of the present invention include:
[0006] As a first aspect of the present invention, a wear-resistant fabric with a heating function is provided, wherein the wear-resistant fabric is woven with iris / cotton blended yarn as warp yarn and far-infrared fiber as weft yarn; wherein the iris / cotton blended yarn is obtained by degumming and softening iris straw to obtain iris fiber, and the iris fiber and cotton fiber are blended in a blending ratio of 10-40:60-90.
[0007] As a further optimization scheme of the present invention, the steps of degumming and softening the Iris stalks include:
[0008] (1) Soak the stalks of Iris edulis in tap water and boil for 1-3 hours;
[0009] (2) combing the Iris stalks treated in step (1) into filaments;
[0010] (3) immersing the filamentous iris straw obtained by the treatment in step (2) in a wood ash aqueous solution for 1-3 hours, performing a cyclic heat treatment during the immersion process, with a bath ratio of 1:30, and washing the iris straw with warm water after the treatment is completed;
[0011] (4) immersing the Iris stalk treated in step (3) in a complex enzyme solution containing equal amounts of β-glucanase and laccase for 1-3 h, with a pH of 5.5, a temperature of 50° C., and a bath ratio of 1:30, and then washing with warm water to complete the degumming treatment;
[0012] (5) Immerse the degummed Iris straw in a softening finishing agent for 20-30 minutes, with a bath ratio of 1:50 and a temperature of 50-70°C. Press dry and air dry to complete the softening treatment.
[0013] As a further optimization scheme of the present invention, in step (3), the amount of wood ash used is 10-15% of the mass of the Ula grass straw.
[0014] As a further optimization scheme of the present invention, in step (3), the cyclic heat treatment is specifically to heat the temperature to 120-140°C at a heating rate of 10°C / min, keep it warm for 10 minutes, then cool it to 40-50°C at a cooling rate of 10°C / min, keep it warm for 10 minutes, and repeat the cycle.
[0015] As a further optimization scheme of the present invention, the dosage of the complex enzyme is 10-15% of the mass of the Iris stalk.
[0016] As a second aspect of the present invention, there is also provided a method for preparing a wear-resistant fabric with a heating function as described above, comprising the following steps:
[0017] (1) degumming and softening iris straw to obtain iris fiber, mixing the iris fiber with cotton fiber according to a set mass ratio, and then opening, carding, drawing, and rotor spinning to obtain iris / cotton blended yarn;
[0018] (2) mixing the dried polyurethane slices with far-infrared ceramic powder, antistatic agent and dispersant uniformly, blending and granulating to obtain far-infrared masterbatch, drying the far-infrared masterbatch, and melt spinning to obtain the far-infrared fiber;
[0019] (3) The wear-resistant fabric with heating function is obtained by weaving the Iris / cotton blended yarn as the warp yarn and the far-infrared fiber as the weft yarn.
[0020] As a further optimization scheme of the present invention, in step (2), the components of the far-infrared fiber, measured by mass percentage, include 90-99% of polyurethane chips, 1-10% of far-infrared ceramic powder, 0.5-1% of antistatic agent, and 0.5-1% of dispersant, wherein the far-infrared ceramic powder is one or more of aluminum oxide, zinc oxide and silicon oxide.
[0021] As a further optimization scheme of the present invention, in step (3), the weaving density of the warp yarn is 50-65 yarns / cm, the weaving density of the weft yarn is 50-80 yarns / cm, and the weaving structure is plain weave.
[0022] In summary, the beneficial effects of the present invention are:
[0023] (1) The present invention blends iris fiber with cotton fiber to obtain a blended yarn, and uses the iris / cotton blended yarn as the warp yarn and the far-infrared fiber as the weft yarn to weave a fabric. The fabric has good far-infrared heating performance. Experimental research shows that the effect of iris fiber on improving the strength of the fabric is better than that of flax and ramie fibers. The fabric made of iris fiber has excellent mechanical properties.
[0024] (2) The present invention degummed the iris straw by first boiling it in water, then soaking it in a wood ash aqueous solution and combining it with a cyclic heating treatment, and then preparing fabrics with the obtained iris fibers, thereby improving the strength of the fabrics, making the fabrics stronger and more functional. DETAILED DESCRIPTION
[0025] The present application is described in further detail below. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technicians in this field can make some non-essential improvements and adjustments to the present application based on the above application content.
[0026] Example 1
[0027] The present embodiment provides a wear-resistant fabric with a heating function, wherein the wear-resistant fabric is woven with iris / cotton blended yarn as warp yarn and far-infrared fiber as weft yarn; wherein the iris / cotton blended yarn is obtained by degumming and softening iris straw to obtain iris fiber, and the iris fiber and cotton fiber are blended in a blending ratio of 40:60.
[0028] In this embodiment, the degumming and softening treatment of the caltrop straw is specifically as follows: the caltrop straw is immersed in tap water and boiled for 1 hour, then combed into filaments, the filamentous caltrop straw is immersed in a wood ash aqueous solution for treatment for 3 hours, and the immersion process is coordinated with cyclic heat treatment, the bath ratio is 1:30, the amount of wood ash is 10% of the mass of the caltrop straw, and the cyclic heat treatment is specifically heated to 140°C at a heating rate of 10°C / min, kept warm for 10 minutes, and then cooled to 40°C at a cooling rate of 10°C / min, kept warm for 10 minutes, and then cyclically repeated. After the treatment is completed, the iris straw is washed with warm water, and then immersed in a complex enzyme solution containing equal masses of β-glucanase and laccase for 1 hour, with a pH of 5.5, a temperature of 50°C, and a bath ratio of 1:30. The degumming treatment is completed by washing with warm water. The dosage of the complex enzyme is 10% of the mass of the iris straw. The degummed iris straw is immersed in a softening finishing agent (commercially available softener SG-6) for 30 minutes, with a bath ratio of 1:50 and a temperature of 50°C. The softening treatment is completed by pressing and drying.
[0029] The preparation method of the wear-resistant fabric comprises the following steps:
[0030] (1) Degumming and softening iris straw to obtain iris fiber, mixing the iris fiber with cotton fiber according to a set mass ratio, and then opening, carding, drawing, and rotor spinning to obtain iris / cotton blended yarn (opening, carding, drawing, and rotor spinning are existing technologies mastered by those skilled in the art, and this embodiment does not improve them, so they are not limited);
[0031] (2) mixing the dried polyurethane chips with far-infrared ceramic powder, antistatic agent and dispersant uniformly, blending and granulating to obtain far-infrared masterbatch, drying the far-infrared masterbatch, and melt spinning to obtain the far-infrared fiber, wherein the components of the far-infrared fiber include 90% of polyurethane chips, 9% of far-infrared ceramic powder, 0.5% of antistatic agent (ethoxylated lauryl amide) and 0.5% of dispersant NNO in terms of mass percentage, wherein the far-infrared ceramic powder is aluminum oxide;
[0032] (3) The wear-resistant fabric with heating function is obtained by weaving the Iris / cotton blended yarn as the warp yarn and the far-infrared fiber as the weft yarn. The weaving density of the warp yarn is 50 yarns / cm, the weaving density of the weft yarn is 50 yarns / cm, and the weaving structure is plain weave.
[0033] Example 2
[0034] The present embodiment provides a wear-resistant fabric with a heating function, wherein the wear-resistant fabric is woven with iris / cotton blended yarn as the warp yarn and far-infrared fiber as the weft yarn; wherein the iris / cotton blended yarn is obtained by degumming and softening iris straw to obtain iris fiber, and the iris fiber and cotton fiber are blended in a blending ratio of 10:90.
[0035] In this embodiment, the degumming and softening treatment of the caltrop straw is specifically as follows: the caltrop straw is immersed in tap water and boiled for 3 hours, then combed into filaments, the filamentous caltrop straw is immersed in a wood ash aqueous solution for treatment for 3 hours, and cyclic heat treatment is carried out during the immersion process. The bath ratio is 1:30, and the amount of wood ash is 15% of the mass of the caltrop straw. The cyclic heat treatment is specifically heated to 120°C at a heating rate of 10°C / min, kept warm for 10 minutes, and then cooled to 50°C at a cooling rate of 10°C / min, kept warm for 10 minutes, and then repeated. After the treatment is completed, the iris straw is washed with warm water, and then immersed in a complex enzyme solution containing equal masses of β-glucanase and laccase for 1 hour, with a pH of 5.5, a temperature of 50°C, and a bath ratio of 1:30. The degumming treatment is completed by washing with warm water. The dosage of the complex enzyme is 15% of the mass of the iris straw. The degummed iris straw is immersed in a softening finishing agent (commercially available softener SG-6) for 30 minutes, with a bath ratio of 1:50 and a temperature of 50°C. The softening treatment is completed by pressing and drying.
[0036] The preparation method of the wear-resistant fabric comprises the following steps:
[0037] (1) Step (1) is the same as in Example 1;
[0038] (2) mixing the dried polyurethane chips with far-infrared ceramic powder, antistatic agent and dispersant, blending and granulating to obtain far-infrared masterbatch, drying the far-infrared masterbatch, and melt spinning to obtain the far-infrared fiber, wherein the components of the far-infrared fiber include 95% of polyurethane chips, 4% of far-infrared ceramic powder, 0.5% of antistatic agent (ethoxylated lauryl amide) and 0.5% of dispersant NNO in terms of mass percentage, wherein the far-infrared ceramic powder is zinc oxide;
[0039] (3) The wear-resistant fabric with heating function is obtained by weaving the Iris / cotton blended yarn as the warp yarn and the far-infrared fiber as the weft yarn. The weaving density of the warp yarn is 65 yarns / cm, the weft yarn is 80 yarns / cm, and the weaving structure is plain weave.
[0040] Example 3
[0041] The present embodiment provides a wear-resistant fabric with a heating function, wherein the wear-resistant fabric is woven with iris / cotton blended yarn as the warp yarn and far-infrared fiber as the weft yarn; wherein the iris / cotton blended yarn is obtained by degumming and softening iris straw to obtain iris fiber, and the iris fiber and cotton fiber are blended in a blending ratio of 30:70.
[0042] In this embodiment, the degumming and softening treatment of the caltrop straw is specifically as follows: the caltrop straw is immersed in tap water and boiled for 3 hours, then combed into filaments, the filamentous caltrop straw is immersed in a wood ash aqueous solution for treatment for 3 hours, and cyclic heat treatment is carried out during the immersion process. The bath ratio is 1:30, and the amount of wood ash is 15% of the mass of the caltrop straw. The cyclic heat treatment is specifically heated to 120°C at a heating rate of 10°C / min, kept warm for 10 minutes, and then cooled to 50°C at a cooling rate of 10°C / min, kept warm for 10 minutes, and then repeated. After the treatment is completed, the iris straw is washed with warm water, and then immersed in a complex enzyme solution containing equal masses of β-glucanase and laccase for 3 hours, with a pH of 5.5, a temperature of 50°C, and a bath ratio of 1:30. The degumming treatment is completed by washing with warm water. The dosage of the complex enzyme is 15% of the mass of the iris straw. The degummed iris straw is immersed in a softening finishing agent (commercially available softener SG-6) for 30 minutes, with a bath ratio of 1:50 and a temperature of 50°C. The softening treatment is completed by pressing and drying.
[0043] The preparation method of the wear-resistant fabric comprises the following steps:
[0044] Step (1) is the same as in Example 1;
[0045] (2) mixing the dried polyurethane chips with far-infrared ceramic powder, antistatic agent and dispersant uniformly, blending and granulating to obtain far-infrared masterbatch, drying the far-infrared masterbatch, and melt spinning to obtain the far-infrared fiber, wherein the components of the far-infrared fiber include 98% of polyurethane chips, 1% of far-infrared ceramic powder, 0.5% of antistatic agent (ethoxylated lauryl amide) and 0.5% of dispersant NNO in terms of mass percentage, wherein the far-infrared ceramic powder is zinc oxide;
[0046] Step (3) is the same as in Example 1.
[0047] Verification test
[0048] 1. In order to study the effect of the addition of iris grass fiber on the performance of the fabric, the composition of the fabric was adjusted according to Table 1. The component composition and preparation method of the far-infrared fiber were the same as in Example 1. The iris grass / cotton blended yarn was used as the warp yarn and the far-infrared fiber was used as the weft yarn to weave the wear-resistant fabric with heating function. The weaving density and weaving structure of the warp yarn and the weft yarn were the same as in Example 1.
[0049] Table 1. Fabric composition design table
[0050]
[0051]
[0052] The tensile properties and elongation at break of fabrics made from fabric AF were tested according to GB / T3923.1-1997 standard. The results are shown in Table 2.
[0053] Table 2. Test results statistics
[0054]
[0055] It can be seen from Table 1 that the tensile strength of fabric AD is higher than that of fabric EF. By comparison, the warp yarn used in fabric AD is flax / cotton blended yarn, while fabric EF uses flax fiber and ramie fiber instead of the flax fiber of the present application respectively. From the data results, it can be seen that the effect of flax fiber in improving the strength of the fabric is better than that of flax fiber and ramie fiber.
[0056] Then, referring to GB / T21196.2-2007 "Determination of the abrasion resistance of textile fabrics by the Martindale method" standard, abrasion resistance tests were carried out on down jacket fabric samples in the initial state and after folding 10,000 times, and their abrasion resistance index Ai (average mass loss per friction) was tested. The results are shown in Table 3.
[0057] Table 3. Test results statistics
[0058]
[0059] It can be seen from Table 2 that the wear resistance of fabric AD is better than that of fabric EF, that is, the wear resistance of the fabric improved by iris fiber is better than that of flax fiber and ramie fiber. In addition, from the comparison of the results of fabric AD, it can be seen that with the change of the blending ratio of iris fiber and cotton fiber, the wear resistance of the fabric also changes accordingly. Specifically, when the proportion of cotton fiber in the blended yarn is high, the wear resistance of the fabric is relatively poor, and when the proportion of cotton fiber in the blended yarn is low, the wear resistance of the fabric is relatively good.
[0060] Finally, the far-infrared performance of the fabric samples was tested according to GB / T30127-2013 “Testing and Evaluation of Far-Infrared Performance of Textiles”, with a far-infrared wavelength range of 8-15 μm. The results are shown in Table 4.
[0061] Table 4. Test results statistics
[0062]
[0063] It can be seen from Table 3 that the far-infrared heating performance of fabric AE is good, the far-infrared emissivity is maintained between 94.7-95.4, and the radiation temperature rise value is more than 2°C. It can be seen that the fabric woven with iris / cotton blended yarn as warp yarn and far-infrared fiber as weft yarn will not affect the thermal insulation performance of the fabric. The fabric has good far-infrared heating performance and excellent thermal insulation performance.
[0064] 2. In order to further explore the effect of the treatment method of iris fiber on the performance of the fabric, the following comparative examples were set:
[0065] Comparative Example 1
[0066] In this comparative example, the degumming and softening treatment of the iris straw is specifically as follows: the iris straw is immersed in tap water and boiled for 1 hour, then combed into filaments, the filamentous iris straw is immersed in a sodium hydroxide solution for treatment for 3 hours, and cyclic heat treatment is carried out during the immersion process. The bath ratio is 1:30, and the amount of sodium hydroxide used is 10% of the mass of the iris straw. The cyclic heat treatment is specifically heated to 140°C at a heating rate of 10°C / min, kept warm for 10 minutes, and then cooled to 40°C at a cooling rate of 10°C / min, kept warm for 10 minutes, and then repeated. After the treatment is completed, the iris straw is washed with warm water, and then immersed in a complex enzyme solution containing equal masses of β-glucanase and laccase for 1 hour, with a pH of 5.5, a temperature of 50°C, and a bath ratio of 1:30. The degumming treatment is completed by washing with warm water. The dosage of the complex enzyme is 10% of the mass of the iris straw. The degummed iris straw is immersed in a softening finishing agent (commercially available softener SG-6) for 30 minutes, with a bath ratio of 1:50 and a temperature of 50°C. The softening treatment is completed by pressing and drying.
[0067] Comparative Example 2
[0068] In this comparative example, the degumming and softening treatment of the iris straw is specifically as follows: the iris straw is immersed in tap water and boiled for 1 hour, then combed into filaments, and the filaments of the iris straw are immersed in a wood ash solution for treatment for 3 hours, the bath ratio is 1:30, the amount of wood ash is 10% of the mass of the iris straw, and the temperature is maintained at 140°C. After the treatment is completed, the iris straw is washed with warm water, and then immersed in a complex enzyme solution containing equal masses of β-glucanase and laccase for 1 hour, with a pH of 5.5, a temperature of 50°C, and a bath ratio of 1:30. The degumming treatment is completed by washing with warm water. The dosage of the complex enzyme is 10% of the mass of the iris straw. The degummed iris straw is immersed in a softening finishing agent (commercially available softener SG-6) for 30 minutes, with a bath ratio of 1:50 and a temperature of 50°C. The softening treatment is completed by pressing and drying.
[0069] Comparative Example 3
[0070] In this comparative example, the degumming and softening treatment of the iris straw is specifically as follows: the iris straw is immersed in tap water and boiled for 1 hour, then combed into filaments, and the filaments of the iris straw are immersed in a wood ash aqueous solution for 3 hours, the bath ratio is 1:30, the amount of wood ash is 10% of the mass of the iris straw, and the temperature is maintained at 40°C. After the treatment is completed, the iris straw is washed with warm water, and then immersed in a complex enzyme solution containing equal masses of β-glucanase and laccase for 1 hour, with a pH of 5.5, a temperature of 50°C, and a bath ratio of 1:30. The degumming treatment is completed by washing with warm water. The dosage of the complex enzyme is 10% of the mass of the iris straw. The degummed iris straw is immersed in a softening finishing agent (commercially available softener SG-6) for 30 minutes, with a bath ratio of 1:50 and a temperature of 50°C. The softening treatment is completed by pressing and drying.
[0071] In addition, the iris fibers obtained by immersing iris straw in tap water and boiling it for 1 hour and then combing it into filaments were used as the control group. The iris fibers obtained by treating the control group and comparative examples 1-3 were used to prepare fabrics according to the method of Example 1. Subsequently, the fabrics prepared in Example 1 and comparative examples 1-3 were tested for tensile properties and elongation at break in accordance with GB / T3923.1-1997 standard. The results are shown in Table 5.
[0072] Table 5. Test results statistics
[0073]
[0074] It can be seen from Table 5 that the treatment method of iris fiber has a certain influence on the mechanical properties of the fabric. Compared with Example 1, Comparative Example 1 uses conventional sodium hydroxide solution instead of the plant ash aqueous solution in Example 1. From the results, the mechanical properties of the fabric obtained in Comparative Example 1 are not as good as those in Example 1. Compared with sodium hydroxide, plant ash causes less damage to iris fiber when treating iris fiber, and the fiber itself loses less toughness. Therefore, after being made into fabric, the fabric can maintain good mechanical properties. Compared with Example 1, Comparative Examples 2-3 use plant ash aqueous solution to soak iris fiber. The comparative example 2 was carried out at 140°C without cyclic heat treatment. The continuous high temperature treatment affected the fiber structure itself, and the mechanical properties of the fabric decreased seriously compared with those in Example 1. The comparative example 3 was carried out at a lower temperature than that in Example 1. From the data, it can be seen that the mechanical properties of the fabric were not improved. In Example 1, the iris straw was soaked in a water solution of wood ash and combined with cyclic heat treatment to increase the splitting degree of the fiber. The fiber structure was loosened and degummed with a composite enzyme treatment, which fully removed the pectin on the fiber and increased the spinnability of the fiber.
[0075] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A wear-resistant fabric with heating function, characterized in that: The wear-resistant fabric is woven with iris / cotton blended yarn as warp yarn and far-infrared fiber as weft yarn; wherein the iris / cotton blended yarn is obtained by degumming and softening iris straw to obtain iris fiber, and the iris fiber and cotton fiber are blended in a blending ratio of 10-40:60-90.
2. The wear-resistant fabric with heating function according to claim 1, characterized in that: The steps of degumming and softening the iris straw include: (1) Soak the stalks of Iris edulis in tap water and boil for 1-3 hours; (2) combing the Iris stalks treated in step (1) into filaments; (3) immersing the filamentous iris straw obtained by the treatment in step (2) in a wood ash aqueous solution for 1-3 hours, performing a cyclic heat treatment during the immersion process, with a bath ratio of 1:30, and washing the iris straw with warm water after the treatment is completed; (4) immersing the Iris stalk treated in step (3) in a complex enzyme solution containing equal amounts of β-glucanase and laccase for 1-3 h, with a pH of 5.5, a temperature of 50° C., and a bath ratio of 1:30, and then washing with warm water to complete the degumming treatment; (5) Immerse the degummed Iris straw in a softening finishing agent for 20-30 minutes, with a bath ratio of 1:50 and a temperature of 50-70°C. Press dry and air dry to complete the softening treatment.
3. The wear-resistant fabric with heating function according to claim 2, characterized in that: In step (3), the amount of wood ash used is 10-15% of the mass of the Ula grass straw.
4. The wear-resistant fabric with heating function according to claim 2, characterized in that: In step (3), the cyclic heat treatment is specifically to heat up to 120-140°C at a heating rate of 10°C / min, keep warm for 10 minutes, then cool down to 40-50°C at a cooling rate of 10°C / min, keep warm for 10 minutes, and repeat the cycle.
5. The wear-resistant fabric with heating function according to claim 2, characterized in that: The dosage of the complex enzyme is 10-15% of the mass of the iris straw.
6. A method for preparing the wear-resistant fabric with heating function as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: (1) degumming and softening iris straw to obtain iris fiber, mixing the iris fiber with cotton fiber according to a set mass ratio, and then opening, carding, drawing, and rotor spinning to obtain iris / cotton blended yarn; (2) mixing the dried polyurethane slices with far-infrared ceramic powder, antistatic agent and dispersant uniformly, blending and granulating to obtain far-infrared masterbatch, drying the far-infrared masterbatch, and melt spinning to obtain the far-infrared fiber; (3) The wear-resistant fabric with heating function is obtained by weaving the Iris / cotton blended yarn as the warp yarn and the far-infrared fiber as the weft yarn.
7. The method for preparing a wear-resistant fabric with heating function according to claim 6, characterized in that: In step (2), the far-infrared fiber comprises, by mass percentage, 90-95% of polyurethane chips, 1-10% of far-infrared ceramic powder, 0.5-1% of antistatic agent, and 0.5-1% of dispersant, wherein the far-infrared ceramic powder is one or more of aluminum oxide, zinc oxide, and silicon oxide.
8. The method for preparing a wear-resistant fabric with heating function according to claim 6, characterized in that: In step (3), the weaving density of the warp yarn is 50-65 yarns / cm, the weaving density of the weft yarn is 50-80 yarns / cm, and the weaving structure is plain weave.
Citation Information
Patent Citations
Method for manufacturing iris lactea pall artificial cotton
CN101892526A
Preparation method of anti-microbial wear-proof protective clothing fabric
CN105862226A
Refined preparation method of Carex meyeriana fiber
CN106119980A
Chem-bio combined preparation method of carex meyeriana fibers
CN106149063A
Infrared heating fabric and preparation method
CN109023649A