Woven fabric
By using warp and weft interwoven structures with different buckling rates in the woven fabric, the problem of insufficient tearing strength in the warp and weft direction of the light and light woven fabric is solved, and the balance between high tear strength and low ventilation is achieved. It is suitable for light and thin down jackets, etc. product.
Patent Information
- Application Number
- CN202310499515.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-05
- Publication Date
- 2024-11-05
AI Technical Summary
The tear strength of existing thin and light woven fabrics in the weft direction is insufficient, which limits its application range.
By using warp and weft interwoven structures with different buckling rates in the woven fabric, the buckling rates of yarn YA, yarn YB and yarn YC meet the relationship of 0.25A≥C≥1.25B, and the yarn is increased during the tearing process. to increase tear strength while maintaining low ventilation.
Even thin and light woven fabrics can show excellent tear strength in the weft direction, extend their service life, and are suitable for making thin down jackets and other products.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a woven fabric, in particular to a woven fabric which is light and thin and has excellent tearing strength in both warp and weft directions. Background Art
[0002] Woven fabrics are made of warp and weft yarns, have a stable structure, a smooth surface and good washing resistance. They are one of the textiles with the longest history and the widest range of uses, and are deeply loved by consumers.
[0003] In the development of woven fabrics, people have also made a lot of efforts to obtain products with superior performance. For example, Japanese patent document 2020-125558 discloses a fabric, which specifically discloses that the woven yarns YA and YB arranged in the same direction each have different curl rates A and B, wherein the curl rate A is 15% to 500%, and the curl rate B is less than 4%. Such a fabric has excellent waterproofness and low air permeability and is soft to the touch, but it does not solve the problem of poor tear strength in the warp and weft directions of thin and light fabrics.
[0004] For another example, Chinese patent document CN111655917A discloses a plain woven fabric, a manufacturing method thereof and a stent graft, and specifically discloses that the woven yarns YA and YB arranged in the same direction respectively have different curl rates A and B, A≥B×1.2, and the curl rate B is above 4%, and the cover factor is above 2400. Such a fabric also has low air permeability and excellent waterproofness, but does not solve the problem of poor tearing strength in the warp and weft directions of thin and light fabrics.
[0005] In addition, the thin fabrics formed by lower denier yarns have lower yarn strength, especially when ordinary plain weave is used, the tearing strength is often relatively small, which greatly limits its application range. Summary of the invention
[0006] The object of the present invention is to provide a woven fabric which is extremely excellent in tearing strength in warp and weft directions even though it is light and thin.
[0007] The technical solution of the present invention is: The woven fabric of the present invention is formed by interweaving warp yarns and weft yarns, the warp yarns at least include yarns YA and YB, the weft yarns are yarns YC, and the curvature A of yarn YA, the curvature B of yarn YB, and the curvature C of yarn YC satisfy the following relationship: 0.25A≥C≥1.25B.
[0008] In the woven fabric of the present invention, the yarn YA, yarn YB and yarn YC have different curvatures and satisfy a specific relationship between the three. Such a structure increases the displacement between the yarns during the tearing process of the woven fabric, and the tearing strength can be guaranteed even for a thin and light type; at the same time, the woven fabric of the present invention also has a lower air permeability. DETAILED DESCRIPTION
[0009] Tear strength is used to evaluate the ability of fabrics to resist tearing along the crack or damage direction during use, and is one of the important factors affecting the service life of fabrics. The tear strength of fabrics includes warp tear strength and weft tear strength. Under certain conditions such as fineness, the factors affecting tear strength are the tensile length of the yarn and the number of yarns in the force triangle. The woven fabric of the present invention is interwoven by warp yarns and weft yarns, and the warp yarns at least include yarns YA and yarns YB, and the weft yarns are yarns YC. As one of the factors affecting tear strength, the longer the tensile length of the yarn, the more conducive to the improvement of tear strength. Therefore, we consider increasing the tensile length of the warp yarn by increasing the curvature of the warp yarn, but considering that if the curvature of all warp yarns is increased, kinking will occur between adjacent warp yarns, which increases the friction between the warp yarns and the weft yarns, which is not conducive to the improvement of the tensile length of the warp yarns. Therefore, the present invention requires that the yarn YA and the yarn YB used as the warp yarn have a relatively high curvature, and the yarn YB has a relatively low curvature. Another factor affecting the tear strength is the number of yarns in the stress triangle. If the weft yarn YC intersects with the warp yarns YA and YB respectively, and its curvature is too large, the contact area between the yarn YC and the yarns YA and YB will increase, and the friction between the yarns will increase, which is not conducive to the slippage of the warp yarn in the weft direction, resulting in a decrease in the number of weft yarns in the stress triangle, and the tear strength in the warp and weft directions is affected. The curvature here refers to the difference between the length of a section of yarn removed from the fabric and straightened under a specified tension and the length of the two ends of the yarn in the fabric, and the percentage of the latter.
[0010] In the warp direction, compared with yarn YA, yarn YB has a smaller curvature, and the contact area between it and yarn YC is smaller, so the friction force is relatively smaller, and the sliding displacement of this part of the warp yarn can reach a larger value, and the number of warp yarns in the force triangle area is increased, which is beneficial to the stretching of yarn YA in the warp direction, and the warp tearing strength is improved. In the present invention, the greater the difference in curvature between yarn YA and yarn YB, the greater the gap between the two on the vertical plane, the greater the degree of freedom of yarn YC, the smaller the effect of yarn YA and yarn YB on yarn YC, and even after the yarn YC is off the machine, it can still maintain a relatively straight state when it is driven in, and a lower curvature can be obtained.
[0011] The yarn YB with a lower curvature in the warp direction and the yarn YC in the weft direction are mutually perpendicular and close to their respective horizontal planes. The sliding freedom of the yarn YB in the weft direction is increased, the number of weft yarns in the force triangle area is increased, and the weft tearing strength is improved. In this way, even for light and thin fabrics, there will be no problem with the warp and weft tearing strength. Therefore, the present invention requires that the curvature A of the yarn YA, the curvature B of the yarn YB, and the curvature C of the yarn YC satisfy the following relationship: 0.25A≥C≥1.25B.
[0012] Preferably, the angle between the three adjacent yarns YC in the present invention is 110° to 160°. When the angle is greater than 160°, it may affect the difference in curvature between the yarn YA and the yarn YB, and the warp tear strength tends to decrease; when the angle is less than 110°, the weft density is extremely high, which greatly increases the contact area between the warp yarn YA and the weft yarn YC, and the friction between the two increases, that is, the degree of freedom of the weft yarn YC is restricted, and the weft tear strength tends to decrease.
[0013] Preferably, the curvature A of the yarn YA is above 25%. If the curvature A of the yarn YA is within the above range, the yarn YA has a greater stretching length during the tearing process, the yarn YB is more likely to slip, the number of warp yarns in the force triangle area increases, and the warp tearing strength is effectively improved. The curvature A is further preferably 30% to 120%, and more preferably 40% to 100%.
[0014] Preferably, the curvature B of the yarn YB is below 4%, more preferably below 3%. The smaller the curvature B of the yarn YB is, the easier it is to slip and gather, and the more it can improve the warp tear strength.
[0015] Under the same conditions, the smaller the curvature of the yarn YC, the smaller the friction between the yarn YB, that is, the smaller the restriction of the warp yarn on the slippage of the yarn YC, the more conducive to the improvement of the warp and weft tearing strength. Preferably, the curvature B of the yarn YC is less than 5%.
[0016] In the present invention, the arrangement ratio of the yarns YA and YB is not particularly limited, and can be 1:1, 2:2, etc., and the warp yarns in the same heddle are counted as 1 warp yarn. The arrangement ratio of the yarns YA and YB is preferably 1:1, so that the friction between adjacent warp yarns is relatively small, and the obtained fabric structure is more stable.
[0017] The weight of the woven fabric of the present invention is not particularly limited, and the preferred weight is 70 g / m 2 The fabric with a gram weight within this range is light and thin, and its tear strength is greatly improved, which is especially suitable for making light down jackets.
[0018] Preferably, the cover factor of the woven fabric of the present invention is greater than 1300 and less than 3000. When the cover factor is less than 1300, the density tends to decrease, and the tear strength of the fabric may be affected. When the cover factor is greater than 3000, the friction between the yarns with a larger weft density increases, and the tear strength of the fabric may decrease. The cover factor of the woven fabric of the present invention is more preferably greater than 1600 and less than 2600.
[0019] Covering factor CF = weft covering factor + warp covering factor = Dw 1 / 2 ×Mw+Dj 1 / 2 ×Mj Among them, Dw is the fineness of the weft yarn (dtex), Mw is the density in the weft direction (roots / inch); Dj is the fineness of the warp yarn (dtex), and Mj is the density in the warp direction (roots / inch).
[0020] When the warp yarn (or weft yarn) has more than two deniers, calculate the number of warp yarns (or weft yarns) of each denier within one inch, obtain the density of warp yarns of each denier (or the density of weft yarns of each denier), and then calculate the covering coefficient of warp yarns of each denier (or the covering coefficient of weft yarns of each denier) according to the formula, and sum them up as the warp covering coefficient (or weft covering coefficient).
[0021] As a preference, the ventilation capacity of the woven fabric of the present invention is 0.10 cm 3 / cm 2 ·1.50cm above sec 3 / cm 2 · sec or less. Fabrics with ventilation volume within the above range can effectively block external air and are particularly suitable for making coats and down jackets.
[0022] Preferably, the tear strength of the woven fabric of the present invention in the warp and weft directions is above 6.0 N. Such a woven fabric can well resist tearing and stretching forces from the outside, and improves durability. Even if it is a light and thin woven fabric, there is no problem with the service life.
[0023] The warp and weft yarns of the woven fabric of the present invention are not particularly limited in form and can be filament, multifilament or staple yarn. The fiber raw materials are also not particularly limited and can be natural fibers, such as cotton, linen, silk, wool, etc., or regenerated cellulose fibers, such as viscose fibers (Tencel, Lyocell, bamboo fiber), acetate fibers, etc., or synthetic fibers, such as polyester fibers (PET), polyamide fibers, polyacrylonitrile fibers, polypropylene fibers (PP), polyvinyl acetal fibers, polyvinyl chloride fibers, etc. One or more of the above fibers can be selected as needed. In the present invention, the materials of the warp and weft yarns can be the same or different. Considering the convenience of post-processing, they are preferably made of the same material.
[0024] In the present invention, the fineness of the warp and weft yarns is not particularly limited and can be reasonably selected according to the application. Considering the use in making high-end clothing, the fineness of the warp and weft yarns in the present invention is preferably 5 to 50 deniers (hereinafter referred to as D), and more preferably 10 to 30D.
[0025] The weave of the woven fabric of the present invention is not particularly limited, and can be plain, twill, satin or a variation thereof, preferably plain, so that a dimensionally stable woven fabric can be obtained. For example, when a plain weave is selected, it can be a common plain weave with one up and one down, or a special plain weave such as a warp weight plain, a weft weight plain or a square weave formed by putting two wefts or one harness double yarn into one weft.
[0026] The woven fabric of the present invention has no particular limitation on its manufacturing method and can be obtained by the following method: yarns YA and YB are selected as warp yarns and yarn YC is used as weft yarns to weave a grey cloth, and then scouring, dyeing, drying, shaping and other processes are performed to obtain the product.
[0027] The loom used for weaving is not particularly limited, and water jet looms, air jet looms, rapier looms, etc. can be used. During the weaving process, the earlier the opening time, the greater the warp tension at the cloth fell. At the same time, because the closing time is early, the clamped weft length is longer, and the weft yarn YC is easier to buckle. Therefore, the preferred opening time is 350° to 5° to ensure a low buckling rate of the yarn YC.
[0028] In the drying process, the temperature is preferably 130 to 150° C., and the cloth feeding speed is preferably 60 to 100 m / min.
[0029] In the shaping process, excessive stretching in the weft direction will increase the weft stress and affect the curvature of the yarn YC. It is preferred that the width of the shaping machine be set to +2% to +3% of the fabric width; at the same time, a certain amount of overfeeding should be added in the warp direction to ensure that the relationship between the warp yarns YA and YB is not destroyed. The overfeeding is generally controlled at 3% to 5%. The shaping process temperature is preferably 160 to 180°C, and the fabric feeding speed is preferably 60 to 80 m / min.
[0030] In order to further improve the tear strength, the present invention preferably performs resin processing between drying and setting. The use of resin can reduce the friction between fibers and yarns, improve the mobility between fibers and yarns, and thus improve the tear strength. The type of resin is not particularly limited, and can be a hydrophilic resin, a soft resin, a waterproof resin, etc., which can be selected according to needs. The hydrophilic resin here specifically includes polyurethane, polyether, polyacrylate resin, etc., and the dosage is preferably 10-40g / L; the soft resin specifically includes silicone, silicone oil, etc., and the dosage is preferably 8-25g / L; the waterproof resin includes fluorocarbon, silicone, melamine, etc., and the dosage is preferably 40-70g / L. When used as a down jacket fabric, it is preferably processed with soft resin and waterproof resin at the same time.
[0031] In the present invention, calendering is preferably performed, which can be single-sided calendering or double-sided calendering. After calendering, the gaps between the yarns are reduced, and the down-proof property is more excellent as a down jacket fabric. The material of the heated roller surface for calendering is not particularly limited, and it can be a fiber roller or a polyamide plastic roller. The calendering pressure is preferably 4 to 10 kgf, the calendering temperature is preferably cold pressing to 220°C, and the number of calendering times is preferably 1 to 4 times. The calendering pressure is more preferably 4 to 6 kgf, and the calendering temperature is more preferably 140°C to 220°C.
[0032] The present invention is further described below in conjunction with examples and comparative examples, but the protection scope of the present invention is not limited to the examples. The physical property parameters in the examples are measured by the following methods.
[0033] (1) Density in longitude and latitude Tested according to JIS L 1096-2010 8.6.
[0034] (2) Buckling rate Tested according to JIS L 1096-2010 8.7 (Method B).
[0035] (3) Coverage factor CF=Dw 1 / 2 ×Mw+Dj 1 / 2 ×Mj, Where Dw is the fineness of the weft yarn (dtex); Mw is the density in the weft direction (roots / inch); Dj is the warp yarn fineness (dtex); Mj is the density in the warp direction (roots / inch).
[0036] (4) Weight Tested according to JIS L 1096-2010.
[0037] (5) Ventilation volume Tested according to JIS L 1096-1999.
[0038] (6) Tearing strength Tested according to GB / T 3917.1-2009 (Pendulum method).
[0039] (7) Anti-down property The test was carried out according to the friction method in Appendix E of GB / T 14272-2011.
[0040] (8) Angle between three adjacent yarns YC Prepare 3 samples of cloth that are flat and wrinkle-free and are 1cm*1cm in size. Take one of the samples, cut it along the warp yarn with a blade under a microscope to obtain the sample to be tested, and fix the sample to be tested on the test table. Be careful not to press the sample to be tested. Take a SEM photo of the weft section of the sample to be tested (with a magnification of 150 times), and pay attention to adjust the sample to be tested in a horizontal position and the section cannot be tilted. Mark the center of the cross section of three adjacent weft yarns on the SEM photo, connect the angle of the three centers with a straight line and measure the angle, and then arbitrarily select two angles on the SEM photo for measurement to obtain 3 sets of data. Measure the remaining two samples in the same way, and obtain a total of 9 sets of data, and take the average value as the angle between the three adjacent yarns YC of the present invention.
[0041] The following examples and comparative examples are used in the following pharmaceutical compositions: Softener: RUCO FIN SIQ, manufactured by Rudolf Chemical (Nantong) Co., Ltd. Waterproofing agent: RUCO-DRY DHT, manufactured by Rudolf Chemical (Nantong) Co., Ltd.
[0042] Embodiment 01: The warp yarns YA and YB and the weft yarns YC are all made of 15D / 36f PET DTY, and are woven in plain weave. The arrangement ratio of the yarns YA and YB is 1:1. The weaving tensions of the yarns YA and YB are 6 cN / root and 24 cN / root, respectively. The beating opening time is 350°. The weaving density is 180 roots / inch in the warp direction and 196 roots / inch in the weft direction to obtain a grey cloth.
[0043] The grey cloth is then scourged (temperature 90°C, time 20min) → dyed (disperse dyeing 135°C*30min) → reduced cleaning (80°C*20min) → dried (temperature 130°C, speed 80m / min) → resin processed (softener dosage: 18g / L, waterproofing agent dosage: 60g / L) → shaped (temperature 160°C, time 1min, overfeed rate +3%, width +2%) → calendered (single side 2 times, temperature 175°C, pressure 5kgf, speed 20m / min) to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0044] Embodiment 02: During weaving, the tension of the yarn YA was 4 cN / yarn, and the rest was the same as in Example 01 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0045] Embodiment 03: During weaving, the tension of the yarn YA was 10 cN / yarn, and the rest was the same as in Example 01 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0046] Embodiment 04: During weaving, the tensions of the yarn YA and the yarn YB were 12 cN / yarn and 22 cN / yarn respectively, and the rest was the same as in Example 01, to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0047] Embodiment 05: During weaving, the tension of the yarn YA was 16 cN / yarn, and the rest was the same as in Example 01 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0048] Embodiment 06: During weaving, the tension of the yarn YA was 8 cN / yarn, and the rest was the same as in Example 03 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0049] Embodiment 07: During weaving, the tensions of the yarn YA and the yarn YB were 12 cN / yarn and 23 cN / yarn respectively, and the rest was the same as in Example 03, to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0050] Embodiment 08: During weaving, the ratio of yarn YA to yarn YB was 2:2, and the rest was the same as in Example 04 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0051] Embodiment 09: 35D / 288f sea-island composite fibers were selected as warp and weft yarns for weaving, that is, yarn YA, yarn YB and yarn YC were all the sea-island composite fibers mentioned above, wherein the sea component was COPET, the island component was PBT and PET (50:50), the composite ratio of the sea component to the island component was 16:84, the weaving density was 125 strands / inch in the warp direction and 145 strands / inch in the weft direction, and the grey cloth was obtained, and the grey cloth was further refined → reduced (dosage of caustic soda NaOH: 20 g / L, temperature 80°C, time 120 min) → dyed → reduced cleaning → dried → resin processed → shaped → calendered, and the rest was the same as in Example 04, to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0052] Embodiment 10: 10D / 24f PET DTY was selected as the warp and weft yarns for weaving, that is, the yarn YA, the yarn YB and the yarn YC were all the above-mentioned PET DTY, the weaving density was 212 yarns / inch in the warp direction and 250 yarns / inch in the weft direction, and the grey cloth was obtained. The rest was the same as in Example 04, and the woven fabric of the present invention was obtained. The specific parameters are shown in Table 1.
[0053] Embodiment 11: During weaving, the beating-up opening time was 330°, and the rest was the same as in Example 09 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 1.
[0054] Embodiment 12: During weaving, the weaving density was 165 strands / inch in the warp direction and 180 strands / inch in the weft direction to obtain a grey cloth, and the rest was the same as in Example 09 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0055] Embodiment 13: During weaving, the weaving density was 190 strands / inch in the warp direction and 212 strands / inch in the weft direction to obtain a grey cloth, and the rest was the same as in Example 09 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0056] Embodiment 14: During weaving, the tensions of the yarn YA and the yarn YB were 12 cN / yarn and 32 cN / yarn respectively, and the rest was the same as in Example 03 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0057] Embodiment 15: During weaving, the tensions of the yarn YA and the yarn YB were 12 cN / yarn and 28 cN / yarn respectively, and the rest was the same as in Example 03 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0058] Embodiment 16: During weaving, the tensions of the yarns YA and YB were 12 cN / yarn and 24 cN / yarn respectively, and the rest was the same as in Example 03 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0059] Embodiment 17: During weaving, the tensions of the yarn YA and the yarn YB were 12 cN / yarn and 20 cN / yarn respectively, and the rest was the same as in Example 03 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0060] Embodiment 18: During weaving, the tensions of the yarn YA and the yarn YB were 14 cN / yarn and 18 cN / yarn respectively, and the rest was the same as in Example 05 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0061] Embodiment 19: During weaving, the tensions of the yarn YA and the yarn YB were 12 cN / yarn and 16 cN / yarn respectively, and the rest was the same as in Example 05 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0062] Embodiment 20: During weaving, one side was calendered 3 times, and the rest was the same as in Example 03 to obtain the woven fabric of the present invention. Specific parameters are shown in Table 2.
[0063] Comparative Example 01: During weaving, the tension of yarn YA and yarn YB was 3 cN / strand, and the rest was the same as in Example 03 to obtain a woven fabric. Specific parameters are shown in Table 2.
[0064] Table 1
[0065] Table 2
[0066] According to Tables 1 and 2 above, (1) It can be seen from Example 05 and Example 18 that, under the same conditions, the woven fabric with a curvature A of 37% has a similar weight to the woven fabric with a curvature A of 25%. Although the air permeability of the former is higher than that of the latter, the tear strength is significantly higher than that of the latter.
[0067] (2) It can be seen from Examples 16 and 17 that, under the same conditions, the woven fabric in which the angle between three adjacent yarns YC is 155° is comparable to the woven fabric in which the angle between three adjacent yarns YC is 162°. Although the air permeability of the former is slightly higher than that of the latter, the tear strength is significantly higher than that of the latter.
[0068] (3) It can be seen from Example 15 and Example 14 that, under the same conditions, the woven fabric in which the angle between three adjacent yarns YC is 119° is compared with the woven fabric in which the angle between three adjacent yarns YC is 107°. The weights of the two are equivalent, the air permeability of the former is lower than that of the latter, and the tear strength is higher than that of the latter.
[0069] (4) It can be seen from Example 18 and Example 19 that, under the same conditions, the woven fabric with a curvature A of 25% has a similar weight and air permeability to the woven fabric with a curvature A of 20%, but the tear strength of the former is higher than that of the latter.
[0070] (5) It can be seen from Example 03 and Example 07 that, under the same conditions, the woven fabric with a curvature C of 5% is comparable to the woven fabric with a curvature C of 6%, and the tear strength of the former is significantly higher than that of the latter.
[0071] (6) It can be seen from Comparative Example 01 and Example 03 that, under the same conditions, the woven fabric with C / A of 0.86 and C / B of 0.86 is compared with the woven fabric with C / A of 0.09 and C / B of 1.67. Although the gram weight of the former is lower than that of the latter and the air permeability is also lower than that of the latter, the tear strength is much lower than that of the latter and is not as durable.
Claims
1. A woven fabric, formed by interweaving warp yarns and weft yarns, characterized in that: The warp yarn includes at least yarn YA and yarn YB, the weft yarn is yarn YC, and the curvature A of yarn YA, the curvature B of yarn YB, and the curvature C of yarn YC satisfy the following relationship: 0.25A≥C≥1.25B.
2. The woven fabric according to claim 1, characterized in that: The angle between three adjacent yarns YC is 110° to 160°.
3. The woven fabric according to claim 1, characterized in that: The buckling rate A is above 25%.
4. The woven fabric according to claim 1, characterized in that: The buckling rate C is below 5%.
5. The woven fabric according to any one of claims 1 to 4, characterized in that: The woven fabric has a grammage of 70 g / m 2 the following.
6. The woven fabric according to any one of claims 1 to 4, characterized in that: The tearing strength of the woven fabric in the warp and weft directions is both above 6.0N.