Post-buckling fatigue characteristic test method for laminated board containing impact damage
By controlling the strain difference of the laminate at the impact damage position and using the pressure-pressure cycle loading method to perform fatigue tests, the post-buckling fatigue characteristics of the composite material under impact damage were verified, and the application and safety of the composite material in the aircraft structure was solved. The problem provides an effective experimental basis.
Patent Information
- Application Number
- CN202410926110.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
The post-buckling fatigue characteristics of composite materials in impact damage are difficult to effectively verify, affecting their application and safety in aircraft structures.
A test method for post-buckling fatigue characteristics of the laminate containing impact damage is adopted. By controlling the difference in strain of the laminate at the front and back surfaces of the impact damage position, it repeatedly enters the post-buckling state, and the fatigue test is carried out through the pressure-pressure cycle loading method. Monitor the damage expansion and determine the post-buckling fatigue characteristics.
It provides a test basis to help composite materials be better applied in civil aircraft structures and ensure their remaining load-bearing capacity and airworthiness under extreme load loads.
Smart Images

Figure CN118896860A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite material strength design and verification, and in particular relates to a post-buckling fatigue property test method for a laminate containing impact damage. Background Art
[0002] Compared with metal structures, composite structures have the advantages of high specific strength, good overall formability, and high designability. In recent years, the application technology of composite materials in civil aircraft has rapidly improved. The new generation of large civil aircraft Boeing 787 and Airbus A350XWB aircraft, the amount of composite materials accounts for 50% and 52% of the fuselage structure weight respectively, and their fuselage, wings and tail wings are all made of a large amount of high-strength carbon fiber composite materials. The proportion of composite materials used in domestic civil aircraft has also increased significantly. The ARJ21-700 aircraft uses composite materials in the winglets, rudders, wing-body fairings and radomes, and the C919 aircraft uses composite materials in the tail, rear fuselage, rear pressure frame and other parts. The amount of composite materials used in the C929 aircraft under development by COMAC will reach the level of Boeing 787.
[0003] At the same time, composite materials also have disadvantages such as complex manufacturing process, large dispersion of material properties, sensitivity to the environment, low impact resistance, and poor out-of-plane load-bearing capacity. Therefore, in the design of composite materials for civil aircraft, it is often necessary to consider the effects of damage and repeated loads at the same time, and verify that the composite materials still have a certain residual load-bearing capacity (can maintain the ultimate load during the life of the aircraft structure\the damage should not expand, or if there is slow expansion or cracking, the residual strength level within the test period must be sufficient to exceed the limit load capacity\have the ability to withstand the limit load or close to the limit load) under the condition of a certain degree of impact damage (BVID\VID\large VID), so as to show that the strength of the composite material structure complies with the airworthiness standards.
[0004] The commonly used composite material structure for domestic aircraft is the reinforced wall panel structure. Relevant research shows that composite laminates still have strong post-buckling bearing capacity after buckling. Making full use of the post-buckling bearing capacity of composite materials is conducive to reducing the weight of aircraft and improving overall performance and economic benefits.
[0005] In summary, it is very important to conduct experimental exploration on the post-buckling fatigue properties of laminates containing impact damage. Summary of the invention
[0006] The purpose of the present invention is to provide a test method for post-buckling fatigue characteristics of impact-damaged laminates. The present invention can provide a test basis for post-buckling fatigue analysis of impact-damaged laminates, so that composite materials can be better applied in civil aircraft structures.
[0007] The technical solution of the present invention is: a test method for post-buckling fatigue characteristics of impact-damaged laminates, which controls the strain difference between the front and back surfaces of the laminates at the impact damage position so that the laminates repeatedly enter the desired post-buckling state to obtain the post-buckling fatigue characteristics of the impact-damaged laminates.
[0008] The aforementioned post-buckling fatigue property test method of the impact-damaged laminate comprises the following steps:
[0009] Step 1: Divide the laminates with the same geometric parameters into three groups, one of which is used as static test pieces of non-destructive laminates, one is used as static test pieces of laminates with impact damage, and one is used as fatigue test pieces of laminates with impact damage;
[0010] Step 2: Introduce impact damage into the static test piece of the laminate with impact damage and the fatigue test piece of the laminate with impact damage; after the impact, perform ultrasonic nondestructive testing on each test piece with impact damage introduced, and record the pit depth and damage range of each test piece;
[0011] Step 3: Conduct a static compression test on the non-destructive laminate static test piece;
[0012] Step 4: Conduct a static compression test on the static test piece of the impact-damaged laminate;
[0013] Step 5: Selection of post-buckling fatigue test load;
[0014] Step 6: Perform post-buckling fatigue property test on the fatigue specimen of the impact-damaged laminate by compression-compression cyclic loading. Ultrasonic non-destructive testing is performed before, after and at specified cycles during the test to monitor damage propagation.
[0015] In the aforementioned post-buckling fatigue property test method of impact-damaged laminates, in step 1, the geometric parameters of the laminates are selected based on the ASTM D 7136 standard.
[0016] In the aforementioned post-buckling fatigue properties test method for impact-damaged laminates, in step 1, the number of laminates in each group is 3.
[0017] In the aforementioned post-buckling fatigue property test method of impact-damaged laminated plates, in step 2, the impact damage introduction method is performed based on the ASTM D 7136 standard.
[0018] In the aforementioned post-buckling fatigue properties test method for impact-damaged laminates, step 3 comprises the following steps:
[0019] Step 3.1: Paste the strain gauge on the surface of the non-destructive laminate static test piece to obtain strain feedback during the test;
[0020] Step 3.2: Installation and loading commissioning of static compression test specimens of non-destructive laminates: Each specimen of the non-destructive static test is installed according to the ASTM D 7137 standard and loaded and commissioned at a preset loading rate. The commissioning requires that when the average strain value displayed by the back-to-back strain gauges of the specimens other than the center point is 1000με, the bending percentage does not exceed 10%;
[0021] Step 3.3: Loading of static compression test of non-destructive laminate. Load at a certain loading rate until the specimen is destroyed. Before destruction, the strain curve should be observed in real time to find obvious buckling of the specimen. At the same time, the strain gauge data, test load, displacement and other data should be collected.
[0022] Step 3.4: Record the failure mode and failure load of the static test piece of the non-destructive laminate.
[0023] In the aforementioned post-buckling fatigue properties test method for impact-damaged laminates, in step 3.2, the bending percentage is calculated as follows:
[0024]
[0025] Wherein: ε1 and ε3 are the strain gauge readings at two locations on the upper surface of the static test piece of the non-destructive laminate, respectively; ε2 and ε4 are the strain gauge readings at two locations on the lower surface of the static test piece of the non-destructive laminate, respectively; among them, the strain gauges corresponding to ε1 and ε2 are pasted back to back, and the strain gauges corresponding to ε3 and ε4 are pasted back to back.
[0026] In the aforementioned post-buckling fatigue properties test method for impact-damaged laminates, step 4 comprises the following steps:
[0027] Step 4.1: Paste strain gauges on static test pieces of impact-damaged laminates: Paste strain gauges on the surface of the test piece to obtain strain feedback during the test;
[0028] Step 4.2: Installation and loading commissioning of static compression test of impact damaged laminates: Each specimen of the static test is installed according to ASTM D 7137 standard and loaded and commissioned at a preset loading rate. The commissioning requires that when the average strain value displayed by the back-to-back strain gauges at the center point of the specimen is 1000με, the bending percentage does not exceed 10%;
[0029] Step 4.3: Loading of static compression test of impact-damaged laminate: Load at a preset loading rate until the specimen is destroyed. Before destruction, the specimen must be observed to observe the strain curve in real time to find obvious buckling. At the same time, strain gauge data, test load, and displacement data are collected;
[0030] Step 4.4: Record the failure mode and failure load of the static test piece of the impact-damaged laminate.
[0031] In the aforementioned post-buckling fatigue property test method of impact-damaged laminated panels, step 5 comprises the following steps:
[0032] Step 5.1: According to the test requirements, the strain difference required for post-buckling fatigue load should be determined and defined as the target strain difference Δε c , and determine the stress ratio, total number of cycles and number of test cycles;
[0033] Step 5.2: Count the average strain difference values corresponding to the other two back-to-back strain gauge positions when the back-to-back strain difference value of the center point of each non-destructive laminate static test piece reaches the target strain difference value, and then average the average values of the two positions to obtain the target strain average value Δε a ;
[0034] Step 5.3: Calculate the average strain difference between the two back-to-back strain gauge positions of each static test piece of impact-damaged laminate to reach Δε a The load at that time is averaged to obtain the target load F a , F a This is the minimum value of the post-buckling compression-compression fatigue load.
[0035] In the aforementioned post-buckling fatigue properties test method for impact-damaged laminates, step 6 comprises the following steps:
[0036] Step 6.1: Installation and loading commissioning of post-buckling fatigue test of laminate with impact damage: Each fatigue test piece of laminate with impact damage in the post-buckling fatigue test is installed according to ASTM D 7137 standard and loaded and commissioned at a preset loading rate. It is required that when the average strain value displayed by the back-to-back strain gauges at the center point of the test piece is 1000με, the bending percentage shall not exceed 10%;
[0037] Step 6.2: Load according to the fatigue load, stress ratio, and number of cycles determined in step 5. The loading frequency is adjusted according to the test conditions. The heating effect inside the test piece should be avoided so that the surface temperature of the test piece does not change.
[0038] Step 6.3: During the test, according to the number of test cycles determined in step 5, when the corresponding number of cycles is reached, ultrasonic nondestructive testing is performed on the test piece to monitor the damage extension of the test piece;
[0039] Step 6.4: After the fatigue test, perform ultrasonic nondestructive testing on the test piece to determine whether the damage does not extend or extends slowly within the specified cycle.
[0040] The advantages of the present invention are: the post-buckling fatigue characteristics test method of the laminate containing impact damage proposed by the present invention controls the strain difference between the front and back surfaces of the laminate at the impact damage position to make it repeatedly enter the required post-buckling state, and after a certain number of fatigue tests, the post-buckling fatigue characteristics of the laminate containing impact damage are obtained, which provides an experimental basis for the post-buckling fatigue analysis of the laminate containing impact damage and enables better application of composite materials in civil aircraft structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is a schematic diagram of the impact damage position of the impact-damaged laminate test piece;
[0042] Figure 2 Schematic diagram of strain gauge pasting on non-destructive laminate test piece;
[0043] Figure 3 Schematic diagram of strain gauge pasting on impact damaged laminate test piece;
[0044] Figure 4 It is a test flow chart of the present invention. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0046] The features and illustrative embodiments of various aspects of the present invention will be described in detail below. In the detailed description below, many specific details are proposed to provide a comprehensive understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present invention by illustrating examples of the present invention. The present invention is by no means limited to any specific settings and methods proposed below, but covers any improvements, replacements and modifications of structures, methods, devices without departing from the spirit of the present invention. In the accompanying drawings and the following description, known structures and technologies are not shown to avoid unnecessary ambiguity in the present invention.
[0047] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other, and the embodiments can refer to and quote each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0048] Example 1. A post-buckling fatigue test method for impact-damaged laminates, see Figure 1-Figure 4 By controlling the strain difference between the front and back surfaces of the laminate at the impact damage position, the laminate is repeatedly put into the desired post-buckling state, and the post-buckling fatigue properties of the laminate containing impact damage are obtained. The following steps are included:
[0049] Step 1: Plan the test matrix. Each laminate configuration that needs to be tested for post-buckling fatigue properties of impact-damaged laminates must include at least 3 static test pieces of non-destructive laminates, 3 static test pieces of impact-damaged laminates, and 3 fatigue test pieces of impact-damaged laminates with the same geometric parameters. The geometric parameters of the test pieces can refer to the ASTM D 7136 standard.
[0050] Step 2: Impact damage introduction. For the impact-damaged laminate test piece, impact damage introduction is performed. The impact damage introduction method can refer to ASTM D 7136. After the impact, ultrasonic nondestructive testing is performed on each test piece with impact damage introduction, and the pit depth and damage range of each test piece are recorded.
[0051] For each laminate configuration that requires post-buckling fatigue testing of impact damaged laminates, perform steps 3 through 6.
[0052] Step 3: Static compression test of non-destructive laminate specimens.
[0053] Step 4: Static compression test of the impact damaged laminate specimen.
[0054] Step 5: Selection of post-buckling fatigue test load.
[0055] Step 6: Post-buckling fatigue test of impact damaged laminates. Post-buckling fatigue test is carried out by compression-compression cyclic loading. Ultrasonic non-destructive testing is performed before and after the test and at specified cycles during the test to monitor damage propagation.
[0056] The step 3 comprises the following steps:
[0057] Step 3.1: Attach strain gauges to the static test specimen of non-destructive laminates. Attach strain gauges to the surface of the test specimen to obtain strain feedback during the test.
[0058] Step 3.2: Installation and loading commissioning of static compression test of non-destructive laminate. Each specimen of non-destructive static test is installed according to ASTM D 7137 standard and loaded and commissioned at a certain loading rate. It is required that when the average strain value displayed by the back-to-back strain gauges (numbered 01 / 02, 03 / 04) except the center point of the specimen is 1000με, the bending percentage shall not exceed 10%. The control of the bending percentage in this step is to prevent the specimen from buckling prematurely and control the dispersion of the buckling load. At this time, the bending percentage is defined as follows:
[0059]
[0060] Where:
[0061] ε1——strain gauge reading No. 01;
[0062] ε2——strain gauge reading No. 02;
[0063] ε3——strain gauge reading No. 03;
[0064] ε4——Strain gauge reading number 04.
[0065] Step 3.3: Loading of static compression test of non-destructive laminate. Load at a certain loading rate until the specimen is destroyed. Before destruction, the strain curve should be observed in real time to find obvious buckling of the specimen. At the same time, the strain gauge data, test load, displacement and other data should be collected.
[0066] Step 3.4: Record the failure mode and failure load of the static test piece of the non-destructive laminate.
[0067] The step 4 comprises the following steps:
[0068] Step 4.1: Paste the strain gauge on the static test piece of impact-damaged laminate. Paste the strain gauge on the surface of the test piece to obtain strain feedback during the test. See the attached diagram for the specimen strain gauge pasting. Figure 3 .
[0069] Step 4.2: Installation and loading commissioning of static compression test of impact damaged laminate. Each specimen of the static test is installed according to ASTM D 7137 standard and loaded and commissioned at a certain loading rate. It is required that when the average strain value displayed by the back-to-back strain gauges (numbered 01 / 02, 03 / 04) at the center of the specimen is 1000με, the bending percentage shall not exceed 10%. The control of the bending percentage in this step is to prevent the specimen from buckling prematurely and to control the dispersion of the buckling load. The bending percentage definition at this time is the same as step 3.2.
[0070] Step 4.3: Loading of static compression test of impact damaged laminates. Load at a certain loading rate until the specimen is destroyed. Before destruction, the strain curve should be observed in real time to find obvious buckling of the specimen. At the same time, the strain gauge data, test load, displacement and other data should be collected.
[0071] Step 4.4: Record the failure mode and failure load of the static test piece of the impact-damaged laminate.
[0072] The step 5 comprises the following steps:
[0073] Step 5.1: According to the test requirements, the strain difference required for post-buckling fatigue load should be determined and defined as the target strain difference Δε c , and determine the stress ratio, total number of cycles and number of test inspection cycles.
[0074] Step 5.2: Count the average strain difference values corresponding to the other two back-to-back strain gauge positions (strain gauge No. 01 / 02 and strain gauge No. 03 / 04) when the back-to-back strain difference value of the center point of each non-destructive laminate static test piece (strain gauge No. 05 / 06) reaches the target strain difference value, and record them as the average value Δε a1 , ..., Δε an , the average is called the target strain average value Δε a .
[0075] Step 5.3: Count the average strain difference values corresponding to the two back-to-back strain gauge positions (strain gauges 01 / 02 and strain gauges 03 / 04) of each static test piece of impact-damaged laminate to reach Δε a The load at that time is denoted as F a1 ,……,F an , the average is called the target load F a , F a This is the minimum value of the post-buckling compression-compression fatigue load.
[0076] The step 6 comprises the following steps:
[0077] Step 6.1: Perform ultrasonic nondestructive testing on the fatigue test piece of the impact-damaged laminate, and mark the pit depth and damage range.
[0078] Step 6.2: Installation and loading commissioning of post-buckling fatigue test of impact damaged laminate. Each specimen of the post-buckling fatigue test is installed according to ASTM D 7137 standard and loaded and commissioned at a certain loading rate. It is required that when the average strain value displayed by the back-to-back strain gauges (numbered 01 / 02, 03 / 04) at the center of the specimen is 1000με, the bending percentage shall not exceed 10%. The control of the bending percentage in this step is to prevent the specimen from buckling prematurely and to control the dispersion of the buckling load. The bending percentage definition at this time is the same as step 3.2.
[0079] Step 6.3: Load according to the fatigue load, stress ratio, and number of cycles determined in step 5. The loading frequency can be adjusted according to the test conditions. The influence of heating inside the test piece should be avoided so that the surface temperature of the test piece does not change.
[0080] Step 6.4: During the test, according to the number of test cycles determined in step 5, when the corresponding number of cycles is reached, ultrasonic nondestructive testing is performed on the test piece to monitor the damage extension of the test piece.
[0081] Step 6.5: After the fatigue test, perform ultrasonic nondestructive testing on the test piece to determine whether the damage does not extend or extends slowly within the specified cycle.
[0082] Example 2. A method for testing post-buckling fatigue properties of impact-damaged laminates. Figure 1-Figure 4 As shown,
[0083] 1. Plan the test matrix according to the test needs. Table 1 is the test matrix table of this embodiment, which ensures that each laminate configuration that needs to undergo post-buckling fatigue property test of impact-damaged laminates must include at least 3 static test pieces of non-destructive laminates with the same geometric parameters, 3 static test pieces of impact-damaged laminates, and 3 fatigue test pieces of impact-damaged laminates, and the number of additional spare parts is used to control the depth of the impact damage pit.
[0084] Table 1
[0085]
[0086] 2. Impact damage introduction. With reference to the ASTM D 7136 standard, impact damage introduction was performed on the impact-damaged laminate test piece. In this embodiment, a hemispherical punch with a diameter of 16 mm produced a pit with a depth of 1.0 mm to 1.2 mm (measured immediately after impact). After impact, ultrasonic nondestructive testing was performed on each test piece with impact damage introduction, and the pit depth and damage range of each test piece were recorded.
[0087] For each laminate configuration that needs to be tested for post-buckling fatigue properties of impact-damaged laminates in this embodiment, steps 3 to 6 are performed. The specific steps are as follows:
[0088] 3. Static compression test of non-destructive laminate test piece. The static compression test of the non-destructive laminate test piece is carried out according to steps 3.1 to 3.4 of Example 1. In this example, the certain loading rate adopted in steps 3.2 and 3.3 is 1.25 mm / min.
[0089] 4. Static compression test of impact-damaged laminate test piece. According to the above steps 4.1 to 4.4, the static compression test of the impact-damaged laminate test piece is carried out. In this embodiment, the certain loading rate adopted in steps 4.2 and 4.3 is 1.25 mm / min.
[0090] 5. Selection of post-buckling fatigue test load. The post-buckling fatigue test load is selected according to steps 5.1 to 5.3 of Example 1. In this example, the target strain difference Δε c =400με, stress ratio R=0.06, total number of cycles is 10 6 , every 10 5 In this embodiment, the target strain average value Δε is obtained. a 、Target load F a As shown in Table 2:
[0091] Configuration number <![CDATA[Target strain average value Δε a (με)]]> <![CDATA[Target load F a (kN)]]> I 178.5 -7.7 II 178.25 -12.5 III 357.3 -21.5
[0092] Step 6: Post-buckling fatigue test of laminates with impact damage. The post-buckling fatigue test is carried out by compression-compression cyclic loading. Ultrasonic non-destructive testing is performed before and after the test and for a specified number of cycles during the test to monitor the damage extension. According to Steps 6.1 to 6.5 of Example 1, the post-buckling fatigue test of laminates with impact damage is carried out. The comparison of the ultrasonic non-destructive testing results before, during and after the test of this example shows that the test piece is 10 6 During the second cycle, the damage did not extend.
[0093] The post-buckling fatigue properties of the laminate containing impact damage obtained in this embodiment can provide an experimental basis for the post-buckling fatigue analysis of the laminate containing impact damage.
[0094] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the field can easily think of various equivalent modifications or substitutions within the technical scope disclosed by the present invention, and these modifications or substitutions should all be covered within the protection scope of the present invention.
Claims
1. A post-buckling fatigue test method for impact-damaged laminates, characterized in that: By controlling the strain difference between the front and back surfaces of the laminate at the impact damage position, the laminate is repeatedly put into the desired post-buckling state, and the post-buckling fatigue properties of the laminate with impact damage are obtained.
2. The post-buckling fatigue properties test method of impact-damaged laminated plates according to claim 1, characterized in that: The following steps are involved: Step 1: Divide the laminates with the same geometric parameters into three groups, one of which is used as static test pieces of non-destructive laminates, one is used as static test pieces of laminates with impact damage, and one is used as fatigue test pieces of laminates with impact damage; Step 2: Introduce impact damage into the static test piece of the laminate with impact damage and the fatigue test piece of the laminate with impact damage; after the impact, perform ultrasonic nondestructive testing on each test piece with impact damage introduced, and record the pit depth and damage range of each test piece; Step 3: Conduct a static compression test on the non-destructive laminate static test piece; Step 4: Conduct a static compression test on the static test piece of the impact-damaged laminate; Step 5: Selection of post-buckling fatigue test load; Step 6: Perform post-buckling fatigue property test on the fatigue specimen of the impact-damaged laminate by compression-compression cyclic loading. Ultrasonic non-destructive testing is performed before, after and at specified cycles during the test to monitor damage propagation.
3. The post-buckling fatigue properties test method of impact-damaged laminated plates according to claim 2, characterized in that: In step 1, the geometric parameters of the laminate are selected based on the ASTM D 7136 standard.
4. The post-buckling fatigue property test method of impact-damaged laminated plates according to claim 2, characterized in that: In step 1, the number of laminates in each group is 3.
5. The post-buckling fatigue property test method of impact-damaged laminated plates according to claim 2, characterized in that: In step 2, the impact damage introduction method is performed based on the ASTM D 7136 standard.
6. The post-buckling fatigue property test method of impact-damaged laminated plates according to claim 2, characterized in that: Step 3 includes the following steps: Step 3.1: Paste the strain gauge on the surface of the non-destructive laminate static test piece to obtain strain feedback during the test; Step 3.2: Installation and loading commissioning of static compression test specimens of non-destructive laminates: Each specimen of the non-destructive static test is installed according to the ASTM D 7137 standard and loaded and commissioned at a preset loading rate. The commissioning requires that when the average strain value displayed by the back-to-back strain gauges of the specimens other than the center point is 1000με, the bending percentage does not exceed 10%; Step 3.3: Loading of static compression test of non-destructive laminate. Load at a certain loading rate until the specimen is destroyed. Before destruction, the strain curve should be observed in real time to find obvious buckling of the specimen. At the same time, the strain gauge data, test load, displacement and other data should be collected. Step 3.4: Record the failure mode and failure load of the static test piece of the non-destructive laminate.
7. The post-buckling fatigue property test method of impact-damaged laminated plates according to claim 6, characterized in that: In step 3.2, the bending percentage is calculated as follows: Wherein: ε1 and ε3 are the strain gauge readings at two locations on the upper surface of the static test piece of the non-destructive laminate, respectively; ε2 and ε4 are the strain gauge readings at two locations on the lower surface of the static test piece of the non-destructive laminate, respectively; among them, the strain gauges corresponding to ε1 and ε2 are pasted back to back, and the strain gauges corresponding to ε3 and ε4 are pasted back to back.
8. The post-buckling fatigue property test method of impact-damaged laminated plates according to claim 2, characterized in that: Step 4 includes the following steps: Step 4.1: Paste strain gauges on static test pieces of impact-damaged laminates: Paste strain gauges on the surface of the test piece to obtain strain feedback during the test; Step 4.2: Installation and loading commissioning of static compression test of impact damaged laminates: Each specimen of the static test is installed according to ASTM D 7137 standard and loaded and commissioned at a preset loading rate. The commissioning requires that when the average strain value displayed by the back-to-back strain gauges at the center point of the specimen is 1000με, the bending percentage does not exceed 10%; Step 4.3: Loading of static compression test of impact-damaged laminate: Load at a preset loading rate until the specimen is destroyed. Before destruction, the specimen must be observed to observe the strain curve in real time to find obvious buckling. At the same time, strain gauge data, test load, and displacement data are collected; Step 4.4: Record the failure mode and failure load of the static test piece of the impact-damaged laminate.
9. The post-buckling fatigue property test method of impact-damaged laminated plates according to claim 2, characterized in that: Step 5 includes the following steps: Step 5.1: According to the test requirements, the strain difference required for post-buckling fatigue load should be determined and defined as the target strain difference Δε c , and determine the stress ratio, total number of cycles and number of test cycles; Step 5.2: Count the average strain difference values corresponding to the other two back-to-back strain gauge positions when the back-to-back strain difference value of the center point of each non-destructive laminate static test piece reaches the target strain difference value, and then average the average values of the two positions to obtain the target strain average value Δε a ; Step 5.3: Calculate the average strain difference between the two back-to-back strain gauge positions of each static test piece of impact-damaged laminate to reach Δε a The load at that time is averaged to obtain the target load F a , F a This is the minimum value of the post-buckling compression-compression fatigue load.
10. The post-buckling fatigue property test method of impact-damaged laminated plates according to claim 2, characterized in that: Step 6 includes the following steps: Step 6.1: Installation and loading commissioning of post-buckling fatigue test of laminate with impact damage: Each fatigue test piece of laminate with impact damage in the post-buckling fatigue test is installed according to ASTM D 7137 standard and loaded and commissioned at a preset loading rate. It is required that when the average strain value displayed by the back-to-back strain gauges at the center point of the test piece is 1000με, the bending percentage shall not exceed 10%; Step 6.2: Load according to the fatigue load, stress ratio, and number of cycles determined in step 5. The loading frequency is adjusted according to the test conditions. The heating effect inside the test piece should be avoided so that the surface temperature of the test piece does not change. Step 6.3: During the test, according to the number of test cycles determined in step 5, when the corresponding number of cycles is reached, ultrasonic nondestructive testing is performed on the test piece to monitor the damage extension of the test piece; Step 6.4: After the fatigue test, perform ultrasonic nondestructive testing on the test piece to determine whether the damage does not extend or extends slowly within the specified cycle.
Citation Information
Cited By
Method and device for testing vertical impact of all-carbon seat of airplane
CN120121333A
A vertical impact test method and test device for an all-carbon aircraft seat
CN120121333B
Pressurizing test method for bent plate of air inlet channel made of carbon fiber composite material
CN120846854A