PET substrate laser and medium-long wave infrared composite reflecting film and preparation method thereof

By combining PET substrate with Ge/ZnS film and optimizing coating technology in the beam synthesizer, a multi-layer film system is designed, which solves the problem of low reflectivity of existing beam synthesizers and realizes efficient laser and medium wave The composite reflection effect of infrared and long-wave infrared multi-band has improved guidance accuracy.

CN118897345APending Publication Date: 2024-11-05HARBIN XINGUANG OPTIC-ELECTRONICS TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310494080.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing beam synthesizer has low reflectivity, which affects the guidance accuracy of multi-mode composite simulation and cannot meet the high-efficiency composite simulation needs of laser, medium-wave infrared and long-wave infrared.

Method used

The PET substrate is used to combine with the Ge/ZnS film, and the film structure is designed as G/H/L/H/L/H/L/H/L/H/L/H/L/H/A through a simple form optimization algorithm, and ion-assisted and low-temperature cold plating is used. The process of plating a multi-band composite reflective film to improve the firmness and reflectivity of the film layer.

Benefits of technology

The reflectivity in the laser wavelength range is greater than 65%, and the reflectivity in the medium-wave infrared and long-wave infrared wavelength ranges is greater than 91% and 92%, which improves the multi-band composite reflection effect and environmental stability of the guidance system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118897345A_ABST
    Figure CN118897345A_ABST
Patent Text Reader

Abstract

The invention discloses a PET substrate laser and medium-long wave infrared composite reflecting film and a preparation method thereof, and relates to a reflecting film and a preparation method thereof. The invention aims to solve the problem that the reflectivity of the existing reflecting film to laser and medium-long wave infrared is low. The structural relationship of the film layer is G / H / L / H / L / H / L / H / H / L / H / A, wherein G is a PET substrate, H is a Ge film material, L is a ZnS film material, and A is an air medium. The preparation method comprises the steps of film system structure design, substrate cleaning, substrate preheating, substrate secondary cleaning, film system plating and the like, before film plating, the background vacuum degree is better than 6 * 10 <-3 > Pa, a Ge film material is evaporated through electron beams, a ZnS film material is evaporated through resistance heating, alternate plating is conducted according to the structural relation, and ion assistance is started in the whole process. The method is used for preparing a laser / medium-wave infrared / long-wave infrared beam synthesizer and a reflecting film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a PET substrate laser, medium-wave infrared and long-wave infrared composite reflective film and a preparation method thereof, and in particular to a PET substrate laser, medium-wave infrared and long-wave infrared composite reflective film and a preparation method thereof for a semi-physical multi-mode composite homing guidance system, and belongs to the technical field of vacuum coating. Background Art

[0002] The guidance technology of multi-mode composite homing has the advantages of long range, high precision, strong anti-interference ability, etc. It can realize the automatic conversion of long-range laser guidance and short-range infrared homing, and has become an important development direction of precision-guided weapons. The semi-physical simulation guidance system of multi-mode composite homing is an effective means to verify the effective combat radius of the multi-mode composite seeker of the multi-mode composite guidance system, shorten the development cycle, and improve the guidance performance of the multi-mode composite homing. Among them, the beam synthesizer is one of the important components of the semi-physical simulation guidance system of the multi-mode composite homing. The reflective film of the beam synthesizer plays the role of co-caliber output of the coupled signal, and is one of the key components that determine whether the simulation guidance system can complete single-mode, dual-mode or multi-mode composite simulation.

[0003] The reflective film in the existing beam synthesizer has many disadvantages. The thin-film infrared-radar beam synthesizer mentioned in CN101303407B can only realize infrared / radar dual-mode simulation, which cannot meet the existing multi-mode composite simulation requirements, and the substrate surface is poor, which in turn affects the infrared spectrum reflection performance; a beam synthesizer mentioned in CN111983565B solves the multi-mode composite simulation of laser / infrared / radar. Although the reflectivity of long-wave infrared and medium-wave infrared reaches more than 90%, the reflectivity of laser is only 54.8%.

[0004] In summary, although the existing beam synthesizers in China can realize infrared / radar dual-mode and laser / infrared / radar multi-mode simulation, their reflectivity is low, which seriously affects the guidance accuracy. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of poor multi-mode composite simulation guidance accuracy caused by low reflectivity of the existing beam synthesizer, and proposes a PET substrate laser, medium and long wave infrared composite reflective film and a preparation method thereof.

[0006] The technical scheme of the present invention is: select Ge / ZnS film material with good bonding force with polyester resin PET substrate to achieve the purpose of stress matching therewith, and lay a good foundation for the firmness of the film layer. After determining the coating material, in order to achieve the purpose of the average reflectivity of the laser in the wavelength range of (1064±10)nm being greater than 65%, the average reflectivity in the infrared (3-5)μm wavelength range being greater than 91%, and the average reflectivity in the infrared (8-12)μm wavelength range being greater than 92%, a simplified optimization algorithm is used to optimize the film system structure, and the final structure of the film system is: G / H / L / H / L / H / L / H / L / H / A, wherein G is PET substrate, H is Ge film material, L is ZnS film material, and A is air medium. On the PET substrate with a high expansion coefficient, by adopting ion-assisted and low-temperature cold plating plating processes, each layer of film material is firmly plated on the PET substrate in turn to plate a multi-band composite reflective film system. Then the multi-band composite reflection effect of PET substrate laser band, medium-wave infrared and long-wave infrared is realized for the multi-mode composite simulation guidance system.

[0007] The present invention also provides a preparation method, which comprises the following steps:

[0008] Step 1: membrane structure design;

[0009] The structure of the reflective film is: G / H / L / H / L / H / L / H / L / H / A, where G is the PET substrate, H is the Ge film material, L is the ZnS film material, and A is the air medium. After optimization by the simplified optimization algorithm, the thickness of the PET substrate is 1.064μm. From the leftmost H to the rightmost H in the structure, the optical thickness of each layer of the film from the inside to the outside corresponds to: 232.6nm, 439.1nm, 233.6nm, 430.9nm, 815.9nm, 1096nm, 583.1nm, 1096nm, 583.1nm;

[0010] Step 2: Clean the substrate surface;

[0011] Clean the surface of the PET substrate to be plated with a cleaning liquid. Preferably, use a dust-free cloth dipped in a 1:1 alcohol-ether mixture to wipe the substrate, check the surface of the substrate to ensure there is no oil or dust, put it into a vacuum chamber and evacuate it to vacuum for plating;

[0012] Step 3: Preheating the substrate;

[0013] The vacuum chamber temperature was set to 50°C and maintained at 50°C for 1 hour;

[0014] Step 4: Secondary cleaning;

[0015] Start the ion source to clean the substrate for 20 minutes;

[0016] Step 5: film plating;

[0017] The coating is performed sequentially according to the film structure and process parameters of each film layer.

[0018] Preferably, the Ge film is prepared by electron beam evaporation, and the deposition rate of the film is 4A / s; ZnS is prepared by barrier evaporation, and the deposition rate of the film is 8A / s;

[0019] Preferably, an ion source assisted evaporation process is adopted, and the ion source parameters are: plate voltage 450V, beam current 30mA, and ion source assisted evaporation is adopted throughout the plating process;

[0020] Preferably, after evaporating the fourth, sixth and eighth thin films, the process and the ion source are suspended for (1-2) hours, and the process is restarted to complete the evaporation when the temperature of the vacuum chamber is lower than 50°C.

[0021] Compared with the prior art, the present invention has the following effects:

[0022] By optimizing the design of the composite reflective film system, using germanium material as the transition layer, and optimizing the process parameters of the film system evaporation, the deformation of the substrate surface is effectively suppressed, the firmness of each film layer is increased, and the environmental stability and product qualification rate of the three-band reflective film on the PET substrate are improved. The optimization goal of preparing the three-band composite reflective film with a reflectivity of more than 65% at 1.064μm±0.01μm, an average reflectivity of more than 91% at 3μm~5μm, and an average reflectivity of more than 92% at 8μm~12μm is achieved, and the multi-band reflection effect of laser, mid-wave infrared, and long-wave infrared is achieved, thereby realizing multi-mode composite simulation of different wavelengths of infrared single mode. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a structural schematic diagram of a PET substrate laser, medium and long wave infrared composite reflective film of the present invention;

[0024] Figure 2 This is the spectrum of the reflectivity effect of the composite reflective film in the measured laser band;

[0025] Figure 3 It is a spectrum diagram of the measured medium-wave and long-wave infrared reflectivity effects of the composite reflective film.

[0026] Description of reference numerals:

[0027] 1-PET substrate 31-first layer of Ge film

[0028] 21-first layer ZnS film material 32-second layer Ge film material

[0029] 22- Second layer ZnS film material 33- Third layer Ge film material

[0030] 23-the third layer of ZnS film material 34-the fourth layer of Ge film material

[0031] 24-the fourth layer of ZnS film material 35-the fifth layer of Ge film material

[0032] 4- Air medium DETAILED DESCRIPTION

[0033] The specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings, but the protection scope of the present invention shall not be limited thereto.

[0034] Specific implementation method 1: A PET substrate laser, medium and long wave infrared composite reflective film mainly consists of a PET substrate (1), 9 layers of film material and an air medium (4). The substrate (1) and the film material (Ge film material and ZnS film material) of the film structure should have a high stress matching degree and good bonding strength. In order to achieve an average reflectivity greater than 65% in the wavelength range of (1064±10)nm, an average reflectivity greater than 91% in the wavelength range of (3-5)μm, and an average reflectivity greater than 92% in the wavelength range of (8-12)μm, a simplified optimization algorithm is used to optimize the film structure. The final structure of the film is: G / H / L / H / L / H / L / H / L / H / A, where G is the PET substrate (1), H is the Ge film material, L is the ZnS film material, and A is the air medium (4);

[0035] Compared with the disclosed CN101303407B and CN111983565B, one of the main differences of the present invention is that Ge and ZnS are alternately evaporated. After testing and verification, this coating can achieve an average reflectivity of more than 65% in the laser (1064±10) nm wavelength range, an average reflectivity of more than 91% in the infrared (3-5) μm medium wave range, and an average reflectivity of more than 92% in the infrared (8-12) μm long wave range. The reflectivity of laser, medium wave infrared and long wave infrared is higher than that of existing beam synthesizers.

[0036] Specific implementation method two: The film system structure G / H / L / H / L / H / L / H / L / H / A is, from left to right, a PET substrate (1), a first layer of Ge film material (31), a first layer of ZnS film material (21), a second layer of Ge film material (32), a second layer of ZnS film material (22), a third layer of Ge film material (33), a third layer of ZnS film material (23), a fourth layer of Ge film material (34), a fourth layer of ZnS film material (24), a fifth layer of Ge film material (35), and an air medium (4).

[0037] Specific implementation method three: This implementation method is described in conjunction with the accompanying drawings. The preparation method of this implementation method includes the following steps:

[0038] Step 1: membrane structure design;

[0039] The substrate (1) material is PET, germanium is a high refractive index material, zinc sulfide is a low refractive index material, and the final structure of the film system is: G / H / L / H / L / H / L / H / L / H / A, wherein G is the substrate, A is air, H and L represent Ge and ZnS with an optical thickness of 1 / 4 wavelength, respectively;

[0040] After the optimized design, the optical thickness of each film layer from left to right corresponds to: PET substrate (1) 1.064 μm, the first layer of Ge film material (31) 232.6 nm, the first layer of ZnS film material (21) 439.1 nm, the second layer of Ge film material (32) 233.6 nm, the second layer of ZnS film material (22) 430.9 nm, the third layer of Ge film material (33) 815.9 nm, the third layer of ZnS film material (23) 1096 nm, the fourth layer of Ge film material (34) 583.1 nm, the fourth layer of ZnS film material (24) 1096 nm, the fifth layer of Ge film material (35) 583.1 nm;

[0041] The first layer of Ge film material (31) in the film system structure serves as a transition layer connecting the substrate (1) and the overlying reflective film;

[0042] Step 2: Cleaning the surface of the substrate (1);

[0043] Use a clean dust-free cloth dipped in a 1:1 alcohol-ether mixture to wipe the substrate (1), check the surface of the substrate (1) to ensure that there is no oil stain or dust particles, and then place the substrate (1) in a vacuum chamber for plating;

[0044] Step 3: Preheating the substrate;

[0045] Before coating, the substrate is heated and baked at a temperature of 50°C for 1 hour;

[0046] Step 4: Secondary cleaning;

[0047] Before starting the coating process, the substrate (1) is cleaned twice with an ion source, the cleaning time is 30 minutes, and the ion source parameters are: plate voltage 450V, beam current 30mA, and working gas is Ar gas;

[0048] Step 5: film plating;

[0049] According to the film system structure, the evaporation process of each film layer is adopted to sequentially plate a first layer of Ge film material (31), a first layer of ZnS film material (21), a second layer of Ge film material (32), a second layer of ZnS film material (22), a third layer of Ge film material (33), a third layer of ZnS film material (23), a fourth layer of Ge film material (34), a fourth layer of ZnS film material (24), and a fifth layer of Ge film material (35) on the PET substrate (1);

[0050] Before coating, the background vacuum is better than 6×10 -3 Pa, film deposition rate and film thickness are controlled by a quartz crystal controller, ion assistance is turned on during the entire plating process, and the parameters are the same as those of ion cleaning;

[0051] The Ge film material is evaporated by electron beam, and the film deposition rate is 4A / s. The ZnS film material is evaporated by resistance heating, and the film deposition rate is 8A / s.

[0052] In the film system preparation process, after evaporating the second layer of ZnS film material (22), the third layer of ZnS film material (23), and the fourth layer of ZnS film material (24), the process and the ion source are suspended for 2 hours to allow the vacuum chamber to cool down naturally, and the process is restarted when the temperature of the vacuum chamber is lower than 50° C. to complete the subsequent plating;

[0053] Step 6: Take out the reflective film;

[0054] After the coating is completed, when the temperature of the vacuum chamber is lower than 40° C., the coated element is taken out to obtain a reflective film;

[0055] Step 7: Reflective film test;

[0056] The reflectivity of the reflective film was measured using a spectrophotometer and an infrared Fourier spectrometer. After actual measurement, the reflectivity of the reflective film to 1.064μm±0.1μm laser was 65.8%, the average reflectivity to 3μm~5μm medium-wave infrared was 91.8%, and the average reflectivity to 8μm~12μm long-wave infrared was 92.5%.

[0057] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A PET-based laser, medium- and long-wave infrared composite reflective film, characterized in that: It comprises a PET substrate (1), a ZnS film material (2), a Ge film material (3) and an air medium (4).

2. The PET-based laser, medium- and long-wave infrared composite reflective film according to claim 1, characterized in that: The ZnS film material (2) includes four layers, namely a first layer of ZnS film material (21), a second layer of ZnS film material (22), a third layer of ZnS film material (23), and a fourth layer of ZnS film material (24); the Ge film material (3) includes five layers, namely a first layer of Ge film material (31), a second layer of Ge film material (32), a third layer of Ge film material (33), a fourth layer of Ge film material (34), and a fifth layer of Ge film material (35).

3. The PET-based laser, medium- and long-wave infrared composite reflective film according to claim 1, characterized in that: The structural relationship between the ZnS film material (2), the Ge film material (3), the PET substrate (1) and the air medium (4) is G / H / L / H / L / H / L / H / L / H / A, wherein G is the PET substrate (1), H is the Ge film material (3), L is the ZnS film material (2), and A is the air medium (4).

4. The PET-based laser, medium- and long-wave infrared composite reflective film according to claim 1, characterized in that: H in the structural relationship, from left to right, respectively, is the first layer of Ge film material (31), the second layer of Ge film material (32), the third layer of Ge film material (33), the fourth layer of Ge film material (34), and the fifth layer of Ge film material (35); L in the structural relationship, from left to right, respectively, is the first layer of ZnS film material (21), the second layer of ZnS film material (22), the third layer of ZnS film material (23), and the fourth layer of ZnS film material (24).

5. A method for preparing a PET substrate laser, medium- and long-wave infrared composite reflective film according to any one of claims 1 to 4, characterized in that: It includes the following steps: Step 1: membrane structure design; After the optimized design, the optical thickness of each film layer from left to right corresponds to: PET substrate (1) 1.064 μm, the first layer of Ge film material (31) 232.6 nm, the first layer of ZnS film material (21) 439.1 nm, the second layer of Ge film material (32) 233.6 nm, the second layer of ZnS film material (22) 430.9 nm, the third layer of Ge film material (33) 815.9 nm, the third layer of ZnS film material (23) 1096 nm, the fourth layer of Ge film material (34) 583.1 nm, the fourth layer of ZnS film material (24) 1096 nm, the fifth layer of Ge film material (35) 583.1 nm; The first layer of Ge film material (31) serves as a transition layer connecting the PET substrate (1) and the overlying reflective film; Step 2: Cleaning the surface of the substrate (1); Use a clean dust-free cloth dipped in a 1:1 alcohol-ether mixture to wipe the PET substrate (1), check the surface of the PET substrate (1) to ensure that there is no oil stain or dust particles, and then place it in a vacuum chamber for plating; Step 3: Preheating the substrate; Before coating, the substrate is heated and baked at a temperature of 50°C for 1 hour; Step 4: Secondary cleaning; Before starting the coating process, the PET substrate (1) is cleaned twice with an ion source. The cleaning time is 30 minutes. The ion source parameters are: plate voltage 450V, beam current 30mA, and working gas is Ar gas. Step 5: film plating; According to the film system structure, the evaporation process of each film layer is adopted to sequentially plate a first layer of Ge film material (31), a first layer of ZnS film material (21), a second layer of Ge film material (32), a second layer of ZnS film material (22), a third layer of Ge film material (33), a third layer of ZnS film material (23), a fourth layer of Ge film material (34), a fourth layer of ZnS film material (24), and a fifth layer of Ge film material (35) on the PET substrate (1); Before coating, the background vacuum is better than 6×10-3Pa. The deposition rate and thickness of the film are controlled by a quartz crystal controller. Ion assist is turned on during the entire coating process, and the parameters are the same as those of ion cleaning. The Ge film material is evaporated by electron beam, and the film deposition rate is 4A / s. The ZnS film material is evaporated by resistance heating, and the film deposition rate is 8A / s. In the film system preparation process, after evaporating the second layer of ZnS film material (22), the third layer of ZnS film material (23), and the fourth layer of ZnS film material (24), the process and the ion source are suspended for 2 hours to allow the vacuum chamber to cool down naturally, and the process is restarted when the temperature of the vacuum chamber is lower than 50° C. to complete the subsequent plating; Step 6: Take out the reflective film; After the coating is completed, when the temperature of the vacuum chamber is lower than 40° C., the coated element is taken out to obtain a reflective film.

Citation Information

Cited By

  • Low-layer-number one-dimensional infrared low-emissivity film system structure insensitive to polarization and incidence angle