Polarizer for IPS type display and preparation method and application thereof
By abolishing the lower TAC layer of the IPS display, and using a laminated structure of the protective film layer, the upper TAC layer, the polarized photon layer and the bidirectional stretched polyester release film layer, the problems of high manufacturing cost and high thickness of the polarizer are solved, and the Cost reduction and product thinning improve light transmittance and reduce haze and release force.
Patent Information
- Application Number
- CN202410921643.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-05
AI Technical Summary
Currently, polarizers used in IPS type displays are costly and generally thick, which cannot meet the thinner development needs of displays.
By abolishing the lower TAC layer in the polarizer, a laminated structure of a protective film layer, an upper TAC layer, a polarized photon layer, a PSA layer and a bidirectional stretched polyester release film layer are adopted, and thermally drying or UV hardening is used with the adsor layer. The polyester release film is peeled off and the protective film and PSA layer are bonded to form a polarizer.
The reduction of polarizer manufacturing cost and product thinning is achieved, and the use of high-cost zero-phase difference film is avoided, and the light transmittance is improved and haze and release force is reduced.
Smart Images

Figure CN118897348A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of optical displays, and in particular to a polarizing film for IPS type displays and a preparation method and application thereof. Background Art
[0002] At present, the structure of the polarizer of IPS display is complex, mainly composed of multiple layers of films such as protective film + upper TAC + polarizer + lower TAC + PSA + release film. The lower TAC used in the polarizer of IPS type display is mainly 0 phase difference film (0 phase difference film refers to a film made of isotropic material, and the refractive index of the film in all directions is almost equal). Currently, 0 phase difference film is mainly made of a few low birefringence materials such as triacetyl cellulose, PMMA, COP, etc. On the one hand, this material is expensive, which increases the overall manufacturing cost of the polarizer; on the other hand, it increases the overall thickness of the polarizer, which does not meet the trend of thin display development. Summary of the invention
[0003] (1) Technical issues to be solved
[0004] The present application provides a polarizer for an IPS type display, and a preparation method and application thereof, to solve the technical problems that the current polarizer for an IPS type display has a relatively high manufacturing cost and is relatively thick overall.
[0005] (2) Technical solution
[0006] In a first aspect, the present application provides a polarizer for an IPS type display, comprising a protective film layer, an upper TAC layer, a polarizing layer, a PSA layer and a release film layer stacked in sequence, wherein the polarizing layer is bonded to the upper TAC layer and the PSA layer respectively through an adhesive layer.
[0007] Furthermore, the protective film layer is made of PC or PE.
[0008] Furthermore, the release film layer is made of PET material.
[0009] In a second aspect, the present application provides a method for preparing a polarizer for an IPS type display as described above, comprising:
[0010] The upper TAC layer, the polarizing layer and the polyester release film layer are sequentially laminated by using an adhesive, and then heat-dried or UV-cured to obtain a laminate 1;
[0011] The polyester release film layer in the laminate 1 is peeled off to obtain a laminate 2;
[0012] A protective film layer is laminated on the upper TAC layer side of the laminate 2, and a PSA layer and a release film layer are laminated in sequence on the polarizing layer side of the laminate 2 to form a laminate 3, that is, to obtain the polarizer.
[0013] Furthermore, the polyester release film layer is a biaxially stretched polyester release film, which is prepared by first longitudinally stretching, then coating a release agent solution online, and then transversely stretching, heat-setting, and track relaxation.
[0014] Furthermore, the stretching ratio of the longitudinal stretching is 1.5 to 4 times, and the stretching temperature is 90 to 120°C.
[0015] Furthermore, the stretching ratio of the transverse stretching is 3 to 6 times, and the stretching temperature is 100 to 140°C.
[0016] Furthermore, the heat setting temperature is 190° C. to 250° C., and the track relaxation ratio is 2% to 10%.
[0017] Furthermore, the biaxially oriented polyester release film has a light transmittance higher than 88%, a haze lower than 3%, and a release force lower than 50 gf / 25 mm.
[0018] In a third aspect, the present application provides the use of the polarizer as described above or the polarizer obtained by the preparation method as described above in the field of optical displays.
[0019] (3) Beneficial effects
[0020] The above technical solution of the present application has the following advantages:
[0021] The polarizer for IPS type display and the preparation method thereof provided in the present application eliminate TAC in the polarizer, thereby avoiding the use of a zero phase difference film, thereby achieving a reduction in the manufacturing cost of the polarizer and a thinner product. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0023] Figure 1 Schematic diagram of a polarizer for an IPS type display provided in this application. DETAILED DESCRIPTION
[0024] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0025] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0026] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0027] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0028] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0029] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0030] The present application provides a polarizer for an IPS type display, a preparation method and an application thereof, making it possible to eliminate the TAC of the IPS type polarizer.
[0031] The specific implementation methods of the present application are further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present application but are not intended to limit the scope of the present application.
[0032] The present application embodiment provides a polarizer for an IPS type display, such as Figure 1 As shown, it includes a protective film layer, an upper TAC layer, a polarizing layer, a PSA layer and a release film layer which are stacked in sequence, and the polarizing layer is bonded to the upper TAC layer and the PSA layer through an adhesive layer.
[0033] In some embodiments, the protective film layer is made of PC or PE.
[0034] In some embodiments, the release film layer is made of PET.
[0035] The present application also provides a method for preparing the polarizer for an IPS type display as described above, comprising:
[0036] The upper TAC layer, the polarizing layer and the polyester release film layer are sequentially laminated by using an adhesive, and then heat-dried or UV-cured to obtain a laminate 1;
[0037] The polyester release film layer in the laminate 1 is peeled off to obtain a laminate 2;
[0038] A protective film layer is laminated on the upper TAC layer side of the laminate 2, and a PSA layer and a release film layer are laminated in sequence on the polarizing layer side of the laminate 2 to form a laminate 3, that is, to obtain the polarizer.
[0039] In some embodiments, the polyester release film layer is a biaxially oriented polyester release film, which is prepared by first longitudinally stretching, then coating a release agent solution online, and then transversely stretching, heat-setting, and track relaxation.
[0040] In some embodiments, the stretching ratio of the longitudinal stretching is 1.5 to 4 times, and the stretching temperature is 90 to 120°C.
[0041] In some embodiments, the stretching ratio of the transverse stretching is 3 to 6 times, and the stretching temperature is 100 to 140°C.
[0042] In some embodiments, the heat setting temperature is 190° C. to 250° C., and the track relaxation ratio is 2% to 10%.
[0043] In some embodiments, the biaxially oriented polyester release film has a light transmittance higher than 88%, a haze lower than 3%, and a release force lower than 50 gf / 25 mm.
[0044] The embodiments of the present application also provide the use of the polarizer as described above or the polarizer obtained by the preparation method as described above in the field of optical displays.
[0045] In application, TAC, polarizer, and polyester release film are bonded together with an adhesive, and then heat-dried or UV-cured to form a laminate 1. The polyester release film is then peeled off to form a laminate 2. The laminate 2 is then bonded with a protective film, PSA, and a release film to form a laminate 3, which becomes the final polarizer product.
[0046] The reason for using a biaxially oriented polyester release film is that the polyester film has high mechanical strength and is easy to use. In addition, the price of polyester is cheap, which is conducive to reducing the overall manufacturing cost. The release film used in this application is an online coating release film, which makes the cost of the release film even lower, thereby reducing the cost of the entire process.
[0047] The polyester release film is longitudinally stretched with a stretching ratio (MD) of 1.5 to 4 times and a stretching temperature of 90 to 120°C, and then coated with a release agent solution online, and then transversely stretched 3 to 6 times with a transverse stretching temperature of 100 to 140°C, and then heat-set at 190 to 250°C and track-relaxed by 2% to 10% to obtain a polyester release film with a transmittance higher than 88%, a haze lower than 3%, and a release force lower than 50gf / 25mm.
[0048] The reason why the polyester release film has a haze lower than 3% is that the laminate 1 needs to be inspected online by CCD, and too high a haze is not conducive to defect detection. The release force is lower than 50gf / 25mm, and too high a release force can easily make it difficult to peel off the polyester release film or cause the laminate 1 to delaminate or break.
[0049] In the process of manufacturing polarizer, a polyester release film is first used to form a laminate 1, and when the adhesive is cured, the polyester release film is peeled off to form a laminate 2. The transition effect of the polyester release film in the whole process makes it possible to eliminate the zero phase difference film.
[0050] The following is an explanation through specific embodiments.
[0051] Example 1
[0052] This embodiment provides a polarizer for an IPS type display, such as Figure 1 As shown, it includes a protective film layer, an upper TAC layer, a polarizing layer, a PSA layer and a release film layer stacked in sequence, and the polarizing layer is bonded to the upper TAC layer and the PSA layer through an adhesive layer. The protective film layer is made of PC material, and the release film layer is made of PET material.
[0053] The preparation method of the polarizer comprises the following steps:
[0054] The upper TAC layer, the polarizing layer and the polyester release film layer are sequentially laminated by using an adhesive, and then heat-dried or UV-cured to obtain a laminate 1;
[0055] The polyester release film layer in the laminate 1 is peeled off to obtain a laminate 2;
[0056] A protective film layer is laminated on the upper TAC layer side of the laminate 2, and a PSA layer and a release film layer are laminated in sequence on the polarizing layer side of the laminate 2 to form a laminate 3, that is, a polarizer is obtained.
[0057] The polyester release film layer is a biaxially stretched polyester release film, which is first longitudinally stretched and then coated with a release agent solution online, and then transversely stretched, heat-set and track relaxed. The stretching ratio of the longitudinal stretching is 2 times, and the stretching temperature is 95°C. The stretching ratio of the transverse stretching is 4 times, and the stretching temperature is 110°C. The heat setting temperature is 200°C, and the track relaxation ratio is 5%. The light transmittance of the biaxially stretched polyester release film is 90%, the haze is 2%, and the release force is 45gf / 25mm.
[0058] Example 2
[0059] This embodiment provides a polarizer for an IPS type display, such as Figure 1 As shown, it includes a protective film layer, an upper TAC layer, a polarizing layer, a PSA layer and a release film layer stacked in sequence, and the polarizing layer is bonded to the upper TAC layer and the PSA layer through an adhesive layer. The protective film layer is made of PE material, and the release film layer is made of PET material.
[0060] The preparation method of the polarizer comprises the following steps:
[0061] The upper TAC layer, the polarizing layer and the polyester release film layer are sequentially laminated by using an adhesive, and then heat-dried or UV-cured to obtain a laminate 1;
[0062] The polyester release film layer in the laminate 1 is peeled off to obtain a laminate 2;
[0063] A protective film layer is laminated on the upper TAC layer side of the laminate 2, and a PSA layer and a release film layer are laminated in sequence on the polarizing layer side of the laminate 2 to form a laminate 3, that is, a polarizer is obtained.
[0064] The polyester release film layer is a biaxially stretched polyester release film, which is first longitudinally stretched and then coated with a release agent solution online, and then transversely stretched, heat-set and track relaxed. The stretching ratio of the longitudinal stretching is 3 times, and the stretching temperature is 110°C. The stretching ratio of the transverse stretching is 5 times, and the stretching temperature is 130°C. The heat setting temperature is 230°C, and the track relaxation ratio is 8%. The light transmittance of the biaxially stretched polyester release film is 95%, the haze is 1%, and the release force is 40gf / 25mm.
[0065] The materials of the upper TAC layer, polarizing layer, and PSA layer in the above embodiments 1 and 2 are consistent with the existing IPS display polarizers. The adhesive layer is made of UV curable glue.
[0066] The method for preparing a polarizer for an IPS type display provided in an embodiment of the present application eliminates TAC in the polarizer, thereby avoiding the use of a zero phase difference film, thereby achieving a reduction in the manufacturing cost of the polarizer and a thinner product.
[0067] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A polarizer for an IPS type display, characterized in that: It comprises a protective film layer, an upper TAC layer, a polarizing layer, a PSA layer and a release film layer which are stacked in sequence, wherein the polarizing layer is bonded to the upper TAC layer and the PSA layer via an adhesive layer.
2. The polarizer for IPS type display according to claim 1, characterized in that: The protective film layer is made of PC or PE material.
3. The polarizer for IPS type display according to claim 1, characterized in that: The release film layer is made of PET material.
4. A method for preparing a polarizer for an IPS type display according to any one of claims 1 to 3, characterized in that: include: The upper TAC layer, the polarizing layer and the polyester release film layer are sequentially laminated by using an adhesive, and then heat-dried or UV-cured to obtain a laminate 1; The polyester release film layer in the laminate 1 is peeled off to obtain a laminate 2; A protective film layer is laminated on the upper TAC layer side of the laminate 2, and a PSA layer and a release film layer are laminated in sequence on the polarizing layer side of the laminate 2 to form a laminate 3, that is, to obtain the polarizer.
5. The preparation method according to claim 4, characterized in that: The polyester release film layer is a biaxially stretched polyester release film, which is prepared by first longitudinally stretching, then coating a release agent solution online, and then transversely stretching, heat-setting, and track relaxation.
6. The preparation method according to claim 5, characterized in that: The stretching ratio of the longitudinal stretching is 1.5 to 4 times, and the stretching temperature is 90 to 120°C.
7. The preparation method according to claim 5, characterized in that: The stretching ratio of the transverse stretching is 3 to 6 times, and the stretching temperature is 100 to 140°C.
8. The preparation method according to claim 5, characterized in that: The temperature of the heat setting is 190° C. to 250° C., and the relaxation ratio of the track is 2% to 10%.
9. The preparation method according to claim 5, characterized in that: The biaxially oriented polyester release film has a light transmittance higher than 88%, a haze lower than 3%, and a release force lower than 50 gf / 25 mm.
10. Use of the polarizer according to any one of claims 1 to 3 or the polarizer obtained by the preparation method according to any one of claims 4 to 9 in the field of optical displays.