Positive photoresist composition and lithography process method of negative photoresist pattern

CN118897438APending Publication Date: 2024-11-05ECHEM SOLUTIONS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310497644.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The negative photoresist used in traditional color filter arrays (CFAs) is difficult to meet the demand for high resolution, so developing new negative photoresist materials and technologies in the microfilm process has become the pursuit of manufacturers.

Method used

The polyimide resin obtained by polymerization of diamine and tetracarboxylic dianhydride is used as the positive photoresist composition, and combined with a photosensitive compound and a solvent to be used for the micro-photographing process of negative photoresist patterns. Specific exposure and development steps form a negative photoresist film with high pattern resolution.

Benefits of technology

A negative photoresist film with high pattern resolution is achieved in the micro-photographing process of negative photoresist pattern, which improves the quality and resolution of the negative photoresist pattern, and reduces problems such as swelling, residue and undercut.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118897438A_ABST
    Figure CN118897438A_ABST
Patent Text Reader

Abstract

A positive photoresist composition includes (A) a polyimide resin, (B) a photosensitive compound, and (C) a solvent. The polyimide resin (A) is obtained by carrying out polymerization reaction on diamine (a) and tetracarboxylic dianhydride (b) and has a structural unit shown in a formula (1); wherein Ar1 in the formula (1) is a tetravalent organic group, Ar2 is a divalent organic group, Ar1 is a group represented by formula (B-1), formula (B-2), formula (B-3) or a combination thereof, Ar2 is at least a group represented by formula (A-1), formula (A-2) or a combination thereof, and in addition, Ar2 can be further a group represented by formula (A-3), formula (A-4), formula (A-5) or a combination thereof. The invention also provides a lithography process method of the negative photoresist pattern. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a positive photoresist composition, in particular to a positive photoresist composition that can be used in a lithography process of a negative photoresist pattern, and a lithography process method of a negative photoresist pattern. Background Art

[0002] Due to the increasing demand for digital cameras and mobile phone cameras, lens modules are developing towards high resolution; among them, color filter array (CFA) is a key component that determines the performance of lens modules. In the lithography process, negative photoresist has a cross-linked structure after exposure, so its chemical resistance, heat resistance, and etching resistance are better than positive photoresist. However, the negative photoresist used in traditional CFA is difficult to meet high resolution requirements, so all manufacturers are committed to developing negative photoresist materials and lithography process technology. Summary of the invention

[0003] Some embodiments of the present invention provide a positive photoresist composition.

[0004] Some embodiments of the present invention provide a positive photoresist composition suitable for a lithography process of a negative photoresist pattern.

[0005] Some embodiments of the present invention further provide a negative photoresist film having high pattern resolution.

[0006] In some embodiments of the present invention, the positive photoresist composition includes (A) a polyimide resin, (B) a photosensitive compound, and (C) a solvent. The (A) polyimide resin is obtained by polymerization of (a) a diamine and (b) a tetracarboxylic dianhydride, and has a structural unit represented by formula (1):

[0007]

[0008] Among them, Ar in formula (1) 1 is a tetravalent organic group, Ar 2 is a divalent organic group, and Ar 1 A group represented by formula (B-1), formula (B-2), formula (B-3) or a combination thereof

[0009]

[0010] * indicates the bonding position; Ar in formula (1) 2 Containing a group represented by formula (A-1), formula (A-2) or a combination thereof

[0011]

[0012] Wherein, m1 and m2 of formula (A-1) are each an integer of 1 to 3, and X 1Each is an alkylene or phenylene group having 1 to 5 carbon atoms; wherein, when X 1 When it is an alkylene group having 1 to 5 carbon atoms, any one of the -CH2- in the alkylene group having 1 to 5 carbon atoms may be substituted by -NH-; X in formula (A-2) 2 is a hydrocarbon group having 1 to 10 carbon atoms, -O-, -S-, -SO2-, -NH-, -C(CF3)2- or

[0013] In one embodiment of the present invention, the Ar 2 Further comprising a group represented by formula (A-3), formula (A-4), formula (A-5) or a combination thereof

[0014]

[0015] Wherein, Y in formula (A-3) is -C(CH3)2-, -C(CF3)2-, -CH2-, -O-, -S- or -SO2-; * indicates the bonding position.

[0016] In one embodiment of the present invention, the above-mentioned (a) diamine includes (a-1) diamine and (a-2) diamine; (a-1) diamine is a diamine having a silicon-oxygen bond and is a compound represented by formula (I-1); (a-2) diamine is a diamine having four benzene rings and is a compound represented by formula (I-2):

[0017]

[0018]

[0019] Wherein, m1 and m2 of formula (I-1) are each an integer of 1 to 3, and X 1 Each is an alkylene or phenylene group having 1 to 5 carbon atoms; wherein, when X 1 When it is an alkylene group having 1 to 5 carbon atoms, any one of the -CH2- in the alkylene group having 1 to 5 carbon atoms may be substituted by -NH-; X in formula (I-2) 2 is a hydrocarbon group having 1 to 10 carbon atoms, -O-, -S-, -SO2-, -NH-, -C(CF3)2- or

[0020] In one embodiment of the present invention, the above-mentioned (a) diamine further includes (a-3) diamine; (a-3) diamine is a diamine having a phenol structure and is a compound represented by formula (I-3):

[0021]

[0022] Wherein, Y in formula (I-3) is -C(CH3)2-, -C(CF3)2-, -CH2-, -O-, -S- or -SO2-.

[0023] In one embodiment of the present invention, the weight average molecular weight of the polyimide resin (A) is 5,000-50,000.

[0024] In one embodiment of the present invention, the photosensitive compound (B) is quinonediazidesulfonic acid, a quinonediazidesulfonic acid derivative or a combination thereof; when the amount of the polyimide resin (A) is 100 parts by weight, the amount of the photosensitive compound (B) is 10-150 parts by weight.

[0025] In one embodiment of the present invention, the above-mentioned (C) solvent is N-methylpyrrolidone, γ-butyrolactone, ethyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide or a combination thereof, and the weight percentage of the (C) solvent in the positive photoresist composition is 50-90wt%.

[0026] Several embodiments of the present invention also provide a lithography process method for a negative photoresist pattern, comprising the following steps: coating the aforementioned positive photoresist composition on a substrate; heating the positive photoresist composition to form a film layer; patterning the film layer to form a positive photoresist pattern; coating a negative photoresist composition on a substrate; heating the negative photoresist composition; patterning the film layer to form a negative photoresist pattern.

[0027] In one embodiment of the present invention, the step of patterning the film layer and forming a positive photoresist pattern further includes exposing and developing the film layer, and the step of patterning the film layer and forming a negative photoresist pattern further includes exposing and developing the film layer, and the positions of the two exposures are the same.

[0028] In one embodiment of the present invention, the step of heating the positive photoresist composition further comprises baking at 100-130° C., and the step of heating the negative photoresist composition further comprises baking at 80-120° C.

[0029] In one embodiment of the present invention, the step of patterning the film layer and forming the positive photoresist pattern further includes making the positive photoresist pattern define a first region and a second region on the substrate.

[0030] In one embodiment of the present invention, the step of coating the negative photoresist composition on the substrate further includes distributing the negative photoresist composition in the second region.

[0031] In one embodiment of the present invention, the step of coating the negative photoresist composition on the substrate further includes distributing the negative photoresist composition in the first region, and the negative photoresist composition distributed in the first region covers the positive photoresist pattern.

[0032] In one embodiment of the present invention, the step of coating the negative photoresist composition on the substrate further includes distributing the negative photoresist composition in the second area; the step of patterning the film layer and forming a negative photoresist pattern further includes exposing the negative photoresist composition distributed in the second area to form a negative photoresist pattern.

[0033] In one embodiment of the present invention, the step of patterning the film layer and forming the negative photoresist pattern further includes developing with an alkaline aqueous solution and removing the positive photoresist pattern.

[0034] In one embodiment of the present invention, the above-mentioned negative photoresist pattern lithography process method further includes using (A) polyimide resin, (B) photosensitive compound and (C) solvent to prepare a positive photoresist composition; wherein (A) polyimide resin has a structural unit shown in formula (1), Ar 1 is a tetravalent organic group, Ar 2 is a divalent organic group, and Ar 1 is a group represented by formula (B-1), formula (B-2), formula (B-3) or a combination thereof, Ar 2 Containing a group represented by formula (A-1), formula (A-2) or a combination thereof

[0035]

[0036] In one embodiment of the present invention, the step of preparing the positive photoresist composition further includes using (a) diamine and (b) tetracarboxylic dianhydride to perform a polymerization reaction to provide (A) polyimide resin.

[0037] The positive photoresist composition of the present invention uses (A) polyimide resin obtained by polymerization of (a) diamine and (b) tetracarboxylic dianhydride, so it is suitable for the lithography process of negative photoresist pattern. The present invention uses the positive photoresist composition in the lithography process of negative photoresist pattern, so the obtained negative photoresist film can have high pattern resolution.

[0038] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 FIG. 4 is a schematic diagram of a process flow of a lithography process for forming a positive photoresist pattern according to an embodiment of the present invention.

[0040] Figure 2 FIG. 4 is a schematic diagram of a process flow of a negative photoresist pattern according to an embodiment of the present invention.

[0041] Figures 3A-3E FIG. 1 is a schematic diagram of an operation of a lithography process for a negative photoresist pattern according to an embodiment of the present invention. DETAILED DESCRIPTION

[0042] Unless otherwise defined, the "hydrocarbon group" mentioned in the present disclosure refers to an organic group consisting only of carbon and hydrogen, such as an alkyl, alkenyl or alkynyl group. In addition, the hydrocarbon group may also be a straight-chain hydrocarbon group, a branched hydrocarbon group or a cyclic hydrocarbon group. A "quadrivalent organic group" is an organic group having four bonding positions, and the "quadrivalent organic group" can form four chemical bonds through these four bonding positions. A "divalent organic group" is an organic group having two bonding positions, and the "divalent organic group" can form two chemical bonds through these two bonding positions. A "photoresist film" may be formed with a "pattern", "graphic" or may not have a "pattern", "graphic", and a "photoresist film pattern" refers to a photoresist film formed with or having a "pattern", "graphic". In the present disclosure, the meanings of "pattern" and "graphic" are essentially the same. In the present disclosure, the meanings of "photoresist pattern" and "photoresist film pattern" are essentially the same, and the former is used to emphasize the pattern of the photoresist film. In the present disclosure, the material obtained by coating and heating in the preparation of the photoresist film is referred to as a "film layer". The “film surface” may be the surface of a photoresist film or the surface of a film layer.

[0043] Positive photoresist composition

[0044] The present invention provides a positive photoresist composition, which can be used for the preparation of positive photoresist films and the lithography process of positive photoresist patterns and negative photoresist patterns. The positive photoresist composition of the present invention includes (A) a polyimide resin, (B) a photosensitive compound and (C) a solvent. In some embodiments of the present invention, the (A) polyimide resin is obtained by polymerization of (a) a diamine and (b) a tetracarboxylic dianhydride, and has a weight average molecular weight of 5,000-50,000, and its weight average molecular weight is preferably 10,000-40,000, and more preferably 25,000-35,000. The (A) polyimide resin may have a structural unit shown in formula (1), wherein Ar 1 is a tetravalent organic group, Ar 2 is a divalent organic group, and Ar 1 It can be a group represented by formula (B-1), formula (B-2), formula (B-3) or a combination thereof, Ar 2 Contains a group represented by formula (A-1), formula (A-2) or a combination thereof, and Ar 2 It may further contain groups represented by formula (A-3), formula (A-4), formula (A-5) or a combination thereof. That is, in the structural unit formula (1) of the polyimide resin (A), there must be Ar 2 is a structural unit of a group represented by formula (A-1) or formula (A-2), and other structural units have Ar2 It may be a group represented by formula (A-3), formula (A-4) or formula (A-5). (A) Ar of the structural unit of the polyimide resin 2 All of them may be groups represented by formula (A-1) or formula (A-2). * indicates the bonding position:

[0045]

[0046]

[0047]

[0048] Wherein, m1 and m2 of formula (A-1) can be integers of 1 to 3, respectively, and X 1 Each of them can be an alkylene or phenylene group having 1 to 5 carbon atoms; wherein, when X 1 When it is an alkylene group having 1 to 5 carbon atoms, any one of the -CH2- in the alkylene group having 1 to 5 carbon atoms may be substituted by -NH-; X in formula (A-2) 2 It can be a hydrocarbon group having 1 to 10 carbon atoms, -O-, -S-, -SO2-, -NH-, -C(CF3)2- or Y in formula (A-3) can be -C(CH3)2-, -C(CF3)2-, -CH2-, -O-, -S- or -SO2-; * indicates the bonding position. The (A) polyimide resin, (B) photosensitive compound and (C) solvent are mixed, dissolved or uniformly dispersed in an appropriate proportion to obtain a positive photoresist composition. For example, relative to 100 parts by weight of the (A) polyimide resin, the amount of the (B) photosensitive compound is 10-150 parts by weight, and preferably 20-80 parts by weight, and more preferably 30-60 parts by weight. There is no particular limitation on the (C) solvent, as long as it can dissolve the (A) polyimide resin and the components in the positive photoresist composition of the present invention and does not react with the components in the positive photoresist composition. Preferably, the (C) solvent can be the solvent used when synthesizing the (A) polyimide resin (described later). The film formed by the positive photoresist composition of the present invention may not be dissolved in the negative photoresist composition or the solvent used for the negative photoresist (described later), and when a lithography process of a negative photoresist pattern is performed, the film formed by the positive photoresist composition and the unexposed negative photoresist composition may be peeled off simultaneously during development.

[0049] (A) Polyimide resin

[0050] The (A) polyimide resin can be obtained by polymerization of (a) diamine and (b) tetracarboxylic dianhydride. The molar ratio of (a) diamine to (b) tetracarboxylic dianhydride can be 0.5-1.2:1, preferably 0.9-1.1:1. The (a) diamine and (b) tetracarboxylic dianhydride are described in detail below.

[0051] (a) Diamine

[0052] The (a) diamine includes at least (a-1) diamine and (a-2) diamine.

[0053] (a-1) Diamine

[0054] (a-1) The diamine is a diamine having a silicon-oxygen bond and may be a compound represented by formula (I-1):

[0055]

[0056] In formula (I-1), m1 and m2 are each an integer of 1 to 3. Preferably, both m1 and m2 are 1. 1 Each of them is an alkylene or phenylene group having 1 to 5 carbon atoms, wherein when X 1 When it is an alkylene group having 1 to 5 carbon atoms, any one of the -CH2- in the alkylene group having 1 to 5 carbon atoms may be substituted with -NH-. 1 Preferably, it is an alkylene group having 1 to 5 carbon atoms or -CH2CH2NHCH2-, and more preferably, it is a propylene group. In some embodiments of the present invention, the diamine (a-1) may be a compound represented by formula (I-1-1):

[0057]

[0058] In formula (I-1-1), m1 and m2 are each an integer of 1-3, and preferably both are 1. n1 and n2 are each an integer of 1-5, and preferably each are an integer of 1-3, and more preferably both are 3. Specific examples of (a-1) diamines include, but are not limited to, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 1,3-bis-(2-aminoethylaminomethyl)tetramethyldisiloxane, 1,3-bis-(4-aminophenyl)-1,1,3,3-tetramethyldisiloxane, or a combination thereof, wherein 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane is preferred.

[0059] (a-2) Diamine

[0060] The diamine (a-2) is a diamine having four benzene rings and may be a compound represented by formula (I-2):

[0061]

[0062] X in formula (I-2) 2 is a hydrocarbon group having 1 to 10 carbon atoms, -O-, -S-, -SO2-, -NH-, -C(CF3)2- or X 2 It is preferably an alkylene group having 1 to 5 carbon atoms or -C(CF3)2-, and more preferably an alkylene group having 3 carbon atoms. 2 A specific example of an alkylene group having 3 carbon atoms is -C(CH3)2-. Specific examples of (a-2) diamines include, but are not limited to, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane (2,2'-Bis[4-(4-aminophenoxy)phenyl]propane, BAPP), 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, bis(4-(4-aminophenoxy)phenyl)sulfone or a combination thereof, wherein 2,2'-bis[4-(4-aminophenoxy)phenyl]propane is preferred.

[0063] The (a) diamine may further include (a-3) diamine. The (a-3) diamine is a diamine having a phenol structure and may be a compound represented by formula (I-3):

[0064]

[0065] Y of formula (I-3) is -C(CH3)2-, -C(CF3)2-, -CH2-, -O-, -S- or -SO2-, preferably -C(CH3)2-. Specific examples of (a-3) diamines include, but are not limited to, 2,2-bis(3-amino-4-hydroxyphenyl)propane (2,2-bis(3-amino-4-hydroxyphenyl)propane, BAHPP), 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis(3-amino-4-hydroxyphenyl)sulfone or a combination thereof, wherein 2,2-bis(3-amino-4-hydroxyphenyl)propane is preferred.

[0066] (a) The diamine may also include (a-4) diamine and (a-5) diamine. (a-4) diamine is not particularly limited and may be appropriately selected according to needs. In some embodiments of the present invention, it may contain a functional group such as that shown in formula (I-4). Specific examples of (a-4) diamine include, but are not limited to, 3,4'-diaminodiphenyl ether, 3,4-diaminodiphenyl ether, 4,4-diaminodiphenyl ether, 3,4-diaminodiphenyl sulfone, 4,4-diaminodiphenyl sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis(4-amino-3-carboxyphenyl)methane or a combination thereof, wherein 3,4'-diaminodiphenyl ether is preferred. (a) The diamine may also include (a-5) diamine. (a-5) diamine is not particularly limited and may be appropriately selected according to needs. In some embodiments of the present invention, it may contain a functional group such as that shown in formula (I-5). Specific examples of (a-5) diamines include, but are not limited to, di(4-amino-3-carboxyphenyl)methane, 3,5-diaminobenzoic acid, and 6,6'-bisamino-3,3'-methoxydibenzoic acid. (a) Diamines may also include (a-6) diamines, specific examples of which include, but are not limited to, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane.

[0067]

[0068]

[0069] *Indicates the bond position.

[0070] (b) Tetracarboxylic dianhydride

[0071] (b) There is no particular limitation on tetracarboxylic dianhydride, and appropriate tetracarboxylic dianhydride can be selected according to the requirements. Specific examples of (b) tetracarboxylic dianhydride include, but are not limited to, 3,3',4,4'-diphenyl ethertetracarboxylic dianhydride (ODPA), bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, dianhydride, BTA), 1,2,4,5-cyclohexanetetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuran)-3-methyl-3-cyclohexene-1,2-dicarbonic anhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, pyromellitic dianhydride, bis(3,4-dicarboxyphenyl) ether dianhydride, bis(3,4-dicarboxyphenyl) sulfide dianhydride, bis(3,4-dicarboxyphenyl) sulfone dianhydride, bis(3,4-dicarboxyphenyl) methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl) propane dianhydride, 2,2-bis(3,4 -dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic dianhydride or a combination thereof, preferably including 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride or a combination thereof, wherein 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride is preferred.

[0072] (A) Preparation of polyimide resin

[0073] The preparation of the (A) polyimide resin may include at least two stages: (A1) polymerization reaction and (A2) dehydration ring-closure reaction. In the (A1) polymerization reaction, (a) diamine and (b) tetracarboxylic dianhydride are polymerized to form a polyamic acid polymer, and in the (A2) dehydration ring-closure reaction, the amic acid functional group in the polyamic acid polymer is converted into an imide functional group (i.e., imidization) via a dehydration ring-closure reaction to obtain a polyimide resin containing an imide functional group. The following further describes the environment, conditions, other reactants, etc. for preparing the (A) polyimide resin.

[0074] environment

[0075] The (A1) polymerization reaction and the (A2) dehydration ring-closing reaction can be carried out in the presence of a solvent, that is, the preparation material of the (A) polyimide resin can further include a (c) solvent. The (c) solvent can be a polar solvent, including but not limited to N-methylpyrrolidone, γ-butyrolactone, dimethylacetamide, methylformamide, diethylacetamide, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, and hexamethylphosphoric triamide. The listed (c) solvent and other solvents can be selected according to needs, and can be used alone or in combination. For example, the requirements can be based on the solubility of the reactants (such as other preparation materials) to select N-methylpyrrolidone. In some embodiments of the present invention, the weight percentage of the (c) solvent in the (A1) polymerization reaction relative to the total weight of the (a) diamine, (b) tetracarboxylic dianhydride and (c) solvent can be 15-45wt%, preferably 20-35wt%.

[0076] condition

[0077] In some embodiments of the present invention, the polymerization reaction (A1) can be carried out at a temperature of 50-80° C. for 3-6 hours. The dehydration ring-closing reaction (A2) can be carried out by a high-temperature dehydration ring-closing method or a chemical dehydration ring-closing method. In some embodiments of the present invention, the high-temperature dehydration ring-closing method can be carried out at 250-350° C. for 3-6 hours, and the chemical dehydration ring-closing method can be carried out at 160-180° C. for 3-6 hours.

[0078] Other reactants

[0079] In some embodiments of the present invention, the reactants of the polymerization reaction (A1) may further include (d) a blocking agent to control the molecular weight of the polyimide resin. The blocking agent (d) is not particularly limited and may include, but is not limited to, 3-aminophenol, phthalic anhydride, maleic anhydride, nadic acid, cyclohexanedicarboxylic anhydride, 3-hydroxyphthalic anhydride, 3-carboxylphenol, 4-carboxylphenol, 3-carboxylthiophenol, 4-carboxylthiophenol, 1-hydroxy-7-carboxylnaphthalene, 1-hydroxy-6-carboxylnaphthalene, 1-hydroxy-5-carboxylnaphthalene, 1-mercapto-7-carboxylnaphthalene, 1-mercapto-6-carboxylnaphthalene, 1-mercapto-5-carboxylnaphthalene, 3-carboxylbenzenesulfonic acid, 4-carboxylbenzenesulfonic acid, or a combination thereof. The reactants of the dehydration ring-closing reaction (A2) may further include (e) a dehydrating agent and (f) a catalyst. In the chemical dehydration closed-loop method, in some embodiments of the present invention, (e) the dehydrating agent is an anhydride such as acetic anhydride, propionic anhydride, trifluoroacetic anhydride, etc., but the present invention is not limited thereto, and other dehydrating agents can be selected as needed. (f) the catalyst can be a tertiary amine such as 1-ethylpiperidine, triethylamine, pyridine, and lutidine, but the present invention is not limited thereto, and other catalysts can be selected as needed.

[0080] In addition to the aforementioned (a) diamine and (b) tetracarboxylic dianhydride, in some embodiments of the present invention, other diamines and tetracarboxylic dianhydrides may be appropriately selected as needed, for example, according to the disclosures of patent applications such as publication numbers TW202128837A, TW202128842A, TW202233722A, US2021 / 0223699A1, US2022 / 0275205A1, and publication numbers CN114957660A, CN113219796A, etc., other diamines and tetracarboxylic dianhydrides are selected as (a) diamine and (b) tetracarboxylic dianhydride to react and obtain (A) polyimide resin. In addition, regarding the preparation of (A) polyimide resin, in some embodiments of the present invention, in addition to the aforementioned environment, conditions, and other reactants, without violating the disclosure herein, the polyimide resin (A) may also be prepared according to the disclosures of the aforementioned patent applications.

[0081] (B) Photo Active Compound (PAC)

[0082] The (B) photosensitive compound is preferably a compound having a quinonediazide group, such as quinonediazidesulfonic acid, quinonediazidesulfonic acid derivatives or combinations thereof, or other substances that are photosensitized to an I-line light source. The (B) photosensitive compound is also preferably a substance that can significantly increase the contrast of the alkali dissolution rate between the exposed area and the non-exposed area of ​​the positive photoresist composition in the positive photoresist patterning process, thereby facilitating the preparation of a high-resolution positive photoresist film. The compound having a quinonediazide group is not particularly limited. In some embodiments of the present invention, it is usually naphthoquinonediazidesulfonyl chloride (e.g., 1,2-naphthoquinonediazide-5-sulfonyl chloride, 1,2-naphthoquinonediazide-4-sulfonyl chloride, etc.) or benzoquinonediazidesulfonyl chloride, etc. In some embodiments of the present invention, for example, the photosensitive compound (B) can be obtained by reacting a quinonediazide compound containing an acid chloride with a low molecular weight compound or a high molecular weight compound, and the low molecular weight compound or the high molecular weight compound has a functional group for condensing with the quinonediazide compound containing an acid chloride. In some embodiments of the present invention, the functional group capable of condensing with the quinonediazide compound containing an acid chloride is mainly a hydroxyl group (hereinafter referred to as a hydroxyl compound), which may include but is not limited to hydroxyphenyl ketones (e.g., hydroquinone, resorcinol, 2,4-dihydroxyphenyl ketone, 2,3,4-trihydroxyphenyl ketone, 2,4,6-trihydroxyphenyl ketone, 2,4,4'-trihydroxyphenyl ketone, 2,3,4,4'-tetrahydroxyphenyl ketone, 2,2',4,4'-tetrahydroxyphenyl ketone, 2,2',3,4,6'-pentahydroxyphenyl ketone (B) Specific examples of photosensitive compounds include PAC1 and PAC2 (described later).

[0083] (C) Solvent

[0084] The (C) solvent is not particularly limited. Preferably, the (C) solvent is the (c) solvent used in synthesizing the (A) polyimide resin. Specific examples of (C) solvents include, but are not limited to, N-methylpyrrolidone, γ-butyrolactone, γ-butyrolactam, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monomethyl ether, butyl lactate, butyl acetate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol n-propyl ether, ethylene glycol isopropyl ether, ethylene glycol n-butyl ether, ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, N,N-dimethylformamide, N,N-dimethylacetamide, or a combination of the foregoing solvents.

[0085] In addition to (A) polyimide resin, (B) photosensitive compound and (C) solvent, the positive photoresist composition may further include (D) additives without affecting the efficacy of the present invention. (D) Additives are not particularly limited and can be appropriately selected according to needs. (D) Additives may include, for example, (D-1) leveling agents to suppress the generation of stripes and increase film thickness uniformity, (D-2) adhesion promoters to improve the adhesion between the photoresist composition and the substrate, (D-3) ultraviolet absorbers to prevent standing wave effects caused by light reflection, but are not limited to these. For example, (D) additives may also include antioxidants, anti-aging agents, and inorganic particles with a light scattering effect.

[0086] Table 1 and Examples 1-4 below illustrate the preparation and materials of the polyimide resin (A) of the present invention. Table 2-1 and Examples 5-11 below illustrate the composition and preparation of the positive photoresist composition of the present invention. Table 2-2 and Comparative Examples 1-4 below serve as controls for Examples 5-11.

[0087] Example 1

[0088] The preparation materials of (A) polyimide resin of Example 1 are shown in Table 1. (a-1) diamine, (a-2) diamine, (a-3) diamine, (a-4) diamine and (b) tetracarboxylic dianhydride including 8.981 g (0.036 mol) of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, 59.340 g (0.015 mol) of 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 37.340 g (0.0145 mol) of 2,2 -bis(3-amino-4-hydroxyphenyl)propane, 7.236 g (0.036 mol) of 3,4-diaminodiphenyl ether and 112.103 g (0.360 mol) of 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride were added to a 1000 ml three-necked round-bottom flask with nitrogen and equipped with a mechanical stirrer, and then (C) 673.200 g of N-methylpyrrolidone as solvent was added and stirred at 70°C for 4 hours. Then, (f) 1.800 g of 1-ethylpiperidine as catalyst was added, the temperature was raised to 180°C and stirred for 4 hours. Then, cooling was performed to obtain a polyimide resin solution. The ratio of the four diamine monomers (a-1) diamine: (a-2) diamine: (a-3) diamine: (a-4) diamine is 0.1:0.4:0.4:0.1.

[0089] Embodiment 2-4

[0090] The preparation materials of each (A) polyimide resin in Examples 2-4 and the ratios of various diamine monomers are shown in Table 1. The preparation of each (A) polyimide resin in Examples 2-4 is the same as that in Example 1.

[0091] Table 1: (A) Polyimide resin of Examples 1-4

[0092]

[0093] Example 5

[0094] The composition of the positive photoresist composition of Example 5 is shown in Table 2-1. In Example 5, 37.46 parts by weight of (A) polyimide resin (solid content of 34.7 wt%) of Example 1 and 2.60 parts by weight of (B) photosensitive compound PAC1 having quinone diazide group were added, 84.35 parts by weight of (C) solvent N-methylpyrrolidone were added, mixed and stirred, and filtered using a 0.1 micron filter to prepare a positive photoresist composition.

[0095]

[0096] Preferably, at least one R has a quinonediazide group.

[0097] Embodiment 6-11

[0098] The compositions of the positive photoresist compositions of Examples 6-11 are shown in Table 2-1. The preparation of the positive photoresist compositions of Examples 6-11 is substantially the same as that of Example 5, except that the amount of (A) polyimide resin, (B) photosensitive compound, and (C) solvent may still be different from that of Example 5.

[0099] Table 2-1: Positive photoresist composition of Examples 5-11

[0100]

[0101]

[0102] Preferably, at least one R has a quinonediazide group.

[0103] Comparative Examples 1-4

[0104] The preparation of each positive photoresist composition in Comparative Examples 1-4 is the same as that in Example 5, except that in Comparative Examples 1-3, the resin used is a novolac resin commonly used in conventional positive photoresists, and the structure can be shown in the following figure.

[0105]

[0106] The solvent used is PGMEA (propylene glycol methyl ether acetate), and the composition is shown in Table 2-2. In Comparative Example 4, the resin used is PHS resin commonly used in conventional positive amplification photoresists, and the structure can be shown in the following figure, where x is, for example, 60, y is, for example, 20, and z is, for example, 20:

[0107]

[0108] The photosensitive material used is a photoacid generator (PAG) with a structure as shown below:

[0109]

[0110] The solvent used is PGMEA (propylene glycol methyl ether acetate), as shown in Table 2-2.

[0111] Table 2-2: Positive photoresist compositions of Comparative Examples 1-4

[0112]

[0113] Positive photoresist film

[0114] The positive photoresist composition of the present invention can be used for the preparation of positive photoresist films and the lithography process of positive photoresist patterns. Figure 1As shown, the lithography process of the positive photoresist pattern of the present invention includes step S110: coating the positive photoresist composition as described above on the substrate, step S120: heating the positive photoresist composition and forming a film layer, and step S130: patterning the film layer and forming a positive photoresist pattern. In some embodiments of the present invention, step S120 further includes baking at 100-130°C, for example, it can be baked on a hot plate at 100°C. Step S130 further includes exposing and developing the film layer. The following further describes the coating, heating, exposure, and development of the positive photoresist pattern lithography process.

[0115] Coating

[0116] The present invention does not limit the coating method, but for example, the coating method can be, for example, spin coating, roller coating, screen coating, curtain coating, dip coating, or spray coating, but is not limited thereto. The substrate can be, for example, a silicon substrate, glass, or indium tin oxide (ITO) glass, and any desired film layer can be formed on the substrate.

[0117] heating

[0118] In some embodiments of the present invention, baking at 100-130° C. can also be used to evaporate the (C) solvent.

[0119] exposure

[0120] The exposure further includes placing a mask on the substrate with the film layer formed thereon, and exposing the film layer to actinic radiation under the mask. The actinic radiation is, for example, X-rays, electron beams, ultraviolet rays, visible rays, or other light sources that can serve as actinic radiation. The energy used for exposure can affect the thickness of the positive photoresist film and the resolution of the pattern (described later).

[0121] development

[0122] In some embodiments of the present invention, an alkaline aqueous developer is used for development to remove the exposed portion of the positive photoresist film layer to obtain a pattern (graphic). The alkaline aqueous developer includes an alkaline aqueous solution. The alkaline aqueous solution may be, for example, an aqueous solution of an inorganic base (e.g., potassium hydroxide or sodium hydroxide), a primary amine (e.g., ethylamine), a secondary amine (e.g., diethylamine), a tertiary amine (e.g., triethylamine), or a quaternary ammonium salt (e.g., tetramethylammonium hydroxide), wherein an aqueous solution containing tetramethylammonium hydroxide is preferred. The present invention does not limit the method of development, but for example, development may be accomplished by soaking, spraying, coating, or other known methods. Preferably, the positive photoresist pattern obtained by development may then be washed with deionized water and then blown dry with an air gun. The development time may affect the thickness of the positive photoresist film and the resolution of the pattern (described later).

[0123] Example 12 illustrates the preparation of positive photoresist films using the compositions of Examples 5-11 and Comparative Examples 1-4. Table 3-1 below and Example 13 illustrate the evaluation method of the pattern of the positive photoresist film, and the preferred pattern resolution that can be achieved by each positive photoresist film prepared using the compositions of Examples 5-11 and Comparative Examples 1-4. Table 3-1 below and Example 14 illustrate the solvent resistance test and test results of each positive photoresist film prepared using the compositions of Examples 5-11 and Comparative Examples 1-4.

[0124] Example 12

[0125] In the preparation of the positive photoresist film of Example 12, the positive photoresist compositions of Examples 5-11 and Comparative Examples 1-4 are coated on the substrate using a spin coating method, and baked on a 100°C hot plate for 360 seconds, and then exposed using a Canon FPA5500iZa exposure machine. The exposure energy is 1000-5000 J / m2, Focus = 0. Then, it is developed for 30 seconds using a 0.3% tetramethylammonium hydroxide (TMAH) developer. The obtained positive photoresist film has a film thickness of 0.6 microns and a graphic resolution of 0.6 microns. In addition, by testing various exposure energies and development times, the minimum resolution of the graphics of each positive photoresist film at a thickness of 0.6 microns can be obtained.

[0126] Embodiment 13

[0127] In the pattern evaluation method of Example 13, a field emission scanning electron microscope (FESEM) SU-8010 was used to confirm the resolution of the positive photoresist films obtained after development of each composition of Examples 5-11 and Comparative Examples 1-4, and to test the optimal pattern resolution that can be achieved by the positive photoresist film at a thickness of 0.6 microns under various exposure energies and development conditions. The smaller the resolution value, the better.

[0128] Embodiment 14

[0129] In the solvent resistance test of Example 14, a mixed solvent of PGMEA and OK73 (propylene glycol methyl ether / propylene glycol methyl ether acetate = 70 / 30) was selected to test the solvent resistance of the positive photoresist film. PGMEA and OK73 are also commonly used solvents for negative photoresist compositions. The positive photoresist films obtained after development of each composition of Examples 5-11 and Comparative Examples 1-4 were respectively subjected to 6 ml of spin coating with a mixed solvent of PGMEA and OK73. Afterwards, a field emission scanning electron microscope (FESEM) SU-8010 was used to observe whether the profile of the positive photoresist film pattern was complete, and whether there was any disappearance or deformation or incompleteness. The one with disappearance or incompleteness was unqualified and marked as ×. The one without disappearance and incompleteness was qualified and marked as ○. The positive photoresist film obtained by the composition had no disappearance and incompleteness, indicating that the composition and its positive photoresist film were suitable for the lithography process of the negative photoresist pattern (described later).

[0130] Table 3-1

[0131] Minimum resolution (μm) PGMEA test resistance OK73 test resistance Example 5 0.6 ○ ○ Example 6 0.5 ○ ○ Example 7 0.4 ○ ○ Example 8 0.6 ○ ○ Example 9 0.4 ○ ○ Example 10 0.4 ○ ○ Embodiment 11 0.4 ○ ○ Comparative Example 1 0.6 × × Comparative Example 2 0.5 × × Comparative Example 3 0.4 × × Comparative Example 4 0.4 × ×

[0132] Negative photoresist pattern lithography process and negative photoresist pattern obtained therefrom

[0133] The positive photoresist composition of the present invention is also suitable for the lithography process of negative photoresist patterns. The present invention also provides a lithography process method of negative photoresist patterns. Figure 2 As shown, the lithography process of the negative photoresist pattern includes step S210: coating the aforementioned positive photoresist composition on the substrate, step S220: heating the positive photoresist composition and forming a film layer, step S230: patterning the film layer and forming a positive photoresist pattern, step S240: coating the negative photoresist composition on the substrate, step S250: heating the negative photoresist composition, step S260: patterning the film layer and forming a negative photoresist pattern. Step S210 is substantially equivalent to step S110, step S220 is substantially equivalent to step S120, and step S230 is substantially equivalent to step S130, that is, the lithography process of the negative photoresist pattern of the present invention uses the positive photoresist composition of the present invention and the positive photoresist pattern obtained therefrom. Further explanation is as follows.

[0134] Please refer to Figures 3A-3E . Figure 3A-3B is a schematic diagram of steps S210-S230. Figure 3B As shown, step S230 further includes using a mask 5 to define a first region 31 and a second region 32 on the substrate using the positive photoresist pattern 30 . Figure 3C-3E is a schematic diagram of steps S240-S260. Figure 3C As shown, step S240 further includes distributing the negative photoresist composition 4 in the second region 32. In some embodiments, as Figure 3C As shown, step S240 further includes distributing a negative photoresist composition 4 in the first region 31, and the negative photoresist composition 4 distributed in the first region 31 covers the positive photoresist pattern 30. As long as the solvent contained in the negative photoresist composition is different from the aforementioned (C) solvent and / or (c) solvent, the present invention does not limit the negative photoresist composition used in steps S240-S260 in principle. The method of coating the negative photoresist composition 4 can refer to the above, and will not be repeated here. In addition, the method of coating the negative photoresist composition 4 can further affect whether the negative photoresist composition 4 is distributed in the first region 31.

[0135] As described above, in the embodiment where the negative photoresist composition 4 is distributed in the first region 31, the negative photoresist composition 4 has different distribution heights in the first region 31 and the second region 32, and the distribution heights can be different based on the positive photoresist pattern 30. For example, when the thickness of the positive photoresist pattern 30 is greater, the second region 32 is also surrounded by a higher positive photoresist pattern 30, and the height of the negative photoresist composition 4 in the second region 32 can be higher. Preferably, the height of the negative photoresist composition 4 in the first region 31 is less than that in the second region 32.

[0136] In some embodiments of the present invention, step S250 further includes baking at 80-120° C., and step S260 further includes exposing and developing the film layer. Figure 3D As shown, the exposure position of step S260 is the same as the exposure position of step S230, that is, the negative photoresist composition 4 distributed in the second area 32 is exposed. Figure 3E As shown, after development, the unexposed portion of the negative photoresist composition is removed to obtain a negative photoresist pattern 40, wherein the positive photoresist pattern 30 and the unexposed negative photoresist composition 4 are also removed at the same time during development. Figure 3D-3EAs shown, the height of the unexposed negative photoresist composition is smaller because there is a positive photoresist pattern 30 underneath, so the volume to be removed is smaller and the time required for development is shorter, thereby reducing the probability of swelling, scum, undercut, etc. of the negative photoresist pattern 40, which helps to improve the quality and resolution of the negative photoresist pattern 40. The radiation used for exposure and the developer used for development in step S260 are as described above and will not be repeated here.

[0137] Example 15 illustrates the preparation of negative photoresist patterns using the compositions of Examples 5-11 and Comparative Examples 1-4, and the evaluation of the prepared negative photoresist patterns.

[0138] Embodiment 15

[0139] In the preparation of the negative photoresist pattern of Example 15, the positive photoresist film patterns obtained after development of each composition of Examples 5-11 and Comparative Examples 1-4 were taken, and 6cc of negative photoresist was spin-coated respectively. In some embodiments of the present invention, the negative photoresist is composed of 12wt% acrylic resin, 6wt% polymerizable monomer, 2wt% photoinitiator, and 80wt% PGMEA solvent. Then, observe whether there is color contamination on the film surface. Then, expose with a mask to cause a cross-linking reaction in the negative photoresist. Then, develop with a 0.3% TMAH developer for 80 seconds to obtain a negative photoresist pattern, and at the same time completely remove the positive photoresist film pattern on the substrate so that only the negative photoresist pattern is left on the substrate. Then, use a field emission scanning electron microscope (FESEM) SU-8010 to observe whether the profile of the negative photoresist pattern is complete, and whether there is deformation, color contamination, residue, etc. If there are deformations, color stains, residues, etc., it is unqualified and marked as ×. If the profile is complete without deformation, color stains, residues, etc., it is qualified and marked as ○. The results are shown in Table 3-2 below.

[0140] Table 3-2

[0141] Negative photoresist pattern evaluation Example 5 ○ Example 6 ○ Example 7 ○ Example 8 ○ Example 9 ○ Example 10 ○ Embodiment 11 ○ Comparative Example 1 × Comparative Example 2 × Comparative Example 3 × Comparative Example 4 ×

[0142] According to Examples 12-15 and Tables 3-1 and 3-2, the positive photoresist film pattern obtained by the positive photoresist composition of the embodiments of the present invention can reach a high resolution of 0.4 microns, and the solvent resistance of the film pattern after development is good. Furthermore, when a negative photoresist is coated on the positive photoresist film pattern, the film pattern will not dissolve and will not produce color pollution. In contrast, the positive photoresist film pattern obtained by the positive photoresist composition of Comparative Examples 1-4, although its resolution can also reach 0.4 microns, its solvent resistance is poor, and after the coating and development of the negative photoresist, its film pattern will produce serious color pollution due to dissolution. Therefore, the positive photoresist composition of the present invention is suitable for the lithography process method of the negative photoresist pattern of the present invention, and a negative photoresist pattern is obtained. The lithography process method of the negative photoresist pattern of the present invention improves swelling, scum, undercut and other conditions of the conventional negative photoresist pattern and helps to obtain a high-resolution negative photoresist pattern.

[0143] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes by using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A positive photoresist composition, characterized in that: include: (A) polyimide resin; the polyimide resin (A) is obtained by polymerization of (a) diamine and (b) tetracarboxylic dianhydride, and has a structural unit represented by formula (1) (B) a photosensitive compound; as well as (C) a solvent; Among them, Ar in formula (1) 1 is a tetravalent organic group, Ar 2 is a divalent organic group, and Ar 1 A group represented by formula (B-1), formula (B-2), formula (B-3) or a combination thereof * indicates the bond position; Ar in formula (1) 2 Containing a group represented by formula (A-1), formula (A-2) or a combination thereof Wherein, m1 and m2 of formula (A-1) are each an integer of 1 to 3, and X 1 Each is an alkylene or phenylene group having 1 to 5 carbon atoms; wherein, when X 1 When it is an alkylene group having 1 to 5 carbon atoms, any one of the -CH2- in the alkylene group having 1 to 5 carbon atoms may be substituted by -NH-; X in formula (A-2) 2 is a hydrocarbon group having 1 to 10 carbon atoms, -O-, -S-, -SO2-, -NH-, -C(CF3)2- or 2. The positive photoresist composition according to claim 1, wherein: Ar 2 Further comprising a group represented by formula (A-3), formula (A-4), formula (A-5) or a combination thereof Wherein, Y in formula (A-3) is -C(CH3)2-, -C(CF3)2-, -CH2-, -O-, -S- or -SO2-; * indicates the bonding position.

3. The positive photoresist composition according to claim 1, wherein: The (a) diamine includes (a-1) diamine and (a-2) diamine; the (a-1) diamine is a diamine having a silicon-oxygen bond and is a compound represented by formula (I-1); the (a-2) diamine is a diamine having four benzene rings and is a compound represented by formula (I-2) Wherein, m1 and m2 of formula (I-1) are each an integer of 1 to 3, and X 1 Each is an alkylene or phenylene group having 1 to 5 carbon atoms; wherein, when X 1 When it is an alkylene group having 1 to 5 carbon atoms, any one of the -CH2- in the alkylene group having 1 to 5 carbon atoms may be substituted by -NH-; X in formula (I-2) 2 is a hydrocarbon group having 1 to 10 carbon atoms, -O-, -S-, -SO2-, -NH-, -C(CF3)2- or 4. The positive photoresist composition according to claim 3, wherein: The (a) diamine further includes (a-3) diamine; the (a-3) diamine is a diamine having a phenol structure and is a compound represented by formula (I-3): Wherein, Y in formula (I-3) is -C(CH3)2-, -C(CF3)2-, -CH2-, -O-, -S- or -SO2-.

5. The positive photoresist composition according to claim 1, wherein: The weight average molecular weight of the (A) polyimide resin is 5,000-50,000.

6. The positive photoresist composition according to claim 1, wherein: The (B) photosensitive compound is quinonediazidesulfonic acid, quinonediazidesulfonic acid derivatives or a combination thereof; when the amount of the (A) polyimide resin is 100 parts by weight, the amount of the (B) photosensitive compound is 10-150 parts by weight.

7. The positive photoresist composition according to claim 1, wherein: The (C) solvent is N-methylpyrrolidone, γ-butyrolactone, ethyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide or a combination thereof, and the (C) solvent accounts for 50-90% by weight of the positive photoresist composition.

8. A lithography process method for a negative photoresist pattern, characterized in that: include: Coating the positive photoresist composition as claimed in any one of claims 1 to 7 on a substrate; heating the positive photoresist composition to form a film layer; Patterning the film layer to form a positive photoresist pattern; coating a negative photoresist composition on the substrate; heating the negative photoresist composition; The film layer is patterned to form a negative photoresist pattern.

9. The method according to claim 8, characterized in that The step of patterning the film layer and forming the positive photoresist pattern further includes exposing and developing the film layer, and the step of patterning the film layer and forming the negative photoresist pattern further includes exposing and developing the film layer, and the positions of the two exposures are the same.

10. The method according to claim 8, characterized in that The step of heating the positive photoresist composition further includes baking at 100-130° C., and the step of heating the negative photoresist composition further includes baking at 80-120° C.

11. The method according to claim 8, characterized in that The step of patterning the film layer and forming the positive photoresist pattern further includes allowing the positive photoresist pattern to define a first region and a second region on the substrate.

12. The method according to claim 11, characterized in that The step of coating the negative photoresist composition on the substrate further includes distributing the negative photoresist composition in the second region.

13. The method according to claim 12, characterized in that The step of coating the negative photoresist composition on the substrate further includes distributing the negative photoresist composition in the first region, and the negative photoresist composition distributed in the first region covers the positive photoresist pattern.

14. The method according to claim 11, characterized in that The step of coating the negative photoresist composition on the substrate further includes distributing the negative photoresist composition in the second area; the step of patterning the film layer and forming the negative photoresist pattern further includes exposing the negative photoresist composition distributed in the second area to form the negative photoresist pattern.

15. The method according to claim 14, characterized in that The step of patterning the film layer and forming the negative photoresist pattern further includes developing with an alkaline aqueous solution and removing the positive photoresist pattern.

16. The method according to claim 8, characterized in that The method further comprises preparing the positive photoresist composition using (A) a polyimide resin, (B) a photosensitive compound and (C) a solvent; wherein the (A) polyimide resin has a structural unit represented by formula (1), Ar 1 and Ar 2 As defined in claim 1 17. The method according to claim 16, characterized in that The step of preparing the positive photoresist composition further includes using (a) a diamine and (b) a tetracarboxylic dianhydride to perform a polymerization reaction to provide the (A) polyimide resin.