High-saturation low-loss soft magnetic composite material and preparation method and application thereof

By mixing the first powder containing iron, silicon, chromium with the second powder containing iron and nickel, and mixing it with resin for pressing and low temperature heat treatment, the low magnetic permeability of soft magnetic composite materials in the prior art is solved. The thermal aging problem has achieved the preparation of soft magnetic materials with high saturation and low loss, which is suitable for the lightweight and thinning needs of electronic products.

CN118899141AActive Publication Date: 2024-11-05HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410983581.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-05
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The prior art cannot prepare soft magnetic composite materials with high saturation and low loss without damaging the coil insulation layer. The traditional inductor materials have low magnetic permeability and poor saturation characteristics, and the thermal aging problem is prominent, which cannot meet the lightness and thinness of electronic products. , miniaturization needs.

Method used

The first powder (including iron, silicon, chromium) and the second powder (including iron, nickel) are mixed with the resin, and press and heat treatment are carried out. The heat treatment temperature is not higher than 220℃ to avoid high-temperature baking. Defects, improve the permeability and moldability of the material.

Benefits of technology

Soft magnetic materials with high saturation characteristics, low loss and high pressure density are achieved, which solves the problems of low magnetic permeability, poor saturation characteristics and thermal aging of traditional inductor materials, simplifies the preparation process, improves the corrosion resistance and DC of the material. Overlay characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004956758640000091
    Figure BDA0004956758640000091
Patent Text Reader

Abstract

The invention belongs to the technical field of magnetic material preparation, and particularly relates to a high-saturation low-loss soft magnetic composite material and a preparation method and application thereof. The preparation method comprises the following steps: (1) uniformly mixing first powder and second powder to obtain a mixture; wherein the components of the first powder comprise iron, silicon and chromium, and the components of the second powder comprise iron and nickel; (2) mixing the mixture with resin, pressing, and carrying out heat treatment; the heat treatment temperature is not higher than 220 DEG C. The soft magnetic material with high saturation characteristic, low loss and high pressing density can be prepared, the formability is good when the soft magnetic material is prepared, and the soft magnetic material is not prone to cracking in the heat treatment process. Complex steps such as coating are not needed when the high-saturation low-loss material is prepared, and the working procedure is simplified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of magnetic material preparation, and specifically relates to a high-saturation, low-loss soft magnetic composite material and a preparation method and application thereof. Background Art

[0002] As the core component of electronic products, inductors have higher requirements on the performance of inductor materials in order to meet the needs of electronic products being thinner and smaller. Traditional molded inductors are formed by integrating coils and powders, and then baked at low temperatures. This is because high-temperature sintering will damage the insulation layer of the coil and cause short circuits between coil layers. The powders of traditional inductors are mostly carbonyl powders, iron silicon powders, iron silicon chromium powders, etc., and the glue used is mostly epoxy resin. The powders prepared in this way have low magnetic permeability, poor saturation characteristics, and high losses. In addition, low-temperature baking cannot enable the powder to exert its magnetic properties; carbonyl powders have thermal aging problems and cannot meet long-term temperature resistance above 130°C. For example, in the preparation of low-loss materials, the prior art uses a mixture of iron silicon aluminum alloy powder and carbonyl iron for phosphating treatment, and then coating, granulation, and baking. Although this method can reduce losses, it still has problems such as low Bs, poor saturation characteristics, and low pressing density.

[0003] Copper-iron co-fired inductors are made by molding alloy powder and copper sheet into one piece and then sintering at high temperature, which greatly reduces losses and improves the magnetic permeability of the powder. However, this type of inductor requires the use of inorganic glue for high-temperature sintering, has poor bonding strength, and is prone to cracking during molding, especially some thinner inductors. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the problem that the prior art cannot make soft magnetic composite materials have high saturation characteristics, low loss, not easy to crack, good formability, etc., so as to provide a high saturation and low loss soft magnetic composite material and its preparation method and application.

[0005] To this end, the present invention provides the following technical solutions.

[0006] The first aspect of the present invention provides a method for preparing a high saturation and low loss soft magnetic composite material, comprising the following steps:

[0007] (1) mixing a first powder and a second powder to obtain a mixture; wherein the first powder comprises iron, silicon, and chromium, and the second powder comprises iron and nickel;

[0008] (2) The mixed material is mixed with resin, pressed and heat treated; the temperature of the heat treatment is not higher than 220°C.

[0009] The present invention uses a first powder and a second powder of specific components to make the soft magnetic material have good magnetic permeability without the need for insulating coating treatment, and can reduce losses, have good DC superposition characteristics, and be easy to press and form. It does not require high-temperature baking. Heat treatment at no more than 220°C can ensure the excellent performance of the composite material, and in particular, the heat treatment process can be carried out at less than 200°C, which overcomes the defect of the prior art that high-temperature baking is required.

[0010] The first powder contains iron, silicon, and chromium, making the first powder an amorphous powder without grain boundaries and grains, which helps the soft magnetic material to present excellent properties such as high sphericity, high resistivity, high saturation magnetic induction intensity, corrosion resistance, low coercivity and low loss. The second powder includes iron and nickel, which helps to improve the saturation magnetic induction and DC superposition characteristics of the material, reduce eddy current loss, and facilitate compression molding. The compounding of the first powder and the second powder enables the soft magnetic composite material to take into account the characteristics of high saturation and low loss, and improves the problem of cracking of ultra-thin magnetic cores.

[0011] The D50 of the first powder is 10-20 μm, and the D50 of the second powder is 0.5-2 μm; and / or,

[0012] The mass ratio of the first powder to the second powder is (3-7):(3-7).

[0013] The D50 of the first powder may be any one of 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, and 20 μm, or an interval between any two values.

[0014] The D50 of the second powder can be any value among 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm, 2.0μm or any value in the interval consisting of two values.

[0015] Furthermore, the mass ratio of the first powder to the second powder of the present invention can be, but is not limited to, 2:3, 1:1, 4:5, 7:3, etc., and is preferably 2:3.

[0016] The present invention regulates the mass ratio and particle size distribution of the first powder and the second powder, which can further improve the filling rate and the pressing density, thereby improving the magnetic permeability of the composite material. The present invention regulates the median particle size of the second powder, which helps to reduce eddy current loss.

[0017] In terms of mass percentage, the iron content in the first powder is 95-97%; and / or,

[0018] The silicon content in the first powder is 2.0-2.6%; and / or,

[0019] The chromium content in the first powder is 1.0-1.5%.

[0020] Furthermore, the first powder material further comprises aluminum and / or manganese in terms of mass percentage;

[0021] Furthermore, the aluminum content in the first powder is 0.02-0.15% by mass percentage;

[0022] Furthermore, in terms of mass percentage, the manganese content in the first powder is 0.01-0.05%.

[0023] For example, the iron content in the first powder can be any value such as 95%, 95.5%, 96%, 96.5%, 97%, etc.; the silicon content can be any value such as 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, etc.; the chromium content can be any value such as 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, etc.; the manganese content can be any value such as 0.02%, 0.04%, 0.06%, 0.08%, 0.1%, 0.12%, 0.14%, 0.15%, etc.; the aluminum content can be any value such as 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, etc. It should be noted that there are inevitable components in the first powder.

[0024] Furthermore, the iron content in the second powder is 47-52% by mass; and / or,

[0025] The nickel content in the second powder is 47-52%.

[0026] The second powder further comprises at least one of manganese, carbon and oxygen;

[0027] Preferably, in terms of mass percentage, the manganese content in the second powder is less than 0.5%;

[0028] Preferably, C<800ppm and O<8000ppm in the second powder.

[0029] The iron content in the second powder can be any value such as 47%, 48%, 49%, 50%, 51%, 52%, etc.; the nickel content can be any value such as 47%, 48%, 49%, 50%, 51%, 52%, etc.; the manganese content is not less than 0.5%, such as 0.4%, 0.3%, 0.2%, etc. It should be noted that there are inevitable components in the second powder.

[0030] The preparation method satisfies at least one of (1) to (2):

[0031] (1) the resin comprises at least two of epoxy resin, polyester resin, polyethylene glycol, polyvinyl butyral resin, micronized wax and phenolic resin; and / or,

[0032] The resin includes epoxy resin and polyvinyl butyral resin; and / or,

[0033] The resin is added in an amount of 1.2 to 1.8 wt % of the mixture;

[0034] In the present invention, the resin accounts for 1.5% of the mass of the mixed material.

[0035] It should be noted that the resin includes at least two of epoxy resin, polyester resin, polyethylene glycol, polyvinyl butyral resin, micro-powder wax and phenolic resin. The ratio between any resins can be determined as needed, for example, the mass ratio of epoxy resin to polyvinyl butyral resin is (3-5):1, preferably 4:1; for another example, polyester resin and polyvinyl butyral resin are compounded for use. Among them, epoxy resin, polyester resin, polyvinyl butyral resin, micro-powder wax, phenolic resin, etc. can all be obtained commercially, and there is no specific restriction on their sources.

[0036] (2) The step (2), when the mixture is mixed with the resin, further comprises the step of adding a coupling agent;

[0037] The coupling agent is added in an amount of 0.2-0.5 wt % of the mixture.

[0038] It should be noted that the coupling agent can be added as needed, and the present invention does not specifically limit the type of coupling agent, such as silane coupling agent, titanate coupling agent, etc., and specific grades include A171, A151, etc.

[0039] The pressing pressure is 12-15 T / cm 2 , and / or,

[0040] The heat treatment time is 4 to 5 hours and / or,

[0041] The temperature of the heat treatment is 180-220°C.

[0042] The present invention can perform heat treatment at a temperature lower than 220°C when preparing soft magnetic composite materials, thereby overcoming the defect of the prior art that high-temperature heat treatment is required. The heat treatment temperature of the present invention can be but is not limited to 180°C, 183°C, 185°C, 188°C, 190°C, 193°C, 195°C, 198°C, 200°C, 203°C, 205°C, 210°C, 215°C, etc.

[0043] The heat treatment time can be 4h, 4.2h, 4.5h, 4.8h, 5h, etc.

[0044] The pressing pressure is 12T / cm 2 , 12.5T / cm 2 , 13T / cm 2 , 13.5T / cm 2 , 14T / cm 2 , 14.5T / cm 2 , 15T / cm 2 Any other value.

[0045] The second aspect of the present invention provides a high-saturation and low-loss soft magnetic composite material obtained by the above preparation method.

[0046] A third aspect of the present invention provides an inductor device, comprising the high-saturation and low-loss soft magnetic composite material prepared by the above preparation method.

[0047] The soft magnetic composite material is made into an inductor by conventional methods in the art. For example, the soft magnetic composite material is integrally formed with a copper sheet during a pressing process; or the soft magnetic composite material is combined with a coil to form an inductor.

[0048] The technical solution of the present invention has the following advantages:

[0049] 1. The preparation method of the high-saturation and low-loss soft magnetic composite material provided by the present invention comprises (1) mixing a first powder and a second powder to obtain a mixture; wherein the first powder comprises iron, silicon, and chromium, and the second powder comprises iron and nickel; (2) the mixture is mixed with a resin, pressed, and heat-treated; the temperature of the heat treatment is not higher than 220°C. The present invention can prepare a soft magnetic material with high saturation characteristics, low loss, and high pressing density, and has good formability when preparing the soft magnetic material, and is not prone to cracking during the heat treatment process. The present invention does not require more complicated steps such as coating when preparing the high-saturation and low-loss material, thereby simplifying the process.

[0050] The first powder material of the present invention comprises iron, silicon and chromium, is an amorphous powder, has no grain boundaries and grains, and exhibits excellent properties of high sphericity, high resistivity and high saturation magnetic induction intensity, corrosion resistance, low coercive force and low loss; the second powder material comprises iron and nickel, has high saturation magnetic induction Bs, has good DC superposition characteristics, low eddy current loss, and is easy to be pressed and formed; the first powder and the second powder are used together without the need for insulation coating treatment, so that the soft magnetic composite material has good magnetic permeability, and the first powder and the second powder are mixed and resin is added to have good formability. Heat treatment at a relatively low temperature (not higher than 220°C) can make the soft magnetic material have both high saturation and low loss, thereby improving the problem of cracking of ultra-thin magnetic cores.

[0051] The inductor device made of the soft magnetic composite material provided by the present invention can be applied to high-computing power application scenarios such as autonomous driving, AI servers, and mining machines, and has the advantages of high current resistance and high efficiency.

[0052] 2. The present invention provides a method for preparing a high-saturation, low-loss soft magnetic composite material. The present invention regulates the mass ratio and particle size grading of the first powder and the second powder to increase the filling rate and pressing density, thereby increasing the magnetic permeability of the composite material.

[0053] Furthermore, the present invention controls the particle size of the second powder, which is relatively small, with a median particle size of 0.5 to 2 μm, and is easy to press and form. Since the eddy current loss in components is proportional to the particle size, the present invention uses a second powder (iron-nickel powder) with a smaller particle size to reduce eddy current loss.

[0054] 3. The preparation method of the high saturation and low loss soft magnetic composite material provided by the present invention, the present invention adopts mixed resin, which can improve the bonding force and formability between particles, and further improve the problem of easy cracking of ultra-thin magnetic cores; the mixed resin of the present invention has high bonding strength and toughness, which can improve the interface of organic or inorganic substances, further improve the insulation resistance of powder materials, and reduce the eddy current loss of magnetic cores. The toughness of the composite resin used in the present invention is good, which can inhibit the cracking caused by the expansion of the resin during the heat treatment process. DETAILED DESCRIPTION

[0055] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0056] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0057] Example 1

[0058] This embodiment provides a method for preparing a high-saturation and low-loss soft magnetic composite material, comprising the following steps:

[0059] (1) In terms of mass percentage, the first powder includes 96.13% Fe, 2.42% Si, 1.26% Cr, 0.104% Al, 0.03% Mn, and inevitable components, and D50 is 16.51 μm. In terms of mass percentage, the second powder includes 49.1% Fe, 49.9% Ni, 0.35% Mn, C is 76 ppm, O is 2691 ppm, and inevitable components, and D50 is 0.95 μm.

[0060] The first powder and the second powder are placed in a stirring barrel at a mass ratio of 4:6, the rotation speed of the stirring barrel is set to 35 r / min, the stirring time is 10 min, and the mixture is evenly mixed to obtain a mixture.

[0061] (2) Weighing a resin according to 1.5% of the mass of the mixed material, dissolving it in an acetone solvent to obtain a uniformly mixed solution; adding the mixed material obtained in step (1) to the above solution, stirring, granulating, drying, and sieving to obtain a powder. The powder is heated to 1200 rpm under a pressure of 12 T / cm 2 The resin is pressed into a standard ring and placed in an oven at 200°C for 4 hours. The resin includes epoxy resin and polyvinyl butyral in a mass ratio of 4:1.

[0062] Example 2

[0063] This embodiment provides a method for preparing a high-saturation and low-loss soft magnetic composite material, comprising the following steps:

[0064] (1) In terms of mass percentage, the first powder includes 96.35% Fe, 2.29% Si, 1.24% Cr, 0.047% Al, 0.024% Mn, and inevitable components, and D50 is 14.67 μm. In terms of mass percentage, the second powder includes 48.7% Fe, 49.7% Ni, 0.44% Mn, 42 ppm C, 1895 ppm O, and inevitable components, and D50 is 1.02 μm.

[0065] The first powder and the second powder are placed in a stirring barrel at a mass ratio of 4:6, the rotation speed of the stirring barrel is set to 35 r / min, the stirring time is 10 min, and the mixture is evenly mixed to obtain a mixture.

[0066] (2) Weighing a resin according to 1.5% of the mass of the mixed material, dissolving it in an acetone solvent to obtain a uniformly mixed solution; adding the mixed material obtained in step (1) to the above solution, stirring, granulating, drying, and sieving to obtain a powder. The powder is heated to 1200 rpm under a pressure of 12 T / cm 2 The resin is pressed into a standard ring and placed in an oven at 200°C for 4 hours. The resin includes epoxy resin and polyvinyl butyral in a mass ratio of 4:1.

[0067] Example 3

[0068] This embodiment provides a method for preparing a high-saturation and low-loss soft magnetic composite material, comprising the following steps:

[0069] (1) In terms of mass percentage, the first powder includes 96.25% Fe, 2.37% Si, 1.23% Cr, 0.061% Al, 0.023% Mn, and inevitable components, and D50 is 16.45 μm. In terms of mass percentage, the second powder includes 49.2% Fe, 50.1% Ni, 0.38% Mn, C is 58 ppm, O is 2133 ppm, and inevitable components, and D50 is 1.08 μm.

[0070] The first powder and the second powder are placed in a stirring barrel at a mass ratio of 4:6, the rotation speed of the stirring barrel is set to 35 r / min, the stirring time is 10 min, and the mixture is evenly mixed to obtain a mixture.

[0071] (2) Weighing a resin according to 1.5% of the mass of the mixed material, dissolving it in an acetone solvent to obtain a uniformly mixed solution; adding the mixed material obtained in step (1) to the above solution, stirring, granulating, drying, and sieving to obtain a powder. The powder is heated to 1200 rpm under a pressure of 12 T / cm 2 The resin is pressed into a standard ring and placed in an oven at 200°C for 4 hours. The resin includes epoxy resin and polyvinyl butyral in a mass ratio of 4:1.

[0072] Example 4

[0073] This embodiment provides a method for preparing a high-saturation and low-loss soft magnetic composite material, comprising the following steps:

[0074] (1) In terms of mass percentage, the first powder includes 96.29% Fe, 2.34% Si, 1.24% Cr, 0.063% Al, 0.027% Mn, and inevitable components, and D50 is 11.5 μm. In terms of mass percentage, the second powder includes 49.5% Fe, 49.7% Ni, 0.39% Mn, C is 66 ppm, O is 2216 ppm, and inevitable components, and D50 is 1.8 μm.

[0075] The first powder and the second powder are placed in a stirring barrel at a mass ratio of 4:6, the rotation speed of the stirring barrel is set to 35 r / min, the stirring time is 10 min, and the mixture is evenly mixed to obtain a mixture.

[0076] (2) Weighing a resin according to 1.5% of the mass of the mixed material, dissolving it in an acetone solvent to obtain a uniformly mixed solution; adding the mixed material obtained in step (1) to the above solution, stirring, granulating, drying, and sieving to obtain a powder. The powder is heated to 150°C at a pressure of 150°C. 2The resin is pressed into a standard ring and placed in an oven at 190°C for heat treatment for 3 hours. The resin includes epoxy resin and polyvinyl butyral in a mass ratio of 4:1.

[0077] Example 5

[0078] This embodiment provides a method for preparing a high-saturation and low-loss soft magnetic composite material, comprising the following steps:

[0079] (1) In terms of mass percentage, the first powder includes 96.13% Fe, 2.42% Si, 1.26% Cr, 0.104% Al, 0.03% Mn, and inevitable components, and D50 is 16.51 μm. In terms of mass percentage, the second powder includes 49.1% Fe, 49.9% Ni, 0.35% Mn, C is 76 ppm, O is 2691 ppm, and inevitable components, and D50 is 0.95 μm.

[0080] The first powder and the second powder are placed in a stirring barrel at a mass ratio of 6.5:3.5, the rotation speed of the stirring barrel is set to 35 r / min, the stirring time is 10 min, and the mixture is evenly mixed to obtain a mixture.

[0081] (2) Weighing a resin according to 1.5% of the mass of the mixed material, dissolving it in an acetone solvent to obtain a uniformly mixed solution; adding the mixed material obtained in step (1) to the above solution, stirring, granulating, drying, and sieving to obtain a powder. The powder is heated to 1200 rpm under a pressure of 12 T / cm 2 The resin is pressed into a standard ring and placed in an oven at 200°C for 4 hours. The resin includes epoxy resin and polyvinyl butyral in a mass ratio of 4:1.

[0082] Example 6

[0083] This embodiment provides a method for preparing a high-saturation and low-loss soft magnetic composite material, comprising the following steps:

[0084] (1) In terms of mass percentage, the first powder includes 96.13% Fe, 2.42% Si, 1.26% Cr, 0.104% Al, 0.03% Mn, and inevitable components, and D50 is 25.2 μm. In terms of mass percentage, the second powder includes 49.1% Fe, 49.9% Ni, 0.35% Mn, C is 76 ppm, O is 2691 ppm, and inevitable components, and D50 is 5 μm.

[0085] The first powder and the second powder are placed in a stirring barrel at a mass ratio of 4:6, the rotation speed of the stirring barrel is set to 35 r / min, the stirring time is 10 min, and the mixture is evenly mixed to obtain a mixture.

[0086] (2) Weighing a resin according to 1.5% of the mass of the mixed material, dissolving it in an acetone solvent to obtain a uniformly mixed solution; adding the mixed material obtained in step (1) to the above solution, stirring, granulating, drying, and sieving to obtain a powder. The powder is heated to 1200 rpm under a pressure of 12 T / cm 2 The resin is pressed into a standard ring and placed in an oven at 200°C for 4 hours. The resin includes epoxy resin and polyvinyl butyral in a mass ratio of 4:1.

[0087] Comparative Example 1

[0088] This comparative example provides a method for preparing a soft magnetic composite material. The difference from Example 1 is that water vapor-atomized iron-silicon-chromium powder (manufacturer: Quanzhou Tianzhi) is used as a raw material instead of the first powder and the second powder, and its D50 is 14.5 μm. The preparation method comprises the following steps:

[0089] Weigh the resin according to 1.5% of the mass of the iron, silicon and chromium powder produced by water vapor atomization, dissolve it in acetone solvent to obtain a uniformly mixed solution; add the iron, silicon and chromium powder produced by water vapor atomization to the above solution, stir, granulate, dry and sieve to obtain powder. The powder is heated to 12T / cm 2 The resin is pressed into a standard ring and placed in an oven at 200°C for 4 hours. The resin includes epoxy resin and polyvinyl butyral in a mass ratio of 4:1.

[0090] Test example

[0091] This test example provides the properties of the materials prepared in each embodiment and comparative example, as follows:

[0092] Magnetic permeability test method: Take the standard ring (from each embodiment and comparative example) to measure the size, and wind it 20 turns of copper wire, test conditions 100kHz, 1V, test instrument HP4284 inductance tester, the measured inductance value is converted into magnetic permeability.

[0093] Magnetic field strength when inductance drops by 20%: The test conditions and test instruments are the same as the magnetic permeability, and current is gradually applied to test the inductance value after load until the inductance value is approximately equal to 80% of the initial inductance value. The current value at this time is recorded and converted into magnetic field strength.

[0094] The test method of magnetic loss Pv is: The copper wire is wound into two wire groups N1 and N2, N1 = 20Ts, N2 = 5Ts, the test conditions and results are shown in Table 1, the test equipment is SY8218 tester; where Ts represents the number of copper wire windings.

[0095] Table 1 Performance test results of various embodiments and comparative examples

[0096]

[0097] It can be seen from the above results that the soft magnetic composite material prepared by the present invention has the advantages of high saturation characteristics, low loss, etc., no cracking and other problems occur during the experiment, and the formability is good.

[0098] Furthermore, from Example 5, the loss of the soft magnetic composite material obtained by the mass ratio of the first powder to the second powder being 6.5:3.5 is higher than that of the material obtained by the mass ratio of the first powder to the second powder being 4:6 in Example 1, and the magnetic permeability and saturation inductance of Example 5 are also slightly worse than those of Example 1, which further indicates that using a specific ratio of the two powders helps to further improve the saturation characteristics of the soft magnetic composite material and reduce losses.

[0099] Furthermore, from Example 6, the particle sizes of the first powder and the second powder also have a certain influence on the saturation characteristics and losses of the material. From the results of Example 1 and Example 6, the first powder and the second powder in Example 1 adopt the specific particle size grading of the present invention to further improve the high saturation characteristics of the soft magnetic composite material and reduce the eddy current loss.

[0100] Example 1 is compared with Comparative Example 1. The iron-silicon-chromium powder that is jointly atomized by water vapor is used as the raw material. The loss of the soft magnetic material prepared according to the method of the present invention is about 3 times that of Example 1, and the saturation magnetic field intensity and magnetic permeability are both worse than those of the material of the present invention. This further illustrates that the use of powders of specific components in the present invention can make the soft magnetic composite material have both low loss and high saturation characteristics.

[0101] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a high saturation and low loss soft magnetic composite material, characterized in that: The following steps are involved: (1) mixing a first powder and a second powder to obtain a mixture; wherein the first powder comprises iron, silicon, and chromium, and the second powder comprises iron and nickel; (2) The mixed material is mixed with resin, pressed and heat treated; the temperature of the heat treatment is not higher than 220°C.

2. The preparation method according to claim 1, characterized in that: The D50 of the first powder is 10-20 μm, and the D50 of the second powder is 0.5-2 μm; and / or, The mass ratio of the first powder to the second powder is (3-7):(3-7).

3. The preparation method according to claim 1 or 2, characterized in that: In terms of mass percentage, the iron content in the first powder is 95-97%; and / or the silicon content in the first powder is 2.0-2.6%; and / or the chromium content in the first powder is 1.0-1.5%.

4. The preparation method according to claim 3, characterized in that: In terms of mass percentage, the first powder further comprises aluminum and / or manganese; In terms of mass percentage, the aluminum content in the first powder is 0.02-0.15%; In terms of mass percentage, the manganese content in the first powder is 0.01-0.05%.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In terms of mass percentage, the iron content in the second powder is 47-52%; and / or the nickel content in the second powder is 47-52%.

6. The preparation method according to claim 5, characterized in that: The second powder further comprises at least one of manganese, carbon and oxygen; Preferably, in terms of mass percentage, the manganese content in the second powder is less than 0.5%; Preferably, C<800ppm and O<8000ppm in the second powder.

7. The preparation method according to any one of claims 1 to 6, characterized in that: Satisfy at least one of (1) to (2): (1) the resin comprises at least two of epoxy resin, polyester resin, polyethylene glycol, polyvinyl butyral resin, micronized wax and phenolic resin; and / or, The resin includes epoxy resin and polyvinyl butyral resin; and / or, The resin is added in an amount of 1.2 to 1.8 wt % of the mixture; (2) The step (2), when the mixture is mixed with the resin, further comprises the step of adding a coupling agent; The coupling agent is added in an amount of 0.2-0.5 wt % of the mixture.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The pressing pressure is 12-15 T / cm 2 , and / or, The heat treatment time is 4 to 5 hours and / or, The temperature of the heat treatment is 180-220°C.

9. The high saturation and low loss soft magnetic composite material obtained by the preparation method according to any one of claims 1 to 8.

10. An inductor device, characterized in that: The invention comprises a high saturation and low loss soft magnetic composite material prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Composite powder, magnetic powder core for magnetic powder and preparation method thereof

    CN101118797A

  • Preparation method of core-shell soft magnetic composite

    CN108597717A

  • Mixed soft magnetic material and integrally molded inductor prepared thereby

    CN110310794A

  • Magnetic core material, and preparation method and application thereof

    CN112768166A

  • Preparation method of high-frequency wide-temperature low-coercivity iron-based soft magnetic composite material

    CN116598085A