Formation method of Nord flash memory device
By adding the second word line polysilicon on both sides of the word line polysilicon of the Nord flash memory device, the cross-sectional area of the cobalt silicide is expanded, the contact hole offset problem is solved, the risks of short circuit and leakage are reduced, and the reliability of the device is improved.
Patent Information
- Application Number
- CN202410949493.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
After the word line size is reduced, the contact holes of existing Nord flash memory devices are prone to deviate from cobalt silicide, resulting in increased risk of control gate short circuit and leakage, reducing device reliability.
The second word line polysilicon is formed on both sides of the word line polysilicon, increasing the size of the top surface of the word line and the cross-sectional area of the cobalt silicide, forming grooves through etching and oxidation treatment, filling the second word line polysilicon to expand the contact hole exposure Process window to reduce the chance of contact hole offset.
It effectively reduces the chance of word lines and control gate short circuits, reduces the risk of leakage, and improves the reliability of Nord flash memory devices.
Smart Images

Figure CN118899223A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for forming a Nord flash memory device. Background Art
[0002] Nord flash memory device formation method With the development of science and technology, the application of data storage media has shifted from some traditional non-volatile memories to flash memory. Large-capacity solid-state storage devices with flash memory as the main storage medium have become one of the mainstream solutions for data storage today.
[0003] Please refer to Figure 1 The prior art Nord flash memory device generally includes a word line 109 (Word Line, WL) and a gate oxide layer 102, a floating gate 103 (Floating Gate, FG), an interlayer dielectric layer 104 and a control gate 105 (Control Gate, CG) located on both sides of the word line 109 and stacked vertically on the substrate 101 in sequence, wherein a first sidewall 106 is formed on the control gate 105, a second sidewall 107 is formed between the control gate 105 and the word line 109, and a tunneling oxide layer 108 is formed between the floating gate 103 and the gate oxide layer 102 and the word line 109. Subsequently, the memory may also be interconnected with other interconnection layers as an interconnection layer, so a contact hole 112 is formed in the interlayer dielectric layer 111 between the interconnection layers, and one end of the contact hole 112 is connected to the word line 109, and the other end is connected to other interconnection layers. The method for forming the contact hole is to etch the interlayer dielectric layer 111 to form a through hole, and then fill the through hole with metal to form a through hole structure. Generally, in order to ensure that the thickness of the through holes of different depths meets the standard and has good contact with the bottom cobalt silicide, there must be a certain amount of over-etching during the interlayer dielectric etching process. The etching of the contact hole should eventually stop in the cobalt silicide layer 110 on the surface of the word line 109.
[0004] However, since the longitudinal cross-section of the word line in the prior art is wide at the top and narrow at the bottom. The material of word line 109 is polysilicon. After chemical mechanical polishing of the word line, there will be a step of ion implantation and dry oxygen oxidation on the surface of the word line polysilicon to form an oxide, which is used as a protective barrier layer for subsequent control gate and floating gate etching, resulting in the top of the word line polysilicon being consumed by oxidation and becoming shorter and narrower. Therefore, in fact, the width of the remaining word line 109 or the size of the top surface is smaller, and as the size of Nord flash memory devices becomes smaller and smaller, the height and width of word line 109 will be smaller. Since the width of word line 109 is very small, the width of cobalt silicide 110 will also be small. When a contact hole is formed on word line 109, the contact hole easily deviates from cobalt silicide 110 to the first sidewalls 106 on both sides. Since cobalt silicide does not grow on the surface of the first sidewall 106, it is very easy to etch through the first sidewall. For example, Figure 2 , Figure 2 It can be seen that the word line 109 is offset to the first sidewall and pierces the first sidewall, exposing the surface of the control gate 105 in the through hole, so the contact hole formed by filling the through hole with metal connects the control gate 105, resulting in a short circuit between the word line 109 and the control gate 105. This leads to the risk of leakage and reduces the reliability of the Nord flash memory device. Summary of the invention
[0005] The object of the present invention is to provide a method for forming a Nord flash memory device, which can increase the size of the top surface of the word line and the size of the cobalt silicide, reduce the probability of the contact hole of the word line offset to the control gate, thereby reducing the probability of short circuit between the word line and the control gate, reducing the risk of leakage, and improving the reliability of the Nord flash memory device.
[0006] In order to achieve the above object, the present invention provides a method for forming a Nord flash memory device, comprising:
[0007] Providing a substrate, and sequentially forming a floating gate layer, an interlayer dielectric layer, a control gate layer, and a hard mask layer on a surface of the substrate, wherein the hard mask layer has a first opening;
[0008] A first sidewall spacer, a second sidewall spacer and a tunneling oxide layer are formed in the first opening, wherein the first sidewall spacer covers the sidewall of the hard mask layer, the second sidewall spacer covers the first sidewall spacer, the sidewall of the control gate layer and the sidewall of the interlayer dielectric layer, the tunneling oxide layer covers the second sidewall spacer, the sidewall of the floating gate layer and the substrate surface, and the tunneling oxide layer forms a word line opening;
[0009] forming a first word line polysilicon in the word line opening, wherein a surface of the first word line polysilicon is lower than a top of the first spacer;
[0010] Etching a first spacer with a partial thickness to form a groove between the first word line polysilicon and the hard mask layer;
[0011] forming a second word line polysilicon on a surface of the first word line polysilicon layer, and the second word line polysilicon fills the groove;
[0012] Oxidizing the second polysilicon on the surface of the first word line polysilicon layer to form a layer of silicon oxide, and retaining the second word line polysilicon layer on the surface of the first sidewall;
[0013] removing the silicon oxide to expose the surface of the first word line polysilicon layer;
[0014] forming cobalt silicide on surfaces of the first wordline polysilicon layer and the second wordline polysilicon layer;
[0015] An interlayer dielectric layer and a through-hole structure located in the interlayer dielectric layer are formed on the surface of the cobalt silicide, and the through-hole structure is connected to the first word line polysilicon layer.
[0016] Optionally, in the method for forming the Nord flash memory device, the method further includes: forming a gate oxide layer on the surface of the substrate, wherein the gate oxide layer is located between the substrate and the floating gate layer.
[0017] Optionally, in the method for forming the Nord flash memory device, a method for forming a first word line polysilicon in the word line opening, wherein a surface of the first word line polysilicon is lower than a top of the first spacer includes:
[0018] The word line opening is filled with first word line polysilicon, the first word line polysilicon covers the surface of the hard mask layer, and the first word line polysilicon is ground to expose the surface of the hard mask layer, and at the same time, the surface of the first word line polysilicon is lower than the top of the first sidewall.
[0019] Optionally, in the method for forming the Nord flash memory device, a first sidewall spacer having a partial thickness is wet-etched to form a groove between the first word line polysilicon and the hard mask layer.
[0020] Optionally, in the method for forming the Nord flash memory device, HF or hot SC1 or BOE is used to wet-etch a portion of the thickness of the first sidewall spacer to form a groove between the first word line polysilicon and the hard mask layer.
[0021] Optionally, in the method for forming the Nord flash memory device, a method in which a second word line polysilicon is formed on a surface of the first word line polysilicon layer, and the second word line polysilicon fills the groove includes:
[0022] Depositing a second word line polysilicon on the surface of the first word line polysilicon, wherein the second word line polysilicon simultaneously fills the groove and covers the surface of the hard mask layer;
[0023] The second word line polysilicon is ground to remove the second word line polysilicon on the surface of the hard mask layer.
[0024] Optionally, in the method for forming the Nord flash memory device, an interlayer dielectric layer and a through-hole structure located in the interlayer dielectric layer are formed on the surface of the cobalt silicide, and a method for the through-hole structure to connect the first word line polysilicon layer includes:
[0025] forming an interlayer dielectric layer on the surface of the cobalt silicide;
[0026] Etching the interlayer dielectric layer to form a through hole in the interlayer dielectric layer, wherein the through hole exposes the surface of the cobalt silicide;
[0027] Filling metal into the through hole to form a through hole structure.
[0028] Optionally, in the method for forming the Nord flash memory device, the materials of the interlayer dielectric layer, the gate oxide layer, the tunneling oxide layer and the first sidewall spacer all include silicon oxide.
[0029] Optionally, in the method for forming the Nord flash memory device, the interlayer dielectric layer includes an ONO layer.
[0030] Optionally, in the method for forming the Nord flash memory device, the materials of the hard mask layer and the second sidewall spacer both include silicon nitride.
[0031] In the method for forming a Nord flash memory device provided by the present invention, a second word line polysilicon is added on both sides of the first word line polysilicon, so the size of the top surface of the word line is increased, thereby increasing the cross-sectional area of the cobalt silicide, increasing the process window of the contact hole exposure process, reducing the probability of the contact hole of the word line offsetting to the control gate, reducing the probability of short circuit between the word line and the control gate, reducing the risk of leakage, and improving the reliability of the Nord flash memory device. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a structural schematic diagram of a Nord flash memory device in the prior art;
[0033] Figure 2 is a schematic diagram of the structure of a Nord flash memory device in which a through hole in the prior art is offset to the first sidewall;
[0034] Figure 3 is a flow chart of a method for forming a Nord flash memory device according to an embodiment of the present invention;
[0035] Figure 4 is a schematic structural diagram of a Nord flash memory device after a word line opening is formed according to an embodiment of the present invention;
[0036] Figure 5 is a schematic structural diagram of a Nord flash memory device after forming first word line polysilicon according to an embodiment of the present invention;
[0037] Figure 6 is a schematic structural diagram of a Nord flash memory device after a groove is formed according to an embodiment of the present invention;
[0038] Figure 7 is a schematic structural diagram of a Nord flash memory device after forming second word line polysilicon according to an embodiment of the present invention;
[0039] Figure 8 is a schematic structural diagram of a Nord flash memory device after grinding the second word line polysilicon according to an embodiment of the present invention;
[0040] Fig. 9 is a schematic structural diagram of a Nord flash memory device after oxidizing the second word line polysilicon according to an embodiment of the present invention;
[0041] Fig.10 is a schematic structural diagram of a Nord flash memory device after word lines are formed according to an embodiment of the present invention;
[0042] Fig.11 is a schematic structural diagram of a Nord flash memory device after a contact hole is formed according to an embodiment of the present invention;
[0043] In the figure: 101-substrate, 102-gate oxide layer, 103-floating gate, 104-interlayer dielectric layer, 105-control gate, 106-first side wall, 107-second side wall, 108-tunneling oxide layer, 109-word line, 110-cobalt silicide, 111-interlayer dielectric layer, 112-contact hole, 201-substrate, 202-gate oxide layer, 203-floating gate, 204-interlayer dielectric layer, 205-control gate, 206-hard mask layer, 207-first side wall, 208-second side wall, 209-tunneling oxide layer, 210-first word line polysilicon, 211-second word line polysilicon, 212-silicon oxide, 213-cobalt silicide, 214-interlayer dielectric layer, 215-contact hole. DETAILED DESCRIPTION
[0044] The specific implementation of the present invention will be described in more detail below in conjunction with the schematic diagram. The advantages and features of the present invention will become clearer based on the following description. It should be noted that the drawings are all in a very simplified form and are not in exact proportions, and are only used to facilitate and clearly assist in explaining the purpose of the embodiments of the present invention.
[0045] Hereinafter, the terms "first", "second", etc. are used to distinguish between similar elements and are not necessarily used to describe a particular order or chronological sequence. It is to be understood that these terms used in this manner are interchangeable where appropriate. Similarly, if the method described herein includes a series of steps, the order of these steps presented herein is not necessarily the only order in which these steps can be performed, and some of the steps described may be omitted and / or some other steps not described herein may be added to the method.
[0046] Furthermore, it should be understood that when a layer (or film), region, pattern or structure is referred to as being "on" a substrate, layer (or film), region and / or pattern, it can be directly on another layer or substrate, and / or there can be intervening layers. In addition, it should be understood that when a layer is referred to as being "under" another layer, it can be directly under another layer, and / or there can be one or more intervening layers. In addition, references to being "on" and "under" each layer can be made based on the accompanying drawings.
[0047] Please refer to Figure 3 The present invention provides a method for forming a Nord flash memory device, comprising:
[0048] S11: providing a substrate, and sequentially forming a floating gate layer, an interlayer dielectric layer, a control gate layer, and a hard mask layer on a surface of the substrate, wherein the hard mask layer has a first opening;
[0049] S12: forming a first spacer, a second spacer and a tunneling oxide layer in the first opening, wherein the first spacer covers the sidewall of the hard mask layer, the second spacer covers the first spacer, the sidewall of the control gate layer and the sidewall of the interlayer dielectric layer, the tunneling oxide layer covers the second spacer, the sidewall of the floating gate layer and the substrate surface, and the tunneling oxide layer forms a word line opening;
[0050] S13: forming a first word line polysilicon in the word line opening, wherein a surface of the first word line polysilicon is lower than a top of the first spacer;
[0051] S14: etching a first spacer with a partial thickness to form a groove between the first word line polysilicon and the hard mask layer;
[0052] S15: forming a second word line polysilicon on the surface of the first word line polysilicon layer, and the second word line polysilicon fills the groove;
[0053] S16: oxidizing the second polysilicon on the surface of the first word line polysilicon layer to form a layer of silicon oxide, and retaining the second word line polysilicon layer on the surface of the first sidewall;
[0054] S17: removing silicon oxide to expose the surface of the first word line polysilicon layer;
[0055] S18: forming cobalt silicide on surfaces of the first word line polysilicon layer and the second word line polysilicon layer;
[0056] S19: forming an interlayer dielectric layer and a through-hole structure in the interlayer dielectric layer on the surface of the cobalt silicide, wherein the through-hole structure is connected to the first word line polysilicon layer.
[0057] First, please refer to Figure 4, a substrate 201 is provided, on which a gate oxide layer 202, a floating gate layer 203, an interlayer dielectric layer 204, a control gate layer 205 and a hard mask layer 206 are sequentially formed, and the hard mask layer 206 is subjected to photolithography and etching to pattern the hard mask layer 206, thereby forming a first opening (not shown in the figure), and the surface of the control gate layer 205 is exposed in the first opening. The interlayer dielectric layer 204 of the embodiment of the present invention can be an ONO stacked structure formed by stacking a silicon oxide layer, a silicon nitride layer and a silicon oxide layer. The gate oxide layer 202 can be silicon oxide, the floating gate layer 203 and the control gate layer 205 can be polysilicon, and the hard mask layer 206 can be silicon nitride. In other embodiments of the present invention, the specific materials of the above-mentioned film layers can be adjusted according to actual needs, and the present invention does not limit this.
[0058] Next, please continue to refer to Figure 4 , a first spacer 207 is formed in the first opening, and the process of forming the first spacer 207 includes: depositing a first spacer material layer (not shown in the figure) in the first opening, the first spacer material layer extending to cover the surface of the control gate layer 205; etching the first spacer material layer to form the first spacer 207 on the sidewall of the hard mask layer 206 in the first opening. The first spacer 207 can be silicon oxide. After the etching process, a wet cleaning process is also included to remove impurities and by-products in the previous etching process. The first spacer 207 is surrounded by a second opening, and a portion of the surface of the control gate layer 205 is exposed in the second opening. Then, the control gate layer 205 and the interlayer dielectric layer 204 exposed in the second opening are removed. Thus, a third opening is formed, and the third opening exposes the sidewalls of the control gate layer 205 and the sidewalls of the interlayer dielectric layer 204 and the surface of the floating gate layer 203. Specifically, the control gate layer 205 exposed in the second opening is first etched to expose the interlayer dielectric layer 204. Next, the interlayer dielectric layer 204 exposed in the second opening is continuously etched to expose the surface of the floating gate layer 203 . The interlayer dielectric layer 204 is an ONO layer, and the ONO layer can be removed by acid wet etching.
[0059] Next, a nitride is formed in the third opening. The nitride covers the sidewalls of the first spacer 207, the sidewalls of the control gate layer 205, and the sidewalls of the interlayer dielectric layer 204, and also covers a portion of the surface of the floating gate layer 203. The nitride forms a second spacer 208, and the second spacer 208 forms a fourth opening, and the fourth opening exposes the surface of the floating gate layer 203.
[0060] Next, the floating gate layer 203 exposed in the fourth opening is etched using the second sidewall 208 as a mask to expose the surface of the gate oxide layer 202 , and the gate oxide layer 202 is further etched to expose the surface of the substrate 201 , finally forming a fifth opening that exposes the surface of the substrate 201 .
[0061] Next, a tunneling oxide layer 209 is formed in the fifth opening. The oxide layer 209 may be silicon oxide. The oxide layer 209 forms a word line opening.
[0062] Next, please refer to Figure 5 , fill the word line opening with first word line polysilicon, the first word line polysilicon simultaneously covers the surface of the hard mask layer 206, grind the first word line polysilicon 210 to expose the surface of the hard mask layer 206, and then continue to grind the first word line polysilicon 210, so that the thickness of the first word line polysilicon 210 in the word line opening continues to decrease, thereby being lower than the top of the first sidewall 207, exposing a portion of the surface of the first sidewall 207, which is of course also lower than the surface of the hard mask layer 206.
[0063] Next, please refer to Figure 6 Partial thickness of the first spacer 207 on both sides of the polysilicon is etched to reduce the height of the first spacer 207. Thus, a groove is formed between the first word line polysilicon 210 and the hard mask layer 206. Specifically, a partial thickness of the first spacer is etched using a wet method such as HF or hot SC1 or BOE to form a groove between the first word line polysilicon 210 and the hard mask layer 206.
[0064] Next, please refer to Figure 7 , a second word line polysilicon 211 is continuously formed on the surface of the first word line polysilicon 210 and the surface of the hard mask layer 206 , and the second word line polysilicon 211 fills the groove at the same time.
[0065] Next, please refer to Figure 8 The second word line polysilicon 211 is ground to remove the second word line polysilicon 211 on the surface of the hard mask layer 206 , leaving the second word line polysilicon 211 in the middle of the hard mask layer 206 , that is, located on the surface of the first word line polysilicon and in the groove.
[0066] Next, please refer to Fig. 9, the second word line polysilicon 211 near the surface and the side will be dry oxidized into silicon oxide 212 for use as a barrier layer for etching the control gate and floating gate in the subsequent process, and then this layer of silicon oxide 212 will be cleaned and removed before forming cobalt silicide. Therefore, the silicon oxide 212 on the surface of the first word line polysilicon 210 is removed to expose the surface of the first word line polysilicon 210. At this time, preferably, the second word line polysilicon 211 on the surface of the first word line polysilicon 210 can be completely oxidized, so the thickness of the second word line polysilicon 211 retained on the surface of the first word line polysilicon 210 is the thickness of the word line polysilicon that can be dry oxidized, and the thickness of the silicon oxide 212 that is dry oxidized can be measured during actual production. After the silicon oxide 212 is subsequently cleaned off, the first word line polysilicon 210 has second word line polysilicon 211 on both sides. The first word line polysilicon 210 and the second word line polysilicon 211 on both sides serve as word lines. Compared with directly forming and grinding the first word line polysilicon 210 to form a word line, the width of the word line in the embodiment of the present invention is increased.
[0067] Next, please refer to Fig.10 , the hard mask layer 206, the control gate layer 205 located below the hard mask layer 206, the interlayer dielectric layer 204, the floating gate layer 203, and the gate oxide layer 202 are removed in sequence to expose the surface of the substrate 201. The remaining control gate layer 205 located below the first spacer 207 is used as a control gate, and the remaining floating gate layer 203 located below the second spacer and the interlayer dielectric layer 204 is used as a floating gate. Next, please refer to Fig.11 , a cobalt silicide 213 is formed on the surface of the word line, an interlayer dielectric layer 214 is formed on the surface of the cobalt silicide 213, and a contact hole 215 is formed in the interlayer dielectric layer 214. Since the size of the word line is increased, the size of the cobalt silicide 213 is increased, so the window for forming the contact hole 215 is increased. This prevents the contact hole 215 from being offset to the first sidewall 207.
[0068] In summary, in the method for forming a Nord flash memory device provided in an embodiment of the present invention, a second word line polysilicon is added on both sides of the first word line polysilicon, so that the size of the top surface of the word line is increased, thereby increasing the cross-sectional area of the cobalt silicide, increasing the process window of the contact hole exposure process, reducing the probability of the contact hole of the word line offset to the control gate, reducing the probability of short circuit between the word line and the control gate, reducing the risk of leakage, and improving the reliability of the Nord flash memory device.
[0069] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.
Claims
1. A method for forming a Nord flash memory device, characterized in that: include: Providing a substrate, and sequentially forming a floating gate layer, an interlayer dielectric layer, a control gate layer, and a hard mask layer on a surface of the substrate, wherein the hard mask layer has a first opening; A first sidewall spacer, a second sidewall spacer and a tunneling oxide layer are formed in the first opening, wherein the first sidewall spacer covers the sidewall of the hard mask layer, the second sidewall spacer covers the first sidewall spacer, the sidewall of the control gate layer and the sidewall of the interlayer dielectric layer, the tunneling oxide layer covers the second sidewall spacer, the sidewall of the floating gate layer and the substrate surface, and the tunneling oxide layer forms a word line opening; forming a first word line polysilicon in the word line opening, wherein a surface of the first word line polysilicon is lower than a top of the first spacer; Etching a first spacer with a partial thickness to form a groove between the first word line polysilicon and the hard mask layer; forming a second word line polysilicon on a surface of the first word line polysilicon layer, and the second word line polysilicon fills the groove; Oxidizing the second polysilicon on the surface of the first word line polysilicon layer to form a layer of silicon oxide, and retaining the second word line polysilicon layer on the surface of the first sidewall; removing the silicon oxide to expose the surface of the first word line polysilicon layer; forming cobalt silicide on surfaces of the first wordline polysilicon layer and the second wordline polysilicon layer; An interlayer dielectric layer and a through-hole structure located in the interlayer dielectric layer are formed on the surface of the cobalt silicide, and the through-hole structure is connected to the first word line polysilicon layer.
2. The method for forming a Nord flash memory device according to claim 1, wherein: Also includes: A gate oxide layer is formed on the surface of the substrate, and the gate oxide layer is located between the substrate and the floating gate layer.
3. The method for forming a Nord flash memory device according to claim 1, wherein: The method of forming a first word line polysilicon in the word line opening, wherein the surface of the first word line polysilicon is lower than the top of the first spacer, comprises: The word line opening is filled with first word line polysilicon, the first word line polysilicon covers the surface of the hard mask layer, and the first word line polysilicon is ground to expose the surface of the hard mask layer, and at the same time, the surface of the first word line polysilicon is lower than the top of the first sidewall.
4. The method for forming a Nord flash memory device according to claim 1, wherein: The first spacer is partially etched by wet etching to form a groove between the first word line polysilicon and the hard mask layer.
5. The method for forming a Nord flash memory device according to claim 4, wherein: HF or hot SC1 or BOE is used to wet-etch a portion of the thickness of the first spacer to form a groove between the first word line polysilicon and the hard mask layer.
6. The method for forming a Nord flash memory device according to claim 1, wherein: The method of forming a second word line polysilicon on the surface of the first word line polysilicon layer, and the second word line polysilicon filling the groove includes: Depositing a second word line polysilicon on the surface of the first word line polysilicon, wherein the second word line polysilicon simultaneously fills the groove and covers the surface of the hard mask layer; The second word line polysilicon is ground to remove the second word line polysilicon on the surface of the hard mask layer.
7. The method for forming a Nord flash memory device according to claim 1, wherein: A method for forming an interlayer dielectric layer and a through-hole structure in the interlayer dielectric layer on the surface of the cobalt silicide, wherein the through-hole structure is connected to the first word line polysilicon layer, comprises: forming an interlayer dielectric layer on the surface of the cobalt silicide; Etching the interlayer dielectric layer to form a through hole in the interlayer dielectric layer, wherein the through hole exposes the surface of the cobalt silicide; Filling metal into the through hole to form a through hole structure.
8. The method for forming a Nord flash memory device according to claim 1, wherein: The materials of the interlayer dielectric layer, the gate oxide layer, the tunneling oxide layer and the first sidewall spacer all include silicon oxide.
9. The method for forming a Nord flash memory device according to claim 1, wherein: The interlayer dielectric layer includes an ONO layer.
10. The method for forming a Nord flash memory device according to claim 1, wherein: The materials of the hard mask layer and the second spacer both include silicon nitride.