Negative pole piece for ultrafast-charging lithium ion battery as well as preparation method and application of negative pole piece

By adopting a composite structure of high-conductive agent and low-conductive agent in the negative electrode sheet of lithium-ion battery, combined with the distribution of small-particle graphite and large-particle graphite, the limitations of fast-charging batteries in charging capacity and energy density are solved. , achieving efficient rate charging and cycle performance improvement.

CN118899400APending Publication Date: 2024-11-05CHONGQING TALENT NEW ENERGY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410945453.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The negative electrode materials of existing fast-charging lithium-ion batteries have limitations in terms of charging capacity and energy density, and it is difficult to take into account both high energy density and large-scale fast charging capabilities.

Method used

A negative electrode sheet for ultrafast charging lithium-ion batteries was designed, using a composite structure of the inner layer and the outer layer, in which the inner layer has a high content of conductive agent, mixed with small particles of graphite, low content of conductive agent, mixed with large particles of conductive agent Graphite and amorphous carbon materials utilize nanostructures to improve charging capacity and cycling performance.

Benefits of technology

It improves the charging capacity and energy density of the negative electrode, is suitable for large-scale production, and significantly improves the rate charging and cycling performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899400A_ABST
    Figure CN118899400A_ABST
Patent Text Reader

Abstract

The invention provides a negative pole piece for an ultrafast charging lithium ion battery and a preparation method and application thereof, the negative pole piece comprises a negative current collector, at least one side surface of the negative current collector is provided with a composite negative active material layer, and the composite negative active material layer comprises a negative active material, a conductive agent and a binder; the composite negative electrode active material layer sequentially comprises an inner layer and an outer layer along the direction far away from the negative electrode current collector; the negative active material comprises graphite, and the particle size D50 of the graphite in the inner layer is smaller than the particle size D50 of the graphite in the outer layer; the content of the conductive agent in the inner layer is greater than the content of the conductive agent in the outer layer; and an amorphous carbon material is doped in the outer layer. The negative pole piece provided by the invention meets the requirement of high energy density on the basis of improving the charging capacity of the negative pole, is beneficial to the application of an ultrafast-charging lithium ion battery prepared on the basis of the negative pole piece in large-scale production, and has great production practice significance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and specifically relates to a negative electrode sheet for an ultra-fast charging lithium-ion battery, and a preparation method and application thereof. Background Art

[0002] In recent years, high-power charging technology has made major breakthroughs, and 800V high-voltage charging piles have been rapidly expanded. Judging from the strategic layout of new energy vehicle models of domestic and foreign OEMs, ultra-fast charging models will be facing large-scale applications in the next one or two years, which has promoted the development of fast charging cell technology. However, there are still certain technical barriers to be broken through in the research and development of main materials such as positive and negative electrode materials, electrolytes and diaphragms in the direction of fast charging, and the improvement of negative electrode charging capacity is currently the main factor restricting the development of fast charging cell technology. At present, the main technical route for fast charging graphite is small particle size, low OI value, hard carbon or conductive agent coating technology. The main technical route for silicon negative electrode developed for fast charging technology is porous hard carbon as the matrix, CVD vapor deposition, carbon coating, and reducing the size of nano-silicon grains. However, in order to better play the fast charging ability of negative electrode materials, it is necessary to match the best electrode formula, electrode structure and coating technology to enable the battery cell to achieve the best fast charging ability based on the application of the step fast charging strategy.

[0003] At present, fast-charge lithium-ion batteries mainly use double-layer coating technology to prepare layered gradient electrodes in terms of electrode structure design, including pore size gradient, porosity distribution gradient, active particle size gradient and active component gradient (formula), etc. The following technical solutions are mainly used for graphite negative electrode systems and graphite-doped silicon negative electrode systems:

[0004] 1) Graphite negative electrode system, the first coating layer, that is, the side close to the current collector is coated with small particles of graphite, and the second coating layer, that is, the side away from the current collector is coated with large particles of graphite. The preferred coating thickness ratio is 5:5. The formula of the electrode slurry of the first coating layer and the second coating layer mainly adopts the traditional main material + CMC + SBR + SP system. The gradient electrode structure prepared by this technical solution has a certain improvement in the battery's charging capacity, which can reach 5C, but the energy density improvement is limited;

[0005] 2) Graphite-doped silicon negative electrode system, the first coating layer, that is, the side close to the current collector is coated with small-particle graphite + high-silicon negative electrode, the second coating layer, that is, the side away from the current collector is coated with large-particle graphite + low-silicon negative electrode, the coating thickness ratio is preferably 5:5, and the formula of the first coating layer and the second coating layer electrode slurry mainly adopts the traditional main material + CMC + SBR + PAA + SP + CNT system. The gradient electrode structure prepared by this technical solution improves the energy density of the battery cell to a certain extent on the basis of improving the negative electrode charging capacity, but the charging capacity is limited.

[0006] Therefore, there is an urgent need to develop a negative electrode plate for ultra-fast charging lithium-ion batteries that can meet the requirements of both high energy density and high-rate fast charging capability. Summary of the invention

[0007] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a negative electrode plate for ultra-fast charging lithium-ion batteries and a preparation method and application thereof. In the negative electrode plate provided by the present invention, the inner layer close to the negative electrode current collector has a high content of conductive agent, and is mixed with small particles of graphite, which is beneficial to improving the charging capacity of the negative electrode; the outer layer has a low content of conductive agent, and is mixed with large particles of graphite, which is beneficial to electrolyte infiltration and improves the cycle performance. At the same time, the outer layer is also mixed with amorphous carbon materials, and its nanostructure provides a high surface area and a large pore volume. The higher surface area maximizes the lithium-philic surface, and the large pore volume provides sufficient space for the volume change of lithium, reduces the barrier for lithium ion embedding, and thus improves the charging capacity of the negative electrode. Therefore, the negative electrode plate not only improves the charging capacity of the negative electrode, but also takes into account the requirements of high energy density, which is beneficial to the application of ultra-fast charging lithium-ion batteries prepared based on this in large-scale production, and has great production practice significance.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a negative electrode plate for an ultra-fast charging lithium-ion battery, the negative electrode plate comprising a negative electrode current collector, a composite negative electrode active material layer being arranged on at least one side surface of the negative electrode current collector, the composite negative electrode active material layer comprising a negative electrode active material, a conductive agent and a binder; the composite negative electrode active material layer sequentially comprises an inner layer and an outer layer along a direction away from the negative electrode current collector;

[0010] The negative electrode active material includes graphite, and the graphite particle size D50 in the inner layer is smaller than the graphite particle size D50 in the outer layer;

[0011] The content of the conductive agent in the inner layer is greater than the content of the conductive agent in the outer layer;

[0012] The outer layer is doped with an amorphous carbon material.

[0013] In the negative electrode sheet provided by the present invention, the inner layer near the negative electrode current collector has a high content of conductive agent, and is mixed with small particles of graphite, which is conducive to improving the charging capacity of the negative electrode; the outer layer has a low content of conductive agent, and is mixed with large particles of graphite, which is conducive to electrolyte infiltration and improves the cycle performance. At the same time, the outer layer is also mixed with amorphous carbon materials, and its nanostructure provides a high surface area and a large pore volume. The high surface area maximizes the lithium-philic surface, and the large pore volume provides sufficient space for the volume change of lithium, reducing the barrier for lithium ion embedding, thereby improving the charging capacity of the negative electrode. Therefore, the negative electrode sheet not only improves the charging capacity of the negative electrode, but also takes into account the requirements of high energy density.

[0014] In the present invention, the inner layer close to the current collector has a high content of conductive agent and is mixed with small particles of graphite, which is beneficial to improving the charging capacity of the negative electrode; the outer layer has a low content of conductive agent and is mixed with large particles of graphite, which is beneficial to improving the cycle performance. At the same time, the outer layer is doped with amorphous carbon material, and its nanostructure provides a high surface area and a large pore volume. The higher surface area maximizes the lithium-philic surface. Therefore, the setting of the outer layer improves the energy density of the battery on the basis of improving the charging capacity of the negative electrode.

[0015] As a preferred technical solution of the present invention, the graphite particle size D50 in the inner layer is 10-13 μm, for example, 10 μm, 11 μm, 12 μm or 13 μm.

[0016] Preferably, the graphite particle size D50 in the outer layer is 14-16 μm, for example, 14 μm, 14.5 μm, 15 μm, 15.5 μm or 16 μm.

[0017] Preferably, the OI value of the graphite is 4-7, for example, 4, 4.58, 5, 5.5, 6, 6.5 or 7.

[0018] In the present invention, the OI value of graphite is 4-7, which helps to improve the isotropy of graphite and enhance the charging capacity of the negative electrode.

[0019] Preferably, the surface of the graphite is provided with a coating layer, and the coating layer is a hard carbon coating layer or a conductive agent coating layer.

[0020] In the present invention, a coating layer is provided on the surface of graphite, which helps to reduce the resistivity of the negative electrode graphite, reduce impedance, increase the lithium ion transmission rate, and enhance the charging capacity of the negative electrode.

[0021] Preferably, the conductive agent in the inner layer includes carbon nanotubes, conductive carbon black and artificial graphite, and the content of the carbon nanotubes is greater than the sum of the contents of the conductive carbon black and the artificial graphite.

[0022] In the present invention, the content of carbon nanotubes in the inner layer is greater than the sum of the contents of conductive carbon black and artificial graphite, which is beneficial to improving the charging capacity of the negative electrode.

[0023] The present invention does not limit the type of artificial graphite. For example, it may be KS-6. The conductive agent KS-6 can provide a long-distance electron transmission path, which is beneficial to improving the cycle performance.

[0024] Preferably, the conductive agent in the outer layer includes carbon nanotubes and conductive carbon black, and the content of the carbon nanotubes is less than the content of the conductive carbon black.

[0025] In the present invention, the content of carbon nanotubes (CNT) in the outer layer is less than that of conductive carbon black (SP), and CNT has higher conductivity and larger surface area, can reduce interface impedance, and increase the wettability of electrolyte; the SP in the outer layer provides optimal porosity, increases the stability of the electrode structure, and the design of porosity and conductivity jointly promotes better electrode performance, which is beneficial to improving rate charge and discharge and cycle performance.

[0026] Preferably, the binder content in the inner layer is greater than the binder content in the outer layer.

[0027] In the present invention, the content of the binder in the inner layer is greater than that in the outer layer, which can improve the charging capacity of the negative electrode.

[0028] Preferably, the binder in the inner layer comprises polyacrylic acid and / or styrene-butadiene rubber, preferably a combination of polyacrylic acid and styrene-butadiene rubber.

[0029] Preferably, in the inner layer, the content of the polyacrylic acid is less than the content of the styrene-butadiene rubber.

[0030] Preferably, the binder in the outer layer comprises polyacrylic acid and / or styrene-butadiene rubber, preferably a combination of polyacrylic acid and styrene-butadiene rubber;

[0031] Preferably, in the outer layer, the content of the polyacrylic acid is less than the content of the styrene-butadiene rubber.

[0032] Preferably, the amorphous carbon material includes hard carbon and / or soft carbon.

[0033] It should be noted that the soft carbon used in the present invention is composed of graphite-like and semi-graphite-like skeletons, and is a soft carbon with regular microcrystalline stacking and a high degree of crystallization.

[0034] Preferably, the doping amount of the amorphous carbon material is 5-12wt%, for example, it can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt% or 12wt%.

[0035] In the present invention, if the doping amount of the amorphous carbon material is too low, the interfacial impedance of the negative electrode increases, affecting the fast charging capability and cycle performance; if the doping amount of the amorphous carbon material is too high, the polarization changes and the cycle capacity decays too quickly.

[0036] Preferably, the particle size D50 of the hard carbon is 1 nm-8 μm, for example, 1 nm, 10 nm, 50 nm, 100 nm, 500 nm, 1 μm, 3 μm, 5 μm or 7 μm.

[0037] Preferably, the hard carbon is flower-like hard carbon.

[0038] In the present invention, the flower-like hard carbon has lithium affinity and nanostructure, which can provide a high surface area and a large pore volume, and is beneficial to reducing the damage of lithium deposition to the SEI film.

[0039] Preferably, the method for preparing the flower-like hard carbon comprises the following steps:

[0040] Acrylonitrile, acetone and azobisisobutyronitrile are mixed and cleaned with N2; then, the obtained solution is polymerized under the protection of an inert gas; the obtained product is vacuum dried and ground to obtain polyacrylonitrile powder; the polyacrylonitrile powder is heated in air for a period of time, and then the obtained stable polyacrylonitrile powder is carbonized in an inert atmosphere to obtain the flower-like hard carbon.

[0041] Preferably, the polymerization reaction temperature is 60-80°C, for example, 60°C, 70°C or 80°C.

[0042] Preferably, the heating temperature is 220-240° C., such as 220° C., 230° C. or 240° C., and the heating time is 1-3 h, such as 1 h, 2 h or 3 h.

[0043] Preferably, the carbonization temperature is greater than 1000° C., such as 1200° C., 1500° C. or 1800° C., and the carbonization time is 1-3 h, such as 1 h, 2 h or 3 h.

[0044] Preferably, the particle size D50 of the soft carbon is 6.5-10.5 μm, for example, 6.5 μm, 7.5 μm, 8.5 μm, 9.5 μm or 10.5 μm.

[0045] As a preferred technical solution of the present invention, the negative electrode active material also includes a silicon-based material.

[0046] Preferably, the silicon-based material includes silicon-carbon material and / or silicon-oxygen material.

[0047] Preferably, the silicon-carbon material is based on porous silicon-carbon and has a carbon layer as a coating layer of the base.

[0048] It should be noted that the carbon layer can be deposited by CVD vapor deposition method.

[0049] Preferably, the silicon-oxygen material is a pre-lithiated silicon-oxygen material.

[0050] Preferably, the surface of the silicon-oxygen material is sequentially coated with a carbon layer and a solid electrolyte layer along a direction away from the silicon-oxygen material.

[0051] Preferably, the particle size D50 of the silicon-based material is 2-12 μm, for example, 2 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm or 12 μm.

[0052] Preferably, the content of the silicon-based material in the inner layer is greater than the content of the silicon-based material in the outer layer.

[0053] In the present invention, the inner layer is high in silicon and the outer layer is low in silicon. The purpose of this setting is that high silicon requires more binder, but the multi-layer electrode structure is designed with a low binder content in the outer layer and a high binder content in the inner layer, which is beneficial to improving the bonding force between the active material and the current collector and improving the cycle performance.

[0054] Preferably, the content of the silicon-based material in the inner layer is 10-15wt%, for example, it may be 10wt%, 11wt%, 12wt%, 13wt%, 14wt% or 15wt%.

[0055] Preferably, the content of the silicon-based material in the outer layer is 3-10wt%, for example, 3wt%, 5wt%, 7wt% or 9wt%.

[0056] As a preferred technical solution of the present invention, an intermediate layer is further provided between the inner layer and the outer layer, and the porosities of the inner layer, the intermediate layer and the outer layer increase in sequence.

[0057] In the present invention, the porosity of the negative electrode active material layer increases successively along the direction away from the negative electrode current collector, which is conducive to the infiltration of the electrolyte. Moreover, the larger pore volume provides sufficient space for the volume change of lithium, reduces the barrier for lithium ion embedding, and thus improves the charging capacity of the negative electrode.

[0058] Preferably, the pore sizes of the inner layer, the middle layer and the outer layer increase sequentially.

[0059] In the present invention, the pore size of the negative electrode active material layer increases successively along the direction away from the negative electrode current collector, which is conducive to the infiltration of the electrolyte. Moreover, the larger pore volume provides sufficient space for the volume change of lithium, reduces the barrier for lithium ion embedding, and thus improves the charging capacity of the negative electrode.

[0060] Preferably, the thickness ratio of the inner layer, the middle layer and the outer layer is 5:(3-4):(1-2), wherein the selection range of the middle layer "3-4" can be, for example, 3, 3.5 or 4, and the selection range of the outer layer "1-2" can be, for example, 1, 1.5 or 2.

[0061] As a preferred technical solution of the present invention, the graphite particle size D50 in the intermediate layer is 14-16 μm, for example, 14 μm, 15 μm or 16 μm.

[0062] In the present invention, the middle layer containing large-particle graphite can improve the energy density of the battery while improving the negative electrode charging capacity.

[0063] Preferably, the negative electrode active material in the intermediate layer further comprises a silicon-based material, and the content of the silicon-based material is 3-10wt%, for example, 3wt%, 5wt%, 7wt% or 9wt%.

[0064] In a second aspect, the present invention provides a method for preparing a negative electrode sheet for an ultra-fast charging lithium-ion battery as described in the first aspect, the preparation method comprising the following steps:

[0065] Sequentially coating the inner layer and the outer layer on at least one side of the negative electrode current collector, and forming a composite negative electrode active material layer after drying to obtain the negative electrode sheet for the ultra-fast charging lithium-ion battery;

[0066] Among them, the composite negative electrode active material layer includes a negative electrode active material, a conductive agent and a binder, the negative electrode active material includes graphite, the graphite particle size D50 in the inner layer is smaller than the graphite particle size D50 in the outer layer, and the conductive agent content in the inner layer is greater than the conductive agent content in the outer layer.

[0067] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0068] (1) Graphite particles with a particle size D50 of 10-13 μm, a silicon-based material with a content of 10-15 wt%, carbon nanotubes with a content of 0.1-1.55 wt% (for example, 0.1 wt%, 0.5 wt%, 0.75 wt%, 1 wt% or 1.5 wt%, etc.), conductive carbon black with a content of 0.1-0.35 wt% (for example, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt% or 0.3 wt%, etc.), and a conductive carbon black with a content of 0.1-0.55 wt% (for example, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt% or 0.3 wt%, etc.) are prepared. t%, 0.2wt%, 0.3wt%, 0.4wt% or 0.5wt% (e.g., 0.5wt%, 1wt%, 1.5wt% or 1.8wt%) of artificial graphite, 0.5-1.85wt% (e.g., 0.5wt%, 1wt%, 1.5wt% or 1.8wt%) of polyacrylic acid, and 0.5-2.95wt% (e.g., 0.5wt%, 1wt%, 1.5wt%, 2wt% or 2.5wt%) of styrene-butadiene rubber to obtain a first slurry, and then coating the first slurry on at least one side of the negative electrode current collector to form an inner layer;

[0069] The content of carbon nanotubes is greater than the sum of the contents of conductive carbon black and artificial graphite, and the content of polyacrylic acid is less than that of styrene-butadiene rubber;

[0070] (2) graphite particles with a particle size D50 of 14-16 μm, silicon-based materials with a content of 3-10 wt% (for example, 3 wt%, 5 wt%, 7 wt%, 8 wt% or 10 wt%), carbon nanotubes with a content of 0.1-0.55 wt% (for example, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt% or 0.5 wt%), and carbon nanotubes with a content of 0.1-1.95 wt% (for example, 0.1 wt%, 0.5 wt%, 1 wt%, 1.5wt% or 1.9wt% (e.g., 0.5wt%, 1.5wt%, 2wt%, 2.2wt%, etc.) of conductive carbon black, 0.5-2.25wt% (e.g., 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.2wt%, etc.) of polyacrylic acid, and 0.5-2.25wt% (e.g., 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.2wt%, etc.) of styrene-butadiene rubber to obtain a second slurry, and then coating the second slurry on the surface of the inner layer to form an intermediate layer;

[0071] The content of carbon nanotubes is less than that of conductive carbon black, and the content of polyacrylic acid is less than that of styrene-butadiene rubber.

[0072] (3) graphite particles with a particle size D50 of 14-16 μm, a silicon-based material with a content of 3-10 wt% (for example, 3 wt%, 5 wt%, 7 wt%, 8 wt% or 10 wt%, etc.), an amorphous carbon material with a doping amount of 5-12 wt% (for example, 5 wt%, 7 wt%, 9 wt%, 10 wt% or 12 wt%, etc.), a carbon nanotube with a content of 0.1-0.35 wt% (for example, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt% or 0.3 wt%, etc.), and a carbon nanotube with a content of 0.1-2.1 5wt% (for example, 0.1wt%, 0.5wt%, 1wt%, 1.5wt% or 2wt%) of conductive carbon black, 0.5-2.65wt% (for example, 0.5wt%, 1wt%, 1.5wt%, 2wt% or 2.5wt%) of polyacrylic acid, and 0.5-2.15wt% (for example, 0.5wt%, 1wt%, 1.5wt%, 2wt% or 2.1wt%) of styrene-butadiene rubber to obtain a third slurry, and then coating the third slurry on the surface of the middle layer to form an outer layer;

[0073] Among them, the content of carbon nanotubes is less than that of conductive carbon black, and the content of polyacrylic acid is less than that of styrene-butadiene rubber.

[0074] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0075] (I) graphite particles with a particle size D50 of 10-13 μm, carbon nanotubes with a content of 0.1-1.55 wt% (for example, 0.1 wt%, 0.5 wt%, 0.75 wt%, 1 wt% or 1.5 wt%, etc.), conductive carbon black with a content of 0.1-0.35 wt% (for example, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt% or 0.3 wt%, etc.), and -0.55wt% (for example, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt% or 0.5wt%) of artificial graphite and 0.5-2.95wt% (for example, 0.5wt%, 1wt%, 1.5wt%, 2wt% or 2.5wt%) of styrene-butadiene rubber to obtain a first slurry, and then coating the first slurry on at least one side of the negative electrode current collector to form an inner layer;

[0076] Among them, the content of carbon nanotubes is greater than the sum of the contents of conductive carbon black and artificial graphite;

[0077] (II) mixing graphite particles having a particle size D50 of 14-16 μm, carbon nanotubes having a content of 0.1-0.55 wt% (for example, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt% or 0.5 wt%, etc.), conductive carbon black having a content of 0.1-1.95 wt% (for example, 0.1 wt%, 0.5 wt%, 1 wt%, 1.5 wt% or 1.9 wt%, etc.), and styrene-butadiene rubber having a content of 0.5-2.25 wt% (for example, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt% or 2.2 wt%, etc.) to obtain a second slurry, and then coating the second slurry on the surface of the inner layer to form an intermediate layer;

[0078] Wherein, the content of carbon nanotubes is less than that of conductive carbon black;

[0079] (III) mixing graphite particles having a particle size D50 of 14-16 μm, amorphous carbon material having a doping amount of 5-12 wt% (for example, 5 wt%, 7 wt%, 9 wt%, 10 wt% or 12 wt%, etc.), carbon nanotubes having a content of 0.1-0.35 wt% (for example, 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt% or 0.3 wt%, etc.), conductive carbon black having a content of 0.1-2.15 wt% (for example, 0.1 wt%, 0.5 wt%, 1 wt%, 1.5 wt% or 2 wt%, etc.) and styrene-butadiene rubber having a content of 0.5-2.15 wt% (for example, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt% or 2.1 wt%, etc.) to obtain a third slurry, and then coating the third slurry on the surface of the intermediate layer to form an outer layer;

[0080] The content of carbon nanotubes is less than that of conductive carbon black.

[0081] As a preferred technical solution of the present invention, the coating methods of the inner layer, the middle layer and the outer layer independently include any one of a blade coating method, an electrospinning method, an extrusion coating method, a spray sputtering method or a gravure printing method;

[0082] Preferably, among the coating methods of the inner layer, the middle layer and the outer layer, the coating methods of at least two layers are different.

[0083] In a third aspect, the present invention provides an ultra-fast charging lithium-ion battery, wherein the ultra-fast charging lithium-ion battery comprises the negative electrode plate for the ultra-fast charging lithium-ion battery as described in the first aspect.

[0084] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0085] Compared with the prior art, the present invention has the following beneficial effects:

[0086] In the negative electrode sheet provided by the present invention, the inner layer near the negative electrode current collector has a high content of conductive agent, and is mixed with small particles of graphite, which is conducive to improving the charging capacity of the negative electrode; the outer layer has a low content of conductive agent, and is mixed with large particles of graphite, which is conducive to electrolyte infiltration and improves the cycle performance. At the same time, the outer layer is also mixed with amorphous carbon materials, and its nanostructure provides a high surface area and a large pore volume. The high surface area maximizes the lithium-philic surface, and the large pore volume provides sufficient space for the volume change of lithium, reducing the barrier for lithium ion embedding, thereby improving the charging capacity of the negative electrode. Therefore, the negative electrode sheet not only improves the charging capacity of the negative electrode, but also takes into account the requirements of high energy density, which is conducive to the application of ultra-fast charging lithium-ion batteries prepared based on this in large-scale production, and has great production practical significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0087] Figure 1 This is a process flow chart for preparing a negative electrode sheet provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0088] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0089] Example 1

[0090] This embodiment provides a negative electrode plate for an ultra-fast charging lithium-ion battery, the negative electrode plate comprising a negative electrode current collector, a composite negative electrode active material layer is arranged on one side surface of the negative electrode current collector, the composite negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; the composite negative electrode active material layer comprises an inner layer, an intermediate layer and an outer layer in sequence along a direction away from the negative electrode current collector;

[0091] The negative electrode active material comprises graphite and a silicon-based material, the OI value of the graphite is 5.5, and a hard carbon coating layer is provided on the surface of the graphite;

[0092] The silicon-based material is a silicon-carbon material, the particle size D50 is 7 μm, the content of the silicon-based material in the inner layer is 12 wt%, the content of the silicon-based material in the middle layer is 5 wt%, and the content of the silicon-based material in the outer layer is 5 wt%;

[0093] The particle size D50 of the small-particle graphite in the inner layer is 12 μm, the particle size D50 of the large-particle graphite in the middle layer is 15 μm, and the particle size D50 of the large-particle graphite in the outer layer is 15 μm;

[0094] The conductive agent in the inner layer includes carbon nanotubes, conductive carbon black and artificial graphite KS-6, wherein the content of the carbon nanotubes is 0.8wt%, the content of the conductive carbon black is 0.15wt%, and the content of the artificial graphite KS-6 is 0.35wt%; the conductive agent in the middle layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.3wt%, and the content of the conductive carbon black is 0.9wt%; the conductive agent in the outer layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.1wt%, and the content of the conductive carbon black is 1.0wt%;

[0095] The binder in the inner layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.95wt%, and the content of the styrene-butadiene rubber is 1.15wt%; the binder in the middle layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.85wt%, and the content of the styrene-butadiene rubber is 0.95wt%; the binder in the outer layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.7wt%, and the content of the styrene-butadiene rubber is 0.8wt%;

[0096] The outer layer is doped with flower-shaped hard carbon, the particle size D50 is 3 μm, and the doping amount is 10 wt%;

[0097] The porosity of the inner layer, the middle layer and the outer layer increases successively, and the pore size of the inner layer, the middle layer and the outer layer increases successively;

[0098] The thickness ratio of the inner layer, the middle layer and the outer layer is 5:3.5:1.5.

[0099] This embodiment also provides a method for preparing the negative electrode sheet for the ultra-fast charging lithium-ion battery, and its process flow chart is as follows: Figure 1 As shown, the preparation method comprises the following steps:

[0100] (1) mixing small-particle graphite with a particle size D50 of 12 μm, a silicon-based material with a content of 12 wt%, carbon nanotubes with a content of 0.8 wt%, conductive carbon black with a content of 0.15 wt%, artificial graphite KS-6 with a content of 0.35 wt%, polyacrylic acid with a content of 0.95 wt%, styrene-butadiene rubber with a content of 1.15 wt%, and deionized water as a solvent to obtain a first slurry;

[0101] (2) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 0.3 wt% of carbon nanotubes, 0.9 wt% of conductive carbon black, 0.85 wt% of polyacrylic acid, 0.95 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a second slurry;

[0102] (3) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 10 wt% of flower-shaped hard carbon doped with carbon nanotubes, 0.1 wt% of conductive carbon black, 0.7 wt% of polyacrylic acid, 0.8 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a third slurry;

[0103] (4) A coating device with a double die head and a double gasket is used to coat the first slurry on one side of the negative electrode current collector copper foil, and an inner layer is formed after drying. Then, the second slurry is coated on the surface of the inner layer, and an intermediate layer is formed after drying. Subsequently, the third slurry is coated on the surface of the intermediate layer by electrospinning technology, and an outer layer is formed after drying. Thus, the negative electrode sheet for the ultra-fast charging lithium-ion battery can be obtained.

[0104] Example 2

[0105] This embodiment provides a negative electrode plate for an ultra-fast charging lithium-ion battery, the negative electrode plate comprising a negative electrode current collector, a composite negative electrode active material layer is arranged on one side surface of the negative electrode current collector, the composite negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; the composite negative electrode active material layer comprises an inner layer, an intermediate layer and an outer layer in sequence along a direction away from the negative electrode current collector;

[0106] The negative electrode active material comprises graphite and a silicon-based material, the OI value of the graphite is 5.5, and a hard carbon coating layer is provided on the surface of the graphite;

[0107] The silicon-based material is a pre-lithiated silicon-oxygen material, the particle size D50 is 7 μm, the content of the silicon-based material in the inner layer is 12 wt %, the content of the silicon-based material in the middle layer is 5 wt %, and the content of the silicon-based material in the outer layer is 5 wt %;

[0108] The particle size D50 of the small-particle graphite in the inner layer is 12 μm, the particle size D50 of the large-particle graphite in the middle layer is 15 μm, and the particle size D50 of the large-particle graphite in the outer layer is 15 μm;

[0109] The conductive agent in the inner layer includes carbon nanotubes, conductive carbon black and artificial graphite KS-6, wherein the content of the carbon nanotubes is 1.55wt%, the content of the conductive carbon black is 0.35wt%, and the content of the artificial graphite KS-6 is 0.55wt%; the conductive agent in the middle layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.55wt%, and the content of the conductive carbon black is 1.7wt%; the conductive agent in the outer layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.35wt%, and the content of the conductive carbon black is 1.5wt%;

[0110] The binder in the inner layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.95wt%, and the content of the styrene-butadiene rubber is 1.5wt%; the binder in the middle layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.85wt%, and the content of the styrene-butadiene rubber is 1.3wt%; the binder in the outer layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.65wt%, and the content of the styrene-butadiene rubber is 1.2wt%;

[0111] The outer layer is doped with flower-shaped hard carbon, the particle size D50 is 3 μm, and the doping amount is 10 wt%;

[0112] The porosity of the inner layer, the middle layer and the outer layer increases successively, and the pore size of the inner layer, the middle layer and the outer layer increases successively;

[0113] The thickness ratio of the inner layer, the middle layer and the outer layer is 5:3.5:1.5.

[0114] This embodiment also provides a method for preparing the negative electrode sheet for the ultra-fast charging lithium-ion battery, the preparation method comprising the following steps:

[0115] (1) mixing small-particle graphite with a particle size D50 of 12 μm, a silicon-based material with a content of 12 wt%, carbon nanotubes with a content of 1.55 wt%, conductive carbon black with a content of 0.35 wt%, artificial graphite KS-6 with a content of 0.55 wt%, polyacrylic acid with a content of 0.95 wt%, styrene-butadiene rubber with a content of 1.5 wt%, and deionized water as a solvent to obtain a first slurry;

[0116] (2) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 0.55 wt% of carbon nanotubes, 1.7 wt% of conductive carbon black, 0.85 wt% of polyacrylic acid, 1.3 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a second slurry;

[0117] (3) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 10 wt% of flower-shaped hard carbon doped with carbon nanotubes, 0.35 wt% of conductive carbon black, 0.65 wt% of polyacrylic acid, 1.2 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a third slurry;

[0118] (4) A coating device with a double die head and a double gasket is used to coat the first slurry on one side of the negative electrode current collector copper foil, and an inner layer is formed after drying. Then, the second slurry is coated on the surface of the inner layer, and an intermediate layer is formed after drying. Subsequently, the third slurry is coated on the surface of the intermediate layer by electrospinning technology, and an outer layer is formed after drying. Thus, the negative electrode sheet for the ultra-fast charging lithium-ion battery can be obtained.

[0119] Example 3

[0120] This embodiment provides a negative electrode plate for an ultra-fast charging lithium-ion battery, the negative electrode plate comprising a negative electrode current collector, a composite negative electrode active material layer is arranged on one side surface of the negative electrode current collector, the composite negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; the composite negative electrode active material layer comprises an inner layer, an intermediate layer and an outer layer in sequence along a direction away from the negative electrode current collector;

[0121] The negative electrode active material comprises graphite and a silicon-based material, the OI value of the graphite is 5.5, and a hard carbon coating layer is provided on the surface of the graphite;

[0122] The silicon-based material is a silicon-carbon material, the particle size D50 is 7 μm, the content of the silicon-based material in the inner layer is 12 wt%, the content of the silicon-based material in the middle layer is 5 wt%, and the content of the silicon-based material in the outer layer is 5 wt%;

[0123] The particle size D50 of the small-particle graphite in the inner layer is 12 μm, the particle size D50 of the large-particle graphite in the middle layer is 15 μm, and the particle size D50 of the large-particle graphite in the outer layer is 15 μm;

[0124] The conductive agent in the inner layer includes carbon nanotubes, conductive carbon black and artificial graphite KS-6, wherein the content of the carbon nanotubes is 1.55wt%, the content of the conductive carbon black is 0.35wt%, and the content of the artificial graphite KS-6 is 0.55wt%; the conductive agent in the middle layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.55wt%, and the content of the conductive carbon black is 1.7wt%; the conductive agent in the outer layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.35wt%, and the content of the conductive carbon black is 1.5wt%;

[0125] The binder in the inner layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.95wt%, and the content of the styrene-butadiene rubber is 1.5wt%; the binder in the middle layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.85wt%, and the content of the styrene-butadiene rubber is 1.3wt%; the binder in the outer layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.65wt%, and the content of the styrene-butadiene rubber is 1.2wt%;

[0126] The outer layer is doped with flower-shaped hard carbon, the particle size D50 is 3 μm, and the doping amount is 10 wt%;

[0127] The porosity of the inner layer, the middle layer and the outer layer increases successively, and the pore size of the inner layer, the middle layer and the outer layer increases successively;

[0128] The thickness ratio of the inner layer, the middle layer and the outer layer is 5:3.5:1.5.

[0129] This embodiment also provides a method for preparing the negative electrode sheet for the ultra-fast charging lithium-ion battery, the preparation method comprising the following steps:

[0130] (1) mixing small-particle graphite with a particle size D50 of 12 μm, a silicon-based material with a content of 12 wt%, carbon nanotubes with a content of 1.55 wt%, conductive carbon black with a content of 0.35 wt%, artificial graphite KS-6 with a content of 0.55 wt%, polyacrylic acid with a content of 0.95 wt%, styrene-butadiene rubber with a content of 1.5 wt%, and deionized water as a solvent to obtain a first slurry;

[0131] (2) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 0.55 wt% of carbon nanotubes, 1.7 wt% of conductive carbon black, 0.85 wt% of polyacrylic acid, 1.3 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a second slurry;

[0132] (3) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 10 wt% of flower-shaped hard carbon doped with carbon nanotubes, 0.35 wt% of conductive carbon black, 0.65 wt% of polyacrylic acid, 1.2 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a third slurry;

[0133] (4) A coating device with a double die head and a double gasket is used to coat the first slurry on one side of the negative electrode current collector copper foil, and an inner layer is formed after drying. Then, the second slurry is coated on the surface of the inner layer, and an intermediate layer is formed after drying. Subsequently, the third slurry is coated on the surface of the intermediate layer by electrospinning technology, and an outer layer is formed after drying. Thus, the negative electrode sheet for the ultra-fast charging lithium-ion battery can be obtained.

[0134] Example 4

[0135] This embodiment provides a negative electrode plate for an ultra-fast charging lithium-ion battery, the negative electrode plate comprising a negative electrode current collector, a composite negative electrode active material layer is arranged on one side surface of the negative electrode current collector, the composite negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; the composite negative electrode active material layer comprises an inner layer, an intermediate layer and an outer layer in sequence along a direction away from the negative electrode current collector;

[0136] The negative electrode active material comprises graphite and a silicon-based material, the OI value of the graphite is 5.5, and a hard carbon coating layer is provided on the surface of the graphite;

[0137] The silicon-based material is a silicon-carbon material, the particle size D50 is 2 μm, the content of the silicon-based material in the inner layer is 12 wt %, the content of the silicon-based material in the middle layer is 5 wt %, and the content of the silicon-based material in the outer layer is 5 wt %;

[0138] The particle size D50 of the small-particle graphite in the inner layer is 13 μm, the particle size D50 of the large-particle graphite in the middle layer is 16 μm, and the particle size D50 of the large-particle graphite in the outer layer is 16 μm;

[0139] The conductive agent in the inner layer includes carbon nanotubes, conductive carbon black and artificial graphite KS-6, wherein the content of the carbon nanotubes is 0.8wt%, the content of the conductive carbon black is 0.15wt%, and the content of the artificial graphite KS-6 is 0.35wt%; the conductive agent in the middle layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.3wt%, and the content of the conductive carbon black is 0.9wt%; the conductive agent in the outer layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.1wt%, and the content of the conductive carbon black is 1.0wt%;

[0140] The binder in the inner layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.95wt%, and the content of the styrene-butadiene rubber is 1.15wt%; the binder in the middle layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.85wt%, and the content of the styrene-butadiene rubber is 0.95wt%; the binder in the outer layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.7wt%, and the content of the styrene-butadiene rubber is 0.8wt%;

[0141] The outer layer is doped with flower-shaped hard carbon, the particle size D50 is 8 μm, and the doping amount is 10 wt%;

[0142] The porosity of the inner layer, the middle layer and the outer layer increases successively, and the pore size of the inner layer, the middle layer and the outer layer increases successively;

[0143] The thickness ratio of the inner layer, the middle layer and the outer layer is 5:3.5:1.5.

[0144] This embodiment also provides a method for preparing the negative electrode sheet for the ultra-fast charging lithium-ion battery, the preparation method comprising the following steps:

[0145] (1) mixing small-particle graphite with a particle size D50 of 13 μm, a silicon-based material with a content of 12 wt%, carbon nanotubes with a content of 0.8 wt%, conductive carbon black with a content of 0.15 wt%, artificial graphite KS-6 with a content of 0.35 wt%, polyacrylic acid with a content of 0.95 wt%, styrene-butadiene rubber with a content of 1.15 wt%, and deionized water as a solvent to obtain a first slurry;

[0146] (2) graphite particles with a particle size D50 of 16 μm, 5 wt% of silicon-based material, 0.3 wt% of carbon nanotubes, 0.9 wt% of conductive carbon black, 0.85 wt% of polyacrylic acid, 0.95 wt% of styrene-butadiene rubber, and deionized water as a solvent are stirred and mixed to obtain a second slurry;

[0147] (3) graphite particles with a particle size D50 of 16 μm, 5 wt% of silicon-based material, 10 wt% of flower-shaped hard carbon doped with carbon nanotubes, 0.1 wt% of conductive carbon black, 0.7 wt% of polyacrylic acid, 0.8 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a third slurry;

[0148] (4) A coating device with a double die head and a double gasket is used to coat the first slurry on one side of the negative electrode current collector copper foil, and an inner layer is formed after drying. Then, the second slurry is coated on the surface of the inner layer, and an intermediate layer is formed after drying. Subsequently, the third slurry is coated on the surface of the intermediate layer by electrospinning technology, and an outer layer is formed after drying. Thus, the negative electrode sheet for the ultra-fast charging lithium-ion battery can be obtained.

[0149] Example 5

[0150] This embodiment provides a negative electrode plate for an ultra-fast charging lithium-ion battery, the negative electrode plate comprising a negative electrode current collector, a composite negative electrode active material layer is arranged on one side surface of the negative electrode current collector, the composite negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; the composite negative electrode active material layer comprises an inner layer, an intermediate layer and an outer layer in sequence along a direction away from the negative electrode current collector;

[0151] The negative electrode active material comprises graphite and a silicon-based material, the OI value of the graphite is 5.5, and a hard carbon coating layer is provided on the surface of the graphite;

[0152] The silicon-based material is a silicon-carbon material, the particle size D50 is 12 μm, the content of the silicon-based material in the inner layer is 12 wt %, the content of the silicon-based material in the middle layer is 5 wt %, and the content of the silicon-based material in the outer layer is 5 wt %;

[0153] The particle size D50 of the small-particle graphite in the inner layer is 12 μm, the particle size D50 of the large-particle graphite in the middle layer is 15 μm, and the particle size D50 of the large-particle graphite in the outer layer is 15 μm;

[0154] The conductive agent in the inner layer includes carbon nanotubes, conductive carbon black and artificial graphite KS-6, wherein the content of the carbon nanotubes is 0.8wt%, the content of the conductive carbon black is 0.15wt%, and the content of the artificial graphite KS-6 is 0.35wt%; the conductive agent in the middle layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.3wt%, and the content of the conductive carbon black is 0.9wt%; the conductive agent in the outer layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.1wt%, and the content of the conductive carbon black is 1.0wt%;

[0155] The binder in the inner layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.95wt%, and the content of the styrene-butadiene rubber is 1.15wt%; the binder in the middle layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.85wt%, and the content of the styrene-butadiene rubber is 0.95wt%; the binder in the outer layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.7wt%, and the content of the styrene-butadiene rubber is 0.8wt%;

[0156] The outer layer is doped with flower-shaped hard carbon, the particle size D50 is 3 μm, and the doping amount is 10 wt%;

[0157] The porosity of the inner layer, the middle layer and the outer layer increases successively, and the pore size of the inner layer, the middle layer and the outer layer increases successively;

[0158] The thickness ratio of the inner layer, the middle layer and the outer layer is 5:3.5:1.5.

[0159] This embodiment also provides a method for preparing the negative electrode sheet for the ultra-fast charging lithium-ion battery, the preparation method comprising the following steps:

[0160] (1) mixing small-particle graphite with a particle size D50 of 12 μm, a silicon-based material with a content of 12 wt%, carbon nanotubes with a content of 0.8 wt%, conductive carbon black with a content of 0.15 wt%, artificial graphite KS-6 with a content of 0.35 wt%, polyacrylic acid with a content of 0.95 wt%, styrene-butadiene rubber with a content of 1.15 wt%, and deionized water as a solvent to obtain a first slurry;

[0161] (2) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 0.3 wt% of carbon nanotubes, 0.9 wt% of conductive carbon black, 0.85 wt% of polyacrylic acid, 0.95 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a second slurry;

[0162] (3) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 10 wt% of flower-shaped hard carbon doped with carbon nanotubes, 0.1 wt% of conductive carbon black, 0.7 wt% of polyacrylic acid, 0.8 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a third slurry;

[0163] (4) A coating device with a double die head and a double gasket is used to coat the first slurry on one side of the negative electrode current collector copper foil, and an inner layer is formed after drying. Then, the second slurry is coated on the surface of the inner layer, and an intermediate layer is formed after drying. Subsequently, the third slurry is coated on the surface of the intermediate layer by electrospinning technology, and an outer layer is formed after drying. Thus, the negative electrode sheet for the ultra-fast charging lithium-ion battery can be obtained.

[0164] Example 6

[0165] This embodiment provides a negative electrode plate for an ultra-fast charging lithium-ion battery, the negative electrode plate comprising a negative electrode current collector, a composite negative electrode active material layer is arranged on one side surface of the negative electrode current collector, the composite negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; the composite negative electrode active material layer comprises an inner layer and an outer layer in sequence along a direction away from the negative electrode current collector;

[0166] The negative electrode active material comprises graphite and a silicon-based material, the OI value of the graphite is 5.5, and a hard carbon coating layer is provided on the surface of the graphite;

[0167] The silicon-based material is a silicon-carbon material, the particle size D50 is 7 μm, the content of the silicon-based material in the inner layer is 12 wt%, and the content of the silicon-based material in the outer layer is 5 wt%;

[0168] The particle size D50 of the small-particle graphite in the inner layer is 12 μm, and the particle size D50 of the large-particle graphite in the outer layer is 15 μm;

[0169] The conductive agent in the inner layer includes carbon nanotubes, conductive carbon black and artificial graphite KS-6, wherein the content of the carbon nanotubes is 0.8wt%, the content of the conductive carbon black is 0.15wt%, and the content of the artificial graphite KS-6 is 0.35wt%; the conductive agent in the outer layer includes carbon nanotubes and conductive carbon black, wherein the content of the carbon nanotubes is 0.1wt%, and the content of the conductive carbon black is 1.0wt%;

[0170] The binder in the inner layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.95wt%, and the content of the styrene-butadiene rubber is 1.15wt%; the binder in the outer layer includes polyacrylic acid and styrene-butadiene rubber, the content of the polyacrylic acid is 0.7wt%, and the content of the styrene-butadiene rubber is 0.8wt%;

[0171] The outer layer is doped with flower-shaped hard carbon, the particle size D50 is 3 μm, and the doping amount is 10 wt%;

[0172] The porosity of the inner layer and the outer layer increases successively, and the pore size of the inner layer and the outer layer increases successively;

[0173] The thickness ratio of the inner layer, the middle layer and the outer layer is 8.5:1.5.

[0174] This embodiment also provides a method for preparing the negative electrode sheet for the ultra-fast charging lithium-ion battery, the preparation method comprising the following steps:

[0175] (1) mixing small-particle graphite with a particle size D50 of 12 μm, a silicon-based material with a content of 12 wt%, carbon nanotubes with a content of 0.8 wt%, conductive carbon black with a content of 0.15 wt%, artificial graphite KS-6 with a content of 0.35 wt%, polyacrylic acid with a content of 0.95 wt%, styrene-butadiene rubber with a content of 1.15 wt%, and deionized water as a solvent to obtain a first slurry;

[0176] (2) graphite particles with a particle size D50 of 15 μm, 5 wt% of silicon-based material, 10 wt% of flower-shaped hard carbon doped with carbon nanotubes, 0.1 wt% of conductive carbon black, 0.7 wt% of polyacrylic acid, 0.8 wt% of styrene-butadiene rubber and deionized water as a solvent are stirred and mixed to obtain a third slurry;

[0177] (3) A coating device with a double die head and a double gasket is used to coat the first slurry on one side of the negative electrode current collector copper foil, and after drying, an inner layer is formed. Then, the third slurry is coated on the surface of the inner layer by electrospinning technology, and after drying, an outer layer is formed, thereby obtaining the negative electrode sheet for the ultra-fast charging lithium-ion battery.

[0178] Example 7

[0179] The difference between this embodiment and embodiment 1 is that the coating method of the third slurry in step (4) is spraying or sputtering.

[0180] The rest of the preparation methods and parameters were the same as those in Example 1.

[0181] Example 8

[0182] The difference between this embodiment and embodiment 1 is that the coating method of the third slurry in step (4) is gravure printing.

[0183] The rest of the preparation methods and parameters were the same as those in Example 1.

[0184] Example 9

[0185] The difference between this embodiment and embodiment 1 is that in step (4), the coating method of the first slurry is blade coating, and the coating method of the second slurry and the third slurry is electrostatic spinning coating.

[0186] The rest of the preparation methods and parameters were the same as those in Example 1.

[0187] Example 10

[0188] The difference between this embodiment and embodiment 1 is that the contents of carbon nanotubes, conductive carbon black and artificial graphite KS-6 in the inner layer are all 0.8 wt %.

[0189] The rest of the preparation methods and parameters were the same as those in Example 1.

[0190] Embodiment 11

[0191] The difference between this embodiment and embodiment 1 is that in the inner layer, the content of polyacrylic acid and the content of styrene-butadiene rubber are both 0.95 wt %.

[0192] The rest of the preparation methods and parameters were the same as those in Example 1.

[0193] Example 12

[0194] The difference between this embodiment and embodiment 1 is that in the outer layer, the contents of carbon nanotubes and conductive carbon black are both 0.1 wt %.

[0195] The rest of the preparation methods and parameters were the same as those in Example 1.

[0196] Example 13

[0197] The difference between this embodiment and embodiment 1 is that in the outer layer, the content of polyacrylic acid and the content of styrene-butadiene rubber are both 0.7 wt %.

[0198] The rest of the preparation methods and parameters were the same as those in Example 1.

[0199] Embodiment 14

[0200] The difference between this embodiment and embodiment 1 is that the outer layer is not doped with flower-shaped hard carbon.

[0201] The rest of the preparation methods and parameters were the same as those in Example 1.

[0202] Comparative Example 1

[0203] The difference between this comparative example and Example 1 is that the first slurry is coated on the surface of the negative electrode current collector by using a single-layer extrusion coating device, that is, only the inner layer is coated on the surface of the negative electrode current collector.

[0204] The rest of the preparation methods and parameters were the same as those in Example 1.

[0205] Comparative Example 2

[0206] The difference between this comparative example and Example 1 is that the second slurry is coated on the surface of the negative electrode current collector by using a single-layer extrusion coating device, that is, only the middle layer is coated on the surface of the negative electrode current collector.

[0207] The rest of the preparation methods and parameters were the same as those in Example 1.

[0208] Comparative Example 3

[0209] The difference between this comparative example and Example 1 is that the third slurry is coated on the surface of the negative electrode current collector by using a single-layer extrusion coating device, that is, only an outer layer is coated on the surface of the negative electrode current collector.

[0210] The rest of the preparation methods and parameters were the same as those in Example 1.

[0211] Performance Testing

[0212] The super-fast charging lithium-ion battery prepared in the above embodiments and comparative examples was assembled with a negative electrode sheet and a positive electrode sheet (positive electrode ternary nickel cobalt manganese oxide lithium), a diaphragm (ceramic) and an electrolyte (NaPF6 / (EC+DEC) (volume ratio 1:1, concentration 1.1 mol / L)) to obtain a super-fast charging lithium-ion battery.

[0213] The rate performance and cycle performance of the ultra-fast charging lithium-ion battery were tested.

[0214] The test conditions of rate performance are: room temperature 25℃, 1C discharge to 2.7V, 4C CCCV constant current charge to 4.2V, and cut-off current 0.05C.

[0215] The test conditions for cycle performance are: room temperature 25°C, 500 cycles, 1C CCCV / 1C DC, 0-100% SOC, voltage range 2.7-4.2V; high temperature 45°C, 500 cycles, 1C CCCV / 1C DC, 0-100% SOC, voltage range 2.7-4.2V.

[0216] The test results are shown in Table 1.

[0217] Table 1

[0218]

[0219]

[0220] analyze:

[0221] It can be seen from the above table that the ultra-fast charging lithium-ion battery prepared based on the negative electrode plate provided by the present invention has significantly improved rate charging capability and cycle performance compared to conventional negative electrode coating technology.

[0222] It can be seen from Example 1 and Examples 10-11 that if the contents of carbon nanotubes, conductive carbon black and artificial graphite KS-6 in the inner layer are equal, it is not conducive to improving the rate and cycle performance; if the content of polyacrylic acid and styrene-butadiene rubber in the inner layer are equal, it is not conducive to improving the cycle performance.

[0223] It can be seen from Example 1 and Examples 12-13 that if the contents of carbon nanotubes and conductive carbon black in the outer layer are equal, it is not conducive to improving the rate and cycle performance; if the contents of polyacrylic acid and styrene-butadiene rubber in the outer layer are equal, it is not conducive to improving the cycle performance.

[0224] It can be seen from Example 1 and Example 14 that if the outer layer is not doped with flower-shaped hard carbon, the rate charging performance deteriorates and the cycle performance improves.

[0225] It can be seen from Example 1 and Comparative Example 1 that if only the inner layer is coated on the surface of the negative electrode current collector, the rate and cycle performance are better, but the energy density is low.

[0226] It can be seen from Example 1 and Comparative Example 2 that if only the intermediate layer is coated on the surface of the negative electrode current collector, the rate charging performance and the cycle performance will deteriorate, and the energy density will be low.

[0227] It can be seen from Example 1 and Comparative Example 3 that if only the outer layer is coated on the surface of the negative electrode current collector, the rate charging performance and the cycle performance will deteriorate, and the energy density will be low.

[0228] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A negative electrode sheet for ultra-fast charging lithium-ion batteries, It is characterized in that The negative electrode sheet comprises a negative electrode current collector, a composite negative electrode active material layer is arranged on at least one side surface of the negative electrode current collector, the composite negative electrode active material layer comprises a negative electrode active material, a conductive agent and a binder; the composite negative electrode active material layer comprises an inner layer and an outer layer in sequence along a direction away from the negative electrode current collector; The negative electrode active material includes graphite, and the graphite particle size D50 in the inner layer is smaller than the graphite particle size D50 in the outer layer; The content of the conductive agent in the inner layer is greater than the content of the conductive agent in the outer layer; The outer layer is doped with an amorphous carbon material.

2. The negative electrode sheet for ultra-fast charging lithium-ion battery according to claim 1, It is characterized in that The graphite particle size D50 in the inner layer is 10-13 μm; Preferably, the graphite particle size D50 in the outer layer is 14-16 μm; Preferably, the OI value of the graphite is 4-7; Preferably, the surface of the graphite is provided with a coating layer, and the coating layer is a hard carbon coating layer or a conductive agent coating layer; Preferably, the conductive agent in the inner layer includes carbon nanotubes, conductive carbon black and artificial graphite, and the content of the carbon nanotubes is greater than the sum of the contents of the conductive carbon black and the artificial graphite; Preferably, the conductive agent in the outer layer includes carbon nanotubes and conductive carbon black, and the content of the carbon nanotubes is less than the content of the conductive carbon black; Preferably, the binder content in the inner layer is greater than the binder content in the outer layer; Preferably, the binder in the inner layer comprises polyacrylic acid and / or styrene-butadiene rubber, preferably a combination of polyacrylic acid and styrene-butadiene rubber; Preferably, in the inner layer, the content of the polyacrylic acid is less than the content of the styrene-butadiene rubber; Preferably, the binder in the outer layer comprises polyacrylic acid and / or styrene-butadiene rubber, preferably a combination of polyacrylic acid and styrene-butadiene rubber; Preferably, in the outer layer, the content of the polyacrylic acid is less than the content of the styrene-butadiene rubber; Preferably, the amorphous carbon material comprises hard carbon and / or soft carbon; Preferably, the doping amount of the amorphous carbon material is 5-12wt%; Preferably, the particle size D50 of the hard carbon is 1 nm-8 μm; Preferably, the hard carbon is flower-shaped hard carbon; Preferably, the particle size D50 of the soft carbon is 6.5-10.5 μm.

3. The negative electrode sheet for ultra-fast charging lithium-ion battery according to claim 1 or 2, It is characterized in that The negative electrode active material also includes a silicon-based material; Preferably, the particle size D50 of the silicon-based material is 2-12 μm; Preferably, the content of silicon-based material in the inner layer is greater than the content of silicon-based material in the outer layer; Preferably, based on the mass of the inner layer, the content of the silicon-based material in the inner layer is 10-15wt%; Preferably, based on the mass of the outer layer, the content of the silicon-based material in the outer layer is 3-10 wt %.

4. The negative electrode sheet for ultra-fast charging lithium-ion battery according to any one of claims 1 to 3, It is characterized in that An intermediate layer is provided between the inner layer and the outer layer, and the porosity of the inner layer, the intermediate layer and the outer layer increases in sequence; Preferably, the pore sizes of the inner layer, the middle layer and the outer layer increase in sequence; Preferably, the thickness ratio of the inner layer, the middle layer and the outer layer is 5:(3-4):(1-2).

5. The negative electrode sheet for ultra-fast charging lithium-ion battery according to claim 4, It is characterized in that The graphite particle size D50 in the intermediate layer is 14-16 μm; Preferably, the negative electrode active material in the intermediate layer further comprises a silicon-based material, and the content of the silicon-based material is 3-10 wt %.

6. A method for preparing a negative electrode sheet for a super-fast charging lithium-ion battery according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: Sequentially coating the inner layer and the outer layer on at least one side of the negative electrode current collector, and forming a composite negative electrode active material layer after drying to obtain the negative electrode sheet for the ultra-fast charging lithium-ion battery; Among them, the composite negative electrode active material layer includes a negative electrode active material, a conductive agent and a binder, the negative electrode active material includes graphite, the graphite particle size D50 in the inner layer is smaller than the graphite particle size D50 in the outer layer, and the conductive agent content in the inner layer is greater than the conductive agent content in the outer layer.

7. The preparation method according to claim 6, It is characterized in that The preparation method comprises the following steps: (1) mixing graphite particles with a particle size D50 of 10-13 μm, a silicon-based material content of 10-15 wt%, carbon nanotubes with a content of 0.1-1.55 wt%, conductive carbon black with a content of 0.1-0.35 wt%, artificial graphite with a content of 0.1-0.55 wt%, polyacrylic acid with a content of 0.5-1.85 wt%, and styrene-butadiene rubber with a content of 0.5-2.95 wt% to obtain a first slurry, and then coating the first slurry on at least one side of the negative electrode current collector to form an inner layer; The content of carbon nanotubes is greater than the sum of the contents of conductive carbon black and artificial graphite, and the content of polyacrylic acid is less than that of styrene-butadiene rubber; (2) mixing graphite particles with a particle size D50 of 14-16 μm, 3-10 wt% of silicon-based material, 0.1-0.55 wt% of carbon nanotubes, 0.1-1.95 wt% of conductive carbon black, 0.5-2.25 wt% of polyacrylic acid, and 0.5-2.25 wt% of styrene-butadiene rubber to obtain a second slurry, and then coating the second slurry on the surface of the inner layer to form an intermediate layer; The content of carbon nanotubes is less than that of conductive carbon black, and the content of polyacrylic acid is less than that of styrene-butadiene rubber. (3) mixing graphite particles with a particle size D50 of 14-16 μm, a silicon-based material with a content of 3-10 wt%, an amorphous carbon material with a doping amount of 5-12 wt%, carbon nanotubes with a content of 0.1-0.35 wt%, conductive carbon black with a content of 0.1-2.15 wt%, polyacrylic acid with a content of 0.5-2.65 wt%, and styrene-butadiene rubber with a content of 0.5-2.15 wt% to obtain a third slurry, and then coating the third slurry on the surface of the middle layer to form an outer layer; Among them, the content of carbon nanotubes is less than that of conductive carbon black, and the content of polyacrylic acid is less than that of styrene-butadiene rubber.

8. The preparation method according to claim 6, It is characterized in that The preparation method comprises the following steps: (I) mixing graphite particles having a particle size D50 of 10-13 μm, carbon nanotubes having a content of 0.1-1.55 wt %, conductive carbon black having a content of 0.1-0.35 wt %, artificial graphite having a content of 0.1-0.55 wt %, and styrene-butadiene rubber having a content of 0.5-2.95 wt % to obtain a first slurry, and then coating the first slurry on at least one side of the negative electrode current collector to form an inner layer; Among them, the content of carbon nanotubes is greater than the sum of the contents of conductive carbon black and artificial graphite; (II) mixing graphite particles having a particle size D50 of 14-16 μm, carbon nanotubes having a content of 0.1-0.55 wt %, conductive carbon black having a content of 0.1-1.95 wt % and styrene-butadiene rubber having a content of 0.5-2.25 wt % to obtain a second slurry, and then coating the second slurry on the surface of the inner layer to form an intermediate layer; Wherein, the content of carbon nanotubes is less than that of conductive carbon black; (III) mixing graphite particles with a particle size D50 of 14-16 μm, amorphous carbon material with a doping amount of 5-12 wt%, carbon nanotubes with a content of 0.1-0.35 wt%, conductive carbon black with a content of 0.1-2.15 wt%, and styrene-butadiene rubber with a content of 0.5-2.15 wt% to obtain a third slurry, and then coating the third slurry on the surface of the intermediate layer to form an outer layer; The content of carbon nanotubes is less than that of conductive carbon black.

9. The preparation method according to claim 7 or 8, It is characterized in that The coating methods of the inner layer, the middle layer and the outer layer independently include any one of a blade coating method, an electrostatic spinning method, an extrusion coating method, a spray sputtering method or a gravure printing method; Preferably, among the coating methods of the inner layer, the middle layer and the outer layer, the coating methods of at least two layers are different.

10. An ultra-fast charging lithium-ion battery, It is characterized in that The ultra-fast charging lithium-ion battery comprises the negative electrode plate for an ultra-fast charging lithium-ion battery as claimed in any one of claims 1 to 5.

Citation Information

Cited By

  • Negative pole piece, battery monomer and secondary battery

    CN120600753A

  • Negative pole piece, preparation method thereof and lithium ion battery

    CN120955086A

  • Secondary battery and electronic device

    CN121506863A