Silicon-based composite material and preparation method thereof, negative pole piece, lithium ion battery and electric device

The Si/MXene composite material was prepared by gradient sintering, which solved the problem of volume expansion of silicon-based anode materials during charge and discharge, improved capacity and cycle performance, and enhanced electron transport and structural stability.

CN118899409APending Publication Date: 2024-11-05QUJING DYNANONIC CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410845481.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Silicon-based anode materials suffer from loss of active material and capacity decay due to volume expansion during charging and discharging, and their low electronic conductivity also affects their application.

Method used

Si/MXene composites were prepared by gradient sintering. By combining MXene with nano-silicon powder, MXene acts as a coating layer to mitigate volume changes and provides excellent electrical conductivity and mechanical robustness, promoting the formation of a uniform SEI layer.

Benefits of technology

It improves the capacity and cycle performance of silicon-based composite materials, enhances electron transport capability, stability and structural stability, and alleviates the volume expansion problem.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004916707150000151
    Figure BDA0004916707150000151
Patent Text Reader

Abstract

The invention discloses a silicon-based composite material and a preparation method thereof, a negative pole piece, a lithium ion battery and an electric device. The invention discloses a preparation method of a silicon-based composite material. The preparation method comprises the following steps: providing MXene; mixing materials containing the Mxene, the nano silicon powder and the solvent, drying, and grinding to obtain powder; carrying out gradient sintering on the powder in an inactive atmosphere to obtain a Si / MXene composite material; wherein Mxene comprises Ti < 3 > C < 2 > T < x >, and T < x > is at least one of-F,-O-and-OH. According to the embodiment of the invention, the problem of volume expansion of the silicon-based negative electrode material in the charging and discharging process can be relieved, so that the capacity and the cycle performance of the silicon negative electrode are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of negative electrode materials for lithium-ion batteries, and in particular relates to a silicon-based composite material and a preparation method thereof, a negative electrode sheet, a lithium-ion battery and an electrical device. Background Art

[0002] With the development of electric vehicles, people have put forward unprecedented requirements for long-cycle, high-energy-density lithium-ion batteries. At present, the mainstream negative electrode material on the market is graphite. This is because natural graphite resources are very abundant, and the layered structure of graphite provides an excellent environment for the intercalation and deintercalation of lithium ions. During the charge and discharge process, the working voltage of graphite is relatively stable, with a low lithium intercalation potential and excellent conductivity. However, graphite has poor solubility in the electrolyte. During the first charge and discharge process, the insertion compound formed by lithium and carbon is very unstable in the electrolyte and is easy to react with the electrolyte. A small part of the product dissolves in the electrolyte, while the other part forms an SEI film on the surface of the negative electrode and the electrolyte. In addition, due to the limitations of the crystal structure, lattice and unit cell parameters of graphite itself, the insertion of Li + The number of lithium ions is limited, which determines that the theoretical specific capacity of graphite negative electrode materials is only 372mAh / g. The theoretical specific capacity of silicon-based negative electrode materials is as high as 4200mAh / g, which is about 10 times that of graphite negative electrode materials. At the same time, it has a lower lithium insertion and extraction potential, which can avoid lithium precipitation on the surface during charging. It is considered to be the most promising negative electrode material for lithium-ion batteries after graphite negative electrodes.

[0003] However, during the charge and discharge process, when Li + When silicon-lithium alloy is formed by embedding in silicon-based negative electrode materials, a large volume expansion will occur. This large volume expansion / contraction will produce a large stress on the electrode surface, which will cause the active material particles to rupture and pulverize, resulting in the loss of active materials and rapid decay of battery capacity. Moreover, during the formation of the SEI film, the volume expansion of the silicon negative electrode will cause the SEI film to rupture and form a new SEI film, which will consume part of the active lithium ions and electrolyte, and increase the polarization and internal resistance of the battery. In addition, silicon has a relatively low electronic conductivity (≈10 - 3 S cm -1 ), which also greatly affects its application. Summary of the invention

[0004] The embodiments of the present application provide a silicon-based composite material and a preparation method thereof, a negative electrode plate, a lithium-ion battery and an electrical device, which can alleviate the volume expansion problem of silicon-based negative electrode materials during the charging and discharging process, thereby improving the capacity and cycle performance of the silicon negative electrode.

[0005] In a first aspect, the present invention provides a method for preparing a silicon-based composite material, comprising: providing MXene; mixing materials containing MXene, nano-silicon powder and a solvent, and grinding them after drying to obtain a powder; gradient sintering the powder in an inactive atmosphere to obtain a Si / MXene composite material; wherein MXene includes Ti 3 C 2 Tx, Tx is at least one of -F, -O- and -OH.

[0006] In any embodiment of the present application, the gradient sintering includes a first sintering and a second sintering; wherein, the temperature of the first sintering is 30 to 260°C, the time is 2 to 4 hours, and the heating rate is 4 to 6°C / min; the temperature of the second sintering is 260 to 600°C, the time is 2 to 4 hours, and the heating rate is 1 to 3°C / min.

[0007] In any embodiment of the present application, the particle size of the nano silicon powder is 50-100 nm.

[0008] In any embodiment of the present application, the mass ratio of Mxene to nano silicon powder is 1:1 to 1:3.

[0009] In any embodiment of the present application, Ti 3 C 2 The preparation method of Tx comprises: 3 AlC 2 The material of the etching solution is mixed, reacted at 25-30°C for 5-7h to obtain a product, and then washed and centrifuged repeatedly until the pH of the supernatant after centrifugation is 5-7, and then dried to obtain Ti 3 C 2 Tx; wherein the etching solution includes lithium fluoride and hydrochloric acid.

[0010] In any embodiment of the present application, Ti 3 AlC 2 The mass ratio of lithium fluoride to the volume ratio of the etching solution is 1g:15mL~1g:25mL; in the etching solution, the mass ratio of lithium fluoride to the volume ratio of hydrochloric acid is 1g:15mL~1g:25mL.

[0011] In a second aspect, an embodiment of the present application provides a silicon-based composite material, including Mxene and nano-silicon particles, wherein Mxene is a single-layer structure and covers the nano-silicon particles.

[0012] In a third aspect, an embodiment of the present application provides a negative electrode plate, which includes a negative electrode collector and a negative electrode film layer located on at least one surface of the negative electrode collector, and the negative electrode film layer includes the silicon-based composite material obtained by the above-mentioned preparation method or the above-mentioned silicon-based composite material.

[0013] In a fourth aspect, an embodiment of the present application provides a lithium-ion battery comprising the above-mentioned negative electrode plate.

[0014] In a fifth aspect, an embodiment of the present application provides an electrical device, comprising the above-mentioned lithium-ion battery, and at least one of a battery module and a battery pack assembled from the above-mentioned lithium-ion batteries, wherein the lithium-ion battery, the battery module, and the battery pack are used as a power source or energy storage unit for the electrical device.

[0015] The silicon-based composite material and its preparation method, negative electrode plate, lithium-ion battery and electrical device of the embodiment of the present application are compounded by MXene and nano-silicon powder, and the addition of MXene can greatly alleviate the volume change of silicon during the cycle, and has excellent conductivity, which can increase the electron transport in the composite material; at the same time, the active particles attached between the MXene sheets can prevent the stacking of MXene nanosheets, expose more reactive sites, and improve its cycle stability and rate performance while maintaining the high capacity of the active material, thereby improving the capacity and cycle performance of the silicon-based composite material as a negative electrode material. In addition, the MXene surface has abundant O- and F-containing groups, which will promote the formation of a uniform SEI layer, and MXene has excellent mechanical robustness and durability, ensuring the structural stability of the silicon-based composite material. DETAILED DESCRIPTION

[0016] In order to more clearly understand the above-mentioned purposes, features and advantages of the present application, the scheme of the present application will be further described below. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0017] In the following description, many specific details are set forth to facilitate a full understanding of the present disclosure, but the present application may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present application, rather than all of the embodiments.

[0018] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0019] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0020] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0021] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0022] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0023] Unless otherwise specified, this application adopts conventional test methods or test methods recommended by the instrument.

[0024] Preparation method of silicon-based composite material

[0025] A method for preparing a silicon-based composite material, comprising: S1, providing MXene; S2, mixing materials containing MXene, nano-silicon powder and a solvent, grinding them after drying to obtain a powder; S3, gradient sintering the powder in an inactive atmosphere to obtain a Si / MXene composite material; wherein MXene includes Ti 3 C 2 Tx, Tx is at least one of -F, -O- and -OH.

[0026] MXene is a two-dimensional material with a layered structure, consisting of transition metal carbides, nitrides or carbonitrides with a thickness of several atomic layers. n+1 X n T m Indicates: "M" represents metal elements, mainly transition metals (such as chromium, molybdenum, manganese, iron, cobalt, copper, aluminum, silver, nickel, palladium, platinum, ruthenium, etc.); "X" represents carbon and nitrogen elements; "T" represents the functional groups on the surface of the material, such as hydroxyl (-OH), halogen groups (-F, -Cl), etc. However, pure MXene is prone to collapse and stacking.

[0027] Ti 3 C 2 Tx is one of Mxene, wherein Tx represents a surface functional group, which may be at least one of -F, -O- and -OH.

[0028] Nano silicon powder refers to silicon particles with a particle size of 50 to 100 nm.

[0029] The solvent may be a solvent that does not chemically react with Mxene and nano silicon powder. The specific type of the solvent is not specifically limited, and those skilled in the art may adjust it as needed. As an example, the solvent may be water.

[0030] Inert atmosphere refers to a gas that does not or is difficult to react chemically, and can isolate the reaction system from the active gas (such as air) outside. The specific type of inert atmosphere is not specifically limited, and those skilled in the art can adjust it as needed. As an example, the inert atmosphere can be at least one of nitrogen, neon or argon.

[0031] Gradient sintering refers to a sintering process at at least two different temperatures. For example, sintering can be performed at a first temperature and then at a second temperature, with a gradient between the first temperature and the second temperature. The first temperature and the second temperature can also be independently subdivided into multiple different or identical temperature intervals. Sintering at multiple gradient temperatures can improve the composite effect of Si / MXene composite materials.

[0032] In the present application, in step S2, after liquid phase mixing for a certain period of time, grinding treatment is performed to modify MXene to obtain a single-layer structure of MXene to avoid collapse and stacking. After gradient sintering in step S3, MXene can be compounded with nano-silicon powder, and the introduction of MXene can greatly alleviate the volume change of silicon during the cycle, and has excellent conductivity, which can increase the electron transport in the composite material; at the same time, the active particles attached between the MXene sheets can prevent the stacking of MXene nanosheets, expose more reactive sites, and improve the cycle stability and rate performance while maintaining the high capacity of the active material, thereby improving the capacity and cycle performance of the silicon-based composite material as a negative electrode material. In addition, the surface of MXene is rich in O- and F-containing groups, which will promote the formation of a uniform SEI layer, and MXene has excellent mechanical robustness and durability, which ensures the structural stability of the silicon-based composite material.

[0033] In some embodiments, the gradient sintering includes a first sintering and a second sintering; wherein the temperature of the first sintering is 30-260°C, the time is 2-4h, and the heating rate is 4-6°C / min; the temperature of the second sintering is 260-600°C, the time is 2-4h, and the heating rate is 1-3°C / min. The first sintering can make the single layer of MXene better cover the nano-silicon, avoid the volume expansion of the nano-silicon, and better form the Si / MXene composite material. The second sintering can remove the oxide layer on the surface of the material, which is beneficial to improve the battery efficiency when it is used as a negative electrode material in the future.

[0034] Optionally, the temperature of the first sintering is independently selected from any value among 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C or any range between two thereof.

[0035] Optionally, the first sintering time is independently selected from any value among 2.0 h, 2.5 h, 3.0 h, 3.5 h, 4 h, or any range therebetween.

[0036] Optionally, the heating rate of the first sintering is independently selected from any value among 4.0℃ / min, 4.2℃ / min, 4.4℃ / min, 4.5℃ / min, 4.6℃ / min, 4.8℃ / min, 5.0℃ / min, 5.2℃ / min, 5.4℃ / min, 5.5℃ / min, 5.6℃ / min, 5.8℃ / min, 6.0℃ / min or any range between two of them.

[0037] Optionally, the second sintering temperature is independently selected from any value of 260°C, 280°C, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, or any range therebetween.

[0038] Optionally, the second sintering time is independently selected from any value among 2.0 h, 2.5 h, 3.0 h, 3.5 h, 4 h, or any range therebetween.

[0039] Optionally, the heating rate of the second sintering is independently selected from any value among 1.0℃ / min, 1.2℃ / min, 1.4℃ / min, 1.5℃ / min, 1.6℃ / min, 1.8℃ / min, 2.0℃ / min, 2.2℃ / min, 2.4℃ / min, 2.5℃ / min, 2.6℃ / min, 2.8℃ / min, 3.0℃ / min or any range between two of them.

[0040] In some embodiments, the particle size of the nano silicon powder is 50-100 nm. Optionally, the particle size of the nano silicon powder is independently selected from any value among 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, or any range between two values.

[0041] In some embodiments, the mass ratio of Mxene to nano-silicon powder is 1:1 to 1:3. Optionally, the mass ratio of Mxene to nano-silicon powder is independently selected from any value of 1:1.0, 1:1.2, 1:1.5, 1:1.8, 1:2.0, 1:2.2, 1:2.5, 1:2.8, 1:3.0 or any range between the two. Under the ratio in this range, Mxene can better cover the nano-silicon powder and avoid the volume expansion of the nano-silicon powder.

[0042] In some embodiments, Ti 3 C 2 The preparation method of Tx comprises: 3 AlC 2 The material of the etching solution is mixed, reacted at 25-30°C for 5-7h to obtain a product, and then washed and centrifuged repeatedly until the pH of the supernatant after centrifugation is 5-7, and then dried to obtain Ti 3 C 2 Tx; wherein the etching solution includes lithium fluoride and hydrochloric acid.

[0043] In the present application, Mxene is prepared by etching MAX phase (MAX phase is a type of nano-layered transition metal compound with a hexagonal lattice structure, and its molecular formula is Mn+1Axn, where M is generally a pre-transition metal, A is mainly a 13-15 main group element, X is carbon and / or nitrogen, and n is usually 1-3). For example, Ti is etched in a solution of lithium fluoride and hydrochloric acid at room temperature. 3 AlC 2 , which can selectively remove A atoms (Al) and introduce -F, -O- and -OH on the surface of the carbide layer.

[0044] In this application, after etching, Ti 3 C 2 Tx, and then repeat the washing and centrifugation until the pH of the supernatant after centrifugation is 5-7, which can ensure the formation of a composite material with uniform morphology in the subsequent sintering process and prevent the generation of dangerous gases during the sintering process to cause accidental injuries.

[0045] In some embodiments, Ti 3 AlC 2 The mass ratio of lithium fluoride to the volume ratio of the etching solution is 1g:15mL~1g:25mL; in the etching solution, the mass ratio of lithium fluoride to the volume ratio of hydrochloric acid is 1g:15mL~1g:25mL.

[0046] Silicon-based composite materials

[0047] A silicon-based composite material comprises Mxene and nano-silicon particles, wherein the Mxene is a single-layer structure and covers the nano-silicon particles.

[0048] Mxene coated nano-silicon particles can alleviate the volume expansion effect of silicon. The single-layer structure of Mxene is not easy to collapse and stack, and the adjustable space is Li + The migration of MXene provides ample space to guide the uniform deposition and growth of Li. Li is evenly distributed between ultra-thin layers, and the limited spacing of MXene effectively limits the growth of lithium dendrites, making dendrite-free lithium deposition possible.

[0049] Negative electrode

[0050] A negative electrode plate comprises a negative electrode current collector and a negative electrode film layer located on at least one surface of the negative electrode current collector, wherein the negative electrode film layer comprises the silicon-based composite material obtained by the above-mentioned preparation method or the above-mentioned silicon-based composite material.

[0051] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As examples of metal foils, copper foil, copper alloy foil, aluminum foil, and aluminum alloy foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0052] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. As an example, the negative electrode binder may include, but is not limited to, one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0053] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. As an example, the negative electrode conductive agent may include but is not limited to one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0054] In some embodiments, the negative electrode film layer may further include other additives. As an example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, and the like.

[0055] The negative electrode sheet can be prepared as follows: the negative electrode active material, the negative electrode binder, the negative electrode conductive agent, etc. are dispersed in a solvent and stirred to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing, etc., a negative electrode sheet is formed. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.

[0056] In some embodiments, the negative electrode plate may not include a negative electrode active material capable of deintercalating and extracting lithium ions. For example, the negative electrode plate may include a lithium plate or a lithium alloy plate; or, the negative electrode plate may include a mesh or foam three-dimensional skeleton layer; or, the negative electrode plate may include a negative electrode current collector and a lithium-containing layer disposed on at least one surface of the negative electrode current collector.

[0057] Lithium-ion battery

[0058] A lithium-ion battery comprises the above-mentioned negative electrode plate.

[0059] Typically, a lithium-ion battery includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator. The separator is arranged between the positive electrode sheet and the negative electrode sheet, and its main function is to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through.

[0060] The lithium-ion battery of the present application includes the silicon-based composite material of the embodiment of the present application or the silicon-based composite material prepared by the method of the embodiment of the present application. The Mxene-coated nano-silicon particles in the silicon-based composite material can alleviate the volume expansion problem of the silicon-based negative electrode material during the charging and discharging process, thereby improving the capacity and cycle performance of the silicon negative electrode.

[0061]

Positive electrode

[0062] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer located on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes an active material.

[0063] For example, the positive electrode current collector has two surfaces opposite to each other in the thickness direction thereof, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0064] In some embodiments, the positive electrode active material may be a conventional active material, for example, including a lithium transition metal oxide. Examples of lithium transition metal oxides may include one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. The modified compounds of the above-mentioned positive electrode active materials may be doping modification and / or surface coating modification of the positive electrode active material.

[0065] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application has no particular restrictions on the type of the positive electrode conductive agent. As an example, the positive electrode conductive agent includes at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene oxide, and carbon nanofibers. In some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the positive electrode conductive agent is ≤5%.

[0066] In some embodiments, the positive electrode film layer may also optionally include a positive electrode binder. The present application has no particular restrictions on the type of positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylic resin. In some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the positive electrode binder is ≤5%.

[0067] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base and a metal material layer formed on at least one surface of the polymer material base. As an example, the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0068] The positive electrode film layer is usually formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, optional conductive agent, optional binder and any other components in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto.

[0069]

Negative electrode

[0070] In some embodiments, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer located on at least one surface of the negative electrode current collector, and the negative electrode film layer includes a silicon-based composite material obtained by the preparation method in the embodiment of the present application or a silicon-based composite material in the embodiment of the present application.

[0071] In some embodiments, the negative electrode active material may also use materials known in the art. In some embodiments, as an example, the negative electrode active material may include, but is not limited to, one or more of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials may include, but are not limited to, one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys. Tin-based materials may include, but are not limited to, one or more of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0072] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As examples of metal foils, copper foil, copper alloy foil, aluminum foil, and aluminum alloy foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0073] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. As an example, the negative electrode binder may include, but is not limited to, one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0074] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. As an example, the negative electrode conductive agent may include but is not limited to one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0075] In some embodiments, the negative electrode film layer may further include other additives. As an example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, and the like.

[0076] The negative electrode sheet can be prepared as follows: the negative electrode active material, the negative electrode binder, the negative electrode conductive agent, etc. are dispersed in a solvent and stirred to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing, etc., a negative electrode sheet is formed. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.

[0077] In some embodiments, the negative electrode plate may not include a negative electrode active material capable of deintercalating and extracting lithium ions. For example, the negative electrode plate may include a lithium plate or a lithium alloy plate; or, the negative electrode plate may include a mesh or foam three-dimensional skeleton layer; or, the negative electrode plate may include a negative electrode current collector and a lithium-containing layer disposed on at least one surface of the negative electrode current collector.

[0078]

Electrolyte

[0079] During the charge and discharge process of lithium-ion batteries, active ions are embedded and released back and forth between the positive electrode and the negative electrode, and the electrolyte plays a role in conducting active ions between the positive electrode and the negative electrode. The present application has no particular restrictions on the type of electrolyte, which can be selected according to actual needs.

[0080] The electrolyte includes an electrolyte salt and a solvent. The types of the electrolyte salt and the solvent are not specifically limited and can be selected according to actual needs. As an example, the electrolyte salt may include but is not limited to lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium perchlorate (LiClO 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO 2 F 2 ), at least one of lithium difluorobis(oxalate)phosphate (LiDFOP) and lithium tetrafluorooxalate)phosphate (LiTFOP). As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0081] In some embodiments, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature power performance.

[0082] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be made into an electrode assembly by a winding process and / or a lamination process.

[0083] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0084] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT) and polybutylene succinate (PBS).

[0085] The preparation method of the lithium-ion battery of the present application is well known. In some embodiments, the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte can be assembled to form a secondary battery. As an example, the positive electrode sheet, the separator and the negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, and the electrolyte is injected after drying, and the lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping and other processes.

[0086] In some embodiments of the present application, the lithium-ion batteries according to the present application can be assembled into a battery module. The number of lithium-ion batteries contained in the battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.

[0087]

Isolation film

[0088] In some embodiments, the separator is disposed between the positive electrode and the negative electrode, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing lithium ions to pass through. The present application has no particular restrictions on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0089] In some embodiments, the material of the isolation membrane may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different.

[0090] Electrical devices

[0091] An electrical device, comprising the above-mentioned lithium-ion battery. The electrical device comprises at least one of the lithium-ion battery, battery module or battery pack of the present application. The lithium-ion battery, battery module or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0092] Example 1

[0093] 1. Ti 3 C2 Synthesis of Tx

[0094] 0.5 g Ti 3 AlC 2 The powder was slowly added to a mixture of 0.5 g lithium fluoride (LiF) and 10 mL 9 M hydrochloric acid (HCl) and stirred at 25 ° C for 24 h to remove the Al layer. The resulting product was then washed with deionized water, centrifuged at 4500 rpm for 5 min, and repeatedly centrifuged with deionized water until the pH value of the supernatant reached 6. Finally, the sample was vacuum dried at 60 ° C for 8 h to obtain MXene powder.

[0095] 2. Preparation of Si / MXene composites.

[0096] 0.3 g of MXene prepared in step (1) and 0.3 g of nano-silicon powder were added to 20 mL of deionized water, stirred at 25 ° C for 6 h, the mixed solution was centrifuged at 4500 rpm for 5 min, and the material was dried in an oven at 60 ° C to obtain a mixed material. The mixed material was ground to obtain a powdered material, and the material was sintered in a nitrogen atmosphere, wherein the sintering was divided into a first sintering stage and a second sintering stage; the first sintering stage was heated from room temperature (20-30 ° C) to 260 ° C at a heating rate of 5 ° C / min, and sintered for 3 h; the second sintering stage was heated from 260 ° C to 600 ° C at a heating rate of 2 ° C / min, and sintered for 3 h; then cooled to room temperature, and the Si / MXene composite material was obtained after cooling.

[0097] 3. Preparation of button cells

[0098] Si / MXene composite material, acetylene black and 2% sodium carboxymethyl cellulose (CMC, solvent is deionized water) aqueous solution were mixed in a mass ratio of 6:2:2, and stirred in a vacuum mixer for 3 hours to prepare the negative electrode slurry; the slurry was evenly coated on aluminum foil, and then placed in a vacuum drying oven at 120°C for 12 hours, and then punched into 14mm diameter discs as negative electrode sheets. The positive electrode sheet (metal lithium sheet with a diameter of 14.5mm), the negative electrode sheet, the separator (Celgard 2400 microporous polypropylene membrane) and the electrolyte (1mo1 / L LiPF 6 / EC+DMC (volume ratio 1:1)) were assembled into CR2025 button lithium-ion batteries in a glove box filled with argon. The electrochemical performance of the prepared batteries can be tested later.

[0099] Example 2

[0100] The experimental steps are basically the same as those in Example 1, except that 0.3 g MXene and 0.3 g nano-silicon powder in step (2) are replaced with 0.3 g MXene and 0.6 g nano-silicon powder.

[0101] Example 3

[0102] The experimental steps are basically the same as those in Example 1, except that 0.3 g MXene and 0.3 g nano-silicon powder in step (2) are replaced with 0.3 g MXene and 0.9 g nano-silicon powder.

[0103] Comparative Example 1

[0104] The experimental steps are basically the same as those in Example 1, except that the Si / MXene composite material in step (3) is replaced by graphite.

[0105] Comparative Example 2

[0106] The experimental steps are basically the same as those in Example 1, except that the Si / MXene composite material in step (3) is replaced by silicon powder.

[0107] Comparative Example 3

[0108] The experimental steps are basically the same as those in Example 1, except that the preparation of step (2) is different. Step (2) of this comparative example is as follows:

[0109] (2) Take 0.3 g of the MXene prepared in step (1), put it in an ultrasonic cleaner, disperse it at a power of 200 W, and after ultrasonication for 30 minutes, add 0.3 g of nano-scale silicon powder dropwise into the MXene suspension. After the addition is completed, the mixed suspension is ultrasonicated at a power of 200 W for 2 hours. Thereafter, the suspension is centrifuged at 10,000 rpm for 10 minutes and dried in a -80°C freeze dryer for 3 days to obtain a Si / MXene composite material.

[0110] Data testing and analysis:

[0111] Electrochemical tests were performed on the CR2025 button-type lithium-ion batteries in Examples 1-3 and Comparative Examples 1-2. The test results are shown in Table 1:

[0112] Table 1

[0113]

[0114] It can be seen from Table 1 that the 0.1C charge-discharge specific capacities of Examples 1-3 are 1299.6 / 1379.6 mAh·g -1 、1426.7 / 1498.6mAh·g -1 、1351.8 / 1421.5mAh·g -1, the coulombic efficiency is 94.3%, 95.2%, and 95.1%, respectively, and the 1C 100-cycle discharge capacity retention rate is 90.5%, 91.3%, and 90.9%, respectively. Compared with Comparative Example 1, the charge and discharge capacity is greatly improved. In terms of 1C 100-cycle discharge capacity retention rate, Examples 1-3 are improved by 80%, 80.8%, and 80.4%, respectively, compared with Comparative Example 2. It can be seen from Example 1 and Comparative Example 3 that gradient sintering will improve the electrochemical properties of Si / MXene composites.

[0115] The above is only a specific implementation of the present application. Those skilled in the art can clearly understand that for the convenience and simplicity of description, the specific working processes of the systems, modules and units described above can refer to the corresponding processes in the aforementioned method embodiments, and will not be repeated here. It should be understood that the protection scope of the present application is not limited to this. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in this application, and these modifications or replacements should be included in the protection scope of this application.

Claims

1. A method for preparing a silicon-based composite material, characterized in that: include: Providing MXene; Mixing the materials containing the Mxene, nano silicon powder and solvent, drying and then grinding to obtain a powder; The powder is subjected to gradient sintering in an inert atmosphere to obtain a Si / MXene composite material; Wherein, the Mxene includes Ti3C2Tx, and Tx is at least one of -F, -O- and -OH.

2. The preparation method according to claim 1, characterized in that The gradient sintering includes a first sintering and a second sintering; Wherein, the temperature of the first sintering is 30-260°C, the time is 2-4 hours, and the heating rate is 4-6°C / min; The second sintering temperature is 260-600° C., the time is 2-4 hours, and the heating rate is 1-3° C. / min.

3. The preparation method according to claim 1, characterized in that The particle size of the nano silicon powder is 50-100 nm.

4. The preparation method according to claim 1, characterized in that The mass ratio of the Mxene to the nano-silicon powder is 1:1 to 1:

3.

5. The preparation method according to claim 1, characterized in that The preparation method of Ti3C2Tx comprises: Mixing materials containing Ti3AlC2 and an etching solution, reacting at 25-30°C for 5-7 hours to obtain a product, and then repeatedly washing and centrifuging until the pH of the supernatant after centrifugation is 5-7, and then drying to obtain the Ti3C2Tx; Wherein, the etching solution includes lithium fluoride and hydrochloric acid.

6. The preparation method according to claim 5, characterized in that The mass ratio of the Ti3AlC2 to the etching solution is 1g:15mL to 1g:25mL; In the etching solution, the volume ratio of the lithium fluoride to the hydrochloric acid is 1 g:15 mL to 1 g:25 mL.

7. A silicon-based composite material, characterized in that: It comprises Mxene and nano-silicon particles, wherein the Mxene is a single-layer structure and covers the nano-silicon particles.

8. A negative electrode plate, characterized in that: The negative electrode plate includes a negative electrode current collector and a negative electrode film layer located on at least one surface of the negative electrode current collector, and the negative electrode film layer includes the silicon-based composite material obtained by the preparation method of any one of claims 1 to 6 or the silicon-based composite material according to claim 7.

9. A lithium-ion battery comprising the negative electrode sheet according to claim 8.

10. An electrical device comprising the lithium-ion battery according to claim 9, and at least one of a battery module and a battery pack assembled from the lithium-ion battery according to claim 9, wherein the lithium-ion battery, battery module, and battery pack are used as a power source or energy storage unit for the electrical device.

Citation Information

Cited By

  • Modified activated carbon, silicon-carbon composite material, preparation method of silicon-carbon composite material, pole piece, application and electrochemical device

    CN119503795A

  • Modified activated carbon, silicon-carbon composite material and preparation method thereof, electrode sheet, application and electrochemical device

    CN119503795B

  • Composite negative electrode material and preparation method thereof, negative electrode plate, battery and electronic device

    CN119812281A