Negative electrode material and preparation method thereof, electrochemical device and electronic device
By using carbon, oxygen, nitrogen and metallic coatings in lithium-ion batteries to coat graphite, the curvature carbon network structure is formed, and the problem of performance attenuation of lithium-ion batteries in low temperature environments is solved, and high energy is achieved Density and excellent low-temperature endurance.
Patent Information
- Application Number
- CN202410961451.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The performance attenuation and reduction of battery life of lithium-ion batteries in low-temperature environments makes it difficult for the prior art to improve the low-temperature performance and energy density at the same time.
Graphite is coated with a coating containing carbon, oxygen, nitrogen and metal elements (such as Zn, Co, Li, Zr or Al). The curvature carbon network structure is formed by cross-linking with graphite by bio-based polyamide and graphite, and lithium is enhanced. The attraction and electronic conductivity of ions improve the low-temperature performance and energy density of electrochemical devices.
It realizes the excellent performance and high energy density of lithium-ion batteries in low-temperature environments, and improves the low-temperature endurance and energy density of electrochemical devices.
Smart Images

Figure CN118899417A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of electrochemical energy storage, and in particular to a negative electrode material and a preparation method thereof, an electrochemical device using the negative electrode material, and an electronic device using the electrochemical device. Background Art
[0002] As a new type of high-energy green battery, lithium-ion batteries are widely used in laptops, mobile phones, new energy electric vehicles and other fields. However, the performance degradation and battery life reduction of lithium-ion batteries in low temperature environments limit the application of lithium-ion batteries. Therefore, it is crucial to improve the capacity and low-temperature battery life of lithium-ion batteries in low temperature environments.
[0003] The performance of lithium-ion batteries in low temperature environments is affected by the lithium ion transmission rate. By using amorphous carbon to coat graphite, such as asphalt or resin, the fast charging and low temperature performance of lithium-ion batteries can be improved, but a higher carbonization temperature is required, which also results in a loss of energy density, making it difficult to achieve the effect of improving both low temperature performance and energy density at the same time. Summary of the invention
[0004] The present application provides a negative electrode material and a preparation method thereof, an electrochemical device and an electronic device.
[0005] In a first aspect, the present application provides a negative electrode material, comprising graphite and a coating located on at least a portion of the surface of the graphite, wherein the coating contains carbon, oxygen, nitrogen and metal elements, and the metal element comprises at least one of Zn, Co, Li, Zr or Al.
[0006] In the present application, a negative electrode material is obtained by coating a metal-containing compound and a bio-based polyamide on the surface of graphite to form a partially carbonized carbon network doped with metals, and a coating containing carbon, nitrogen, oxygen and metal elements is formed on the surface of the graphite. Bio-based polyamide contains oxygen-containing five-membered rings and amide bonds. Oxygen-containing five-membered rings, amide bonds and metal elements also exist on the surface of graphite. The oxygen-containing five-membered rings are cross-linked with graphite to form a curvature carbon network structure (the oxygen-containing five-membered rings are cross-linked between the layers of graphite, and the oxygen-containing five-membered rings and the graphite layers are not in the same plane, which changes the curvature of the carbon network structure). The carbon network structure enhances the attraction to lithium ions, thereby inducing rapid desolvation of lithium ions and improving the low-temperature performance of the negative electrode material; the metal elements in the above-mentioned negative electrode material are doped in the curvature carbon network structure, which improves the electronic conductivity of the negative electrode material. At the same time, the amide bonds present in the coating are conducive to increasing the adsorption capacity of lithium ions, and are more conducive to increasing the capacity of the electrochemical device at room temperature, thereby improving the energy density of the electrochemical device, so that the electrochemical device has excellent low-temperature performance and a higher energy density.
[0007] Based on the first aspect, in some possible embodiments, based on the mass of the negative electrode material, the mass proportion of the metal element is 0.05% to 0.2%, which is beneficial to reducing the impedance of the electrochemical device and improving the conductivity of the negative electrode material, so as to further enable the electrochemical device to have excellent low temperature performance and energy density.
[0008] Based on the first aspect, in some possible embodiments, the coating contains at least one of the following structural fragments:
[0009]
[0010] The above structural fragments contain oxygen-containing five-membered rings, amide bonds, nitrogen-containing benzene rings or nitrogen-containing five-membered rings, wherein the above five-membered ring structures can be cross-linked between graphite layers, can change the curvature of the carbon network structure of graphite, and the carbon network structure can enhance the attraction to lithium ions, improve the desolvation ability, and improve the low-temperature performance of the electrochemical device; the amide bond can increase the adsorption capacity of lithium ions and increase the energy density of the electrochemical device; the nitrogen-containing benzene ring contained in the coating can improve the electronic conductivity and structural stability of the carbon network structure, which is beneficial to improving the low-temperature performance of the electrochemical device.
[0011] Based on the first aspect, in some possible embodiments, in an inert atmosphere, the weight loss rate of the negative electrode material when the temperature is increased from 35° C. to 800° C. is 0.15% to 0.3%. The weight loss rate of the negative electrode material is within a specific range, which corresponds to keeping the mass of the coating in the negative electrode material within a certain range, so that the negative electrode material contains a certain amount of coating, which is beneficial to improving the low temperature performance and energy density of the electrochemical device.
[0012] Based on the first aspect, in some possible embodiments, based on the mass of the negative electrode material, the mass proportion of nitrogen is 0.1% to 2%, which is beneficial to improving the electronic conductivity of the negative electrode material; and a certain amount of amide bonds may be contained on the surface of the negative electrode material to further improve the energy density and low temperature performance of the electrochemical device.
[0013] Based on the first aspect, in some possible implementations, based on the mass of the negative electrode material, the mass proportion of oxygen element is 0.1% to 3%, which can improve the stability of the negative electrode material, thereby facilitating the improvement of the cycle performance and energy density of the electrochemical device.
[0014] Based on the first aspect, in some possible embodiments, based on the mass of the negative electrode material, the mass of the carbon element accounts for 95% to 99%, which is beneficial to improve the conductivity and cycle performance of the negative electrode material and make the electrochemical device have a higher energy density.
[0015] Based on the first aspect, in some possible embodiments, the graphite includes at least one of artificial graphite or natural graphite. Artificial graphite and natural graphite can improve the lithium ion transport performance of the negative electrode material, so that the electrochemical device has a better charging performance and even a better low-temperature charging performance under the premise of having a higher energy density.
[0016] Based on the first aspect, in some possible embodiments, the graphitization degree of the negative electrode material is 94% to 98%, which can make the negative electrode material have a higher capacity and excellent kinetic performance, which is beneficial to improve the energy density of the electrochemical device; and the graphitization degree of the negative electrode material is within the above range, which can give full play to the performance of graphite.
[0017] Based on the first aspect, in some possible embodiments, the particle size Dv50 of the negative electrode material is 8 μm to 15 μm, which is beneficial to reduce the side reaction between the negative electrode material and the electrolyte, so that the electrochemical device has good low temperature performance and good energy density.
[0018] Based on the first aspect, in some possible embodiments, the tap density of the negative electrode material is 0.9 g / cm 3 Up to 1.1g / cm 3 The tap density within this range is beneficial to improving the energy density of the negative electrode material, and when the negative electrode material is used to prepare the slurry, it is also beneficial to reduce the amount of binder used and has good processing performance.
[0019] Based on the first aspect, in some possible embodiments, the specific surface area of the negative electrode material is 0.5 m 2 / g to 3m 2 / g, which is beneficial to reduce the side reactions between the negative electrode material and the electrolyte, so that the electrochemical device has good low-temperature performance and energy density.
[0020] The second aspect of the present application also provides a method for preparing a negative electrode material, wherein a biomass polyamide is dissolved in a solvent, and a metal-containing compound is added, and the mixture is stirred to obtain a coating slurry, wherein the residual carbon mass ratio of the biomass polyamide to the metal-containing compound at the same carbonization temperature is 1:(1-5), and the metal element in the metal-containing compound comprises at least one of Zn, Co, Li, Zr or Al;
[0021] Adding the coating slurry to the graphite and mixing them evenly to obtain an intermediate;
[0022] In an inert atmosphere, the intermediate is placed at a carbonization temperature of 400° C. to 800° C. for a carbonization time of 2 h to 5 h to obtain a negative electrode material.
[0023] In the above preparation method, the coating slurry is coated on graphite. After the above carbonization process, the coating slurry is evenly coated on the surface of the graphite. Part of the coating slurry is carbonized and forms a carbon network containing metal doping, and part of the coating slurry will remain on the surface of the graphite, so that the coating will contain oxygen-containing five-membered rings and amide bonds, so that the electrochemical device has good low-temperature performance and a higher energy density.
[0024] Based on the second aspect, in some possible embodiments, the biomass polyamide contains at least one of the following structural fragments:
[0025]
[0026] The degree of polymerization n of the structural fragment is 500 to 2000. The oxygen-containing five-membered ring structure contained in the structural fragment can cross-link with graphite, change the curvature of the carbon network structure of graphite, enhance the attraction to lithium ions, facilitate lithium ion desolvation, improve the low-temperature performance of the negative electrode material, and also facilitate the doping of metal elements in the oxygen-containing five-membered ring structure, improve the electronic conductivity of the negative electrode material, thereby improving the low-temperature performance and energy density of the electrochemical device.
[0027] Based on the second aspect, in some possible embodiments, the metal-containing compound is selected from at least one of the following compounds: C8H 10 N4Zn、C 24 H 12 O 13 Zn4, C4H6N2C o, Li3 P O4, LiF, C 48 H 24 O 32 Zr6、C 24 H 16 O 32 Zr6 or C 18 H 10 Al3O 17 The metal-containing compounds will partially remain on the surface of graphite during the carbonization process. The residues and the metal elements doped in the carbon network structure can not only improve the electronic conductivity of the negative electrode material, but the ligands in the metal-containing compounds are also conducive to promoting the desolvation ability of lithium ions and improving the low-temperature performance of the electrochemical device.
[0028] A third aspect of the present application provides an electrochemical device, including a negative electrode material, wherein the negative electrode material contains an oxygen-containing five-membered ring, an amide bond, and a metal element, so that the electrochemical device has excellent low-temperature performance and a high energy density.
[0029] A fourth aspect of the present application provides an electronic device, including an electrochemical device. The electronic device includes an electrochemical device, and the electrochemical device has excellent low-temperature performance and energy density, which is beneficial to improving the service life of the electronic device and the universality of low-temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0031] Figure 1 In the figure, (a) is a scanning electron microscope image of the negative electrode material in Example 1 of the present application; (b) is a local enlarged image of (a).
[0032] Figure 2 This is a charge and discharge curve diagram of the button cell co-embedded capacity test of the negative electrode materials in Example 1 and Comparative Example 1 of the present application.
[0033] Figure 3 This is a full battery 0 degree cycle capacity retention curve of the negative electrode materials in Example 1 and Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0034] The technical scheme in the embodiment of the present application is described clearly and in detail below. Obviously, the described embodiment is a part of the embodiment of the present application, rather than all the embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present application. The terms used in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application.
[0035] When an electrochemical device is charged, the solvated lithium ions in the electrolyte diffuse in the electrolyte liquid phase; after the lithium ions diffuse to the solid electrolyte membrane (SEI membrane) on the surface of the negative electrode, the outer solvation sheath is peeled off, commonly known as the desolvation process. The desolvated lithium ions diffuse through the SEI membrane to the negative electrode surface, and the lithium ions are embedded in the lattice of the negative electrode material. When the battery is discharged, similar microscopic steps occur on the positive electrode side. The slow desolvation process will produce severe electrochemical polarization when the battery is charged and discharged in a low temperature environment, causing the battery to quickly reach the cut-off voltage, thereby limiting the normal use of lithium-ion batteries under low temperature conditions.
[0036] The present application provides a negative electrode material and a preparation method thereof, an electrochemical device and an electronic device.
[0037] An embodiment of the present application provides an electrochemical device, which includes a housing, an electrode assembly and an electrolyte. The electrode assembly and the electrolyte are both located in the housing.
[0038] The shell can be a packaging bag encapsulated by a packaging film (such as an aluminum-plastic film), such as the electrochemical device is a soft-pack battery. In other embodiments, the electrochemical device can also be a steel shell battery, an aluminum shell battery, etc.
[0039] The electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet. The electrode assembly may be a laminated structure, which is formed by alternating the positive electrode sheet, the separator and the negative electrode sheet. In other embodiments, the electrode assembly may also be a wound structure, which is formed by stacking the positive electrode sheet, the separator and the negative electrode sheet and then winding them.
[0040] Negative electrode
[0041] The negative electrode sheet includes a negative electrode current collector and a negative electrode active layer disposed on the negative electrode current collector. The negative electrode current collector may be at least one of copper foil, nickel foil, stainless steel foil, titanium foil or carbon-based current collector, or may be any composite current collector disclosed in the prior art, such as but not limited to a current collector formed by combining the aforementioned conductive foil and a polymer substrate. The negative electrode active layer contains a negative electrode material.
[0042] The negative electrode material includes graphite and a coating located on at least a portion of the surface of the graphite, wherein the coating contains carbon, oxygen, nitrogen and metal elements, and the metal element includes at least one of Zn, Co, Li, Zr or Al.
[0043] The negative electrode material provided in the present application is obtained by coating a metal-containing compound and a bio-based polyamide on the surface of graphite to form a partially carbonized carbon network doped with metals. In the process of forming the carbon network, a coating containing carbon elements, nitrogen elements, oxygen elements and metal elements is formed on the surface of the graphite. Bio-based polyamide contains oxygen-containing five-membered rings and amide bonds. There are oxygen-containing five-membered rings, amide bonds and metal elements on the surface of graphite. The oxygen-containing five-membered rings are cross-linked with graphite to form a curvature carbon network structure (the oxygen-containing five-membered rings can be cross-linked between graphite layers, and the oxygen-containing five-membered rings and the graphite layers are not in the same plane, which changes the curvature of the carbon network structure). The carbon network structure enhances the attraction to lithium ions, thereby inducing rapid desolvation of lithium ions and improving the low-temperature performance of the negative electrode material; the metal elements in the above-mentioned negative electrode material are doped in the curvature carbon network structure, which improves the electronic conductivity of the negative electrode material. At the same time, the amide bonds present in the coating are conducive to improving the adsorption capacity of lithium ions, and are more conducive to improving the capacity of the electrochemical device at room temperature, thereby improving the energy density of the negative electrode material, so that the negative electrode material has excellent low-temperature performance and a high energy density.
[0044] In some embodiments, based on the mass of the negative electrode material, the mass proportion of the metal element is 0.05% to 0.2%. The content of the metal element affects the low temperature performance and energy density of the electrochemical device. The content of the metal element within the above range is conducive to reducing the impedance of the electrochemical device and improving the conductivity of the negative electrode material, so as to further enable the electrochemical device to have excellent low temperature performance and energy density. If the mass proportion of the metal element in the negative electrode material is large, the content of the metal element is high, and the metal element is easy to form an alloy with lithium ions, which increases the impedance of the electrochemical device, thereby affecting the low temperature performance and energy density of the electrochemical device; if the mass proportion of the metal element in the negative electrode material is small, the content of the metal element is low, and the effect of the metal element on the improvement of the low temperature performance and energy density of the electrochemical device is limited. In some embodiments, based on the mass of the negative electrode material, the mass proportion of the metal element can be 0.05%, 0.08%, 0.1%, 0.12%, 0.15%, 0.18%, 0.2% or any value within the range composed of any two of the above values.
[0045] In some embodiments, the coating contains at least one of the following structural fragments:
[0046] The above structural fragments contain oxygen-containing five-membered rings, amide bonds, nitrogen-containing benzene rings or nitrogen-containing five-membered rings, wherein the structure of the five-membered rings can be cross-linked between graphite layers, which can change the curvature of the carbon network structure of graphite. The carbon network structure will enhance the attraction to lithium ions, thereby improving the desolvation ability and the low-temperature performance of the electrochemical device; the amide bond can increase the adsorption capacity of lithium ions and increase the energy density of the electrochemical device; the nitrogen-containing benzene ring can improve the electronic conductivity and structural stability of the carbon network structure, which is beneficial to improving the low-temperature performance of the electrochemical device.
[0047] In some embodiments, in an inert atmosphere, the weight loss rate of the negative electrode material when the temperature is increased from 35°C to 800°C is 0.15% to 0.3%. In an inert atmosphere and at the above reaction temperature, the graphite in the negative electrode material does not react and produce losses, and its corresponding coating is pyrolyzed within the above temperature range, and some substances in the coating react. Within the above temperature range, the weight loss rate of the negative electrode material is within a specific range, which corresponds to keeping the mass of the coating in the negative electrode material within a certain range, so that the negative electrode material contains a certain amount of coating, which is beneficial to improve the low temperature performance and energy density of the electrochemical device. In some embodiments, the weight loss rate of the negative electrode material when the temperature is increased from 35°C to 800°C can be 0.15%, 0.18%, 0.2%, 0.23%, 0.25%, 0.27%, 0.3% or any value within the range composed of any two of the above values.
[0048] In some embodiments, the graphite includes at least one of artificial graphite and natural graphite. Artificial graphite and natural graphite can improve the lithium ion transport performance of the negative electrode material, so that the electrochemical device has a better charging performance and even a better low-temperature charging performance under the premise of having a higher energy density.
[0049] In some embodiments, based on the mass of the negative electrode material, the mass proportion of nitrogen is 0.1% to 2%. When the mass proportion of nitrogen is within the above range, on the one hand, the electronic conductivity can be improved through the nitrogen-doped carbon network structure, and on the other hand, a certain amount of amide bonds can be maintained on the surface of the negative electrode material to further improve the energy density and low temperature performance of the electrochemical device. In some embodiments, the mass proportion of nitrogen in the negative electrode material can be 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 1.3%, 1.5%, 1.8%, 2% or any value within the range formed by any two of the above values.
[0050] In some embodiments, based on the mass of the negative electrode material, the mass proportion of carbon element is 95% to 99%. The carbon content is within a specific range, which is beneficial to improve the conductivity and cycle performance of the negative electrode material and make the electrochemical device have a higher energy density. In some embodiments, based on the mass of the negative electrode material, the mass proportion of carbon element can be 95%, 96%, 97%, 98%, 99% or any value within the range formed by any two of the above values.
[0051] In some embodiments, based on the mass of the negative electrode material, the mass proportion of oxygen element is 0.1% to 3%, which can improve the stability of the negative electrode material, so as to improve the cycle performance and energy density of the electrochemical device. In some embodiments, based on the mass of the negative electrode material, the mass proportion of oxygen element can be 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 2.7%, 3% or any value within the range of any two of the above values.
[0052] In some embodiments, the degree of graphitization of the negative electrode material is 94% to 98%. The degree of graphitization of the negative electrode material within the above range can make the negative electrode material have a higher capacity and excellent kinetic performance, which is beneficial to improve the energy density of the electrochemical device; and the degree of graphitization of the negative electrode material within the above range can give full play to the performance of graphite. In some embodiments, the degree of graphitization of the negative electrode material can be 94%, 94.5%, 95%, 95.5%, 96%, 96.5%, 97%, 97.5%, 98% or any value within the range formed by any two of the above values.
[0053] In some embodiments, the particle size Dv50 of the negative electrode material is 8 μm to 15 μm. The particle size Dv50 of the negative electrode material within the above range is beneficial to reduce the side reaction between the negative electrode material and the electrolyte, so as to facilitate the electrochemical device to have good low temperature performance and energy density. V 50 is also called "median particle size", which means that in the particle size distribution of the negative electrode material particles, the particle size measured from the small particle size reaches 50% of the cumulative volume, that is, the volume of the negative electrode material particles smaller than this particle size accounts for 50% of the total volume of the negative electrode material particles. In some embodiments, the particle size Dv50 of the negative electrode material can be 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, or any value within the range formed by any two of the above values.
[0054] In some embodiments, the tap density of the negative electrode material is 0.9 g / cm 3 Up to 1.1g / cm 3 The tap density within this range is conducive to improving the energy density of the negative electrode material, and when the negative electrode material is used to prepare the slurry, it is also conducive to reducing the amount of binder used, and the processing performance is good. In some embodiments, the tap density of the negative electrode material can be 0.9 g / cm 3 , 0.95g / cm 3 、0.98g / cm 3 , 1g / cm 3 , 1.05g / cm 3 , 1.1g / cm 3 Or any value within the range formed by any two of the above values.
[0055] In some embodiments, the specific surface area of the negative electrode material is 0.5 m 2 / g to 3m 2 / g, the specific surface area of the negative electrode material is within the above range, which is conducive to reducing the side reaction between the negative electrode material and the electrolyte, so that the electrochemical device has good low temperature performance and energy density. In some embodiments, the specific surface area of the negative electrode material can be 0.5m 2 / g, 0.8m 2 / g, 1m 2 / g, 1.2m 2 / g, 1.5m 2 / g, 2m 2 / g, 2.5m 2 / g, 3m 2 / g or any value within the range formed by any two of the above values.
[0056] The present application also provides a method for preparing a negative electrode material, comprising:
[0057] (1) Dissolving biomass polyamide in a solvent, adding a metal-containing compound, and stirring to obtain a coated slurry, wherein the residual carbon mass ratio of the biomass polyamide and the metal-containing compound at the same carbonization temperature is 1:(1-5), and the metal element in the metal-containing compound comprises at least one of Zn, Co, Li, Zr or Al.
[0058] In the above preparation steps, the biomass polyamide contains oxygen-containing five-membered rings and amide bond groups, thereby providing a source for the formation of the coating, and the metal-containing compound provides a source of metal elements in the coating.
[0059] Under an inert gas (such as nitrogen or argon), the residual carbon mass ratio of the biomass polyamide and the metal-containing compound is controlled at the same carbonization temperature, so that the element content ratio in the coating formed by the biomass polyamide and the metal-containing compound after carbonization can be controlled and adjusted. The carbonization temperature refers to the carbonization temperature of the coating slurry and graphite after mixing in an inert atmosphere. The residual carbon mass ratio of the biomass polyamide and the metal-containing compound at the same carbonization temperature can be 1:1, 1:2, 1:3, 1:4, 1:5 or any value within the range formed by any two of the above values.
[0060] The solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, toluene, dichloromethane, dichloroethane, tetrahydrofuran, dimethyl sulfoxide or water.
[0061] (2) Add the coating slurry to the graphite and mix well to obtain an intermediate.
[0062] In the above adding process, the graphite powder is first added into the V-type high-efficiency mixer, and the coating slurry is slowly added while stirring, so that the coating slurry and graphite are fully and evenly mixed.
[0063] (3) In an inert atmosphere, the intermediate is placed at a carbonization temperature of 400° C. to 800° C. for a carbonization time of 2 h to 5 h to obtain a negative electrode material.
[0064] The percentage of the coating in the final negative electrode material to the graphite mass is 0.5-2%.
[0065] In an inert atmosphere, the graphite and the coating slurry in the intermediate are carbonized, and the coating slurry is coated on the graphite to obtain a negative electrode material.
[0066] In some embodiments, the inert atmosphere includes at least one of nitrogen or argon.
[0067] The carbonization temperature can be 400°C, 500°C, 600°C, 700°C, 800°C or any value within the range of any two of the above values. Compared with graphite-coated asphalt (carbonization temperature of about 1100°C), the carbonization temperature used in this application reduces the temperature of carbonized graphite-coated carbide, which is also conducive to reducing the loss of energy density in the negative electrode material. During the carbonization process, the temperature is increased at a heating rate of 5°C / min.
[0068] The carbonization time can be 2 h, 3 h, 3.5 h, 4 h, 5 h or any value within the range formed by any two of the above values. Within a specific time, the coating slurry is fully coated on the graphite to obtain the negative electrode material.
[0069] In the above preparation method, the coating slurry is coated on graphite. After the above carbonization process, the coating slurry is evenly coated on the surface of the graphite. Part of the coating slurry is carbonized and forms a carbon network containing metal doping, and part of the coating slurry will remain on the surface of the graphite, so that the coating will contain oxygen-containing five-membered rings and amide bonds, so that the electrochemical device has good low-temperature performance and a higher energy density.
[0070] In some embodiments, the biomass polyamide contains at least one of the following structural segments:
[0071]
[0072] The degree of polymerization n of the structural fragment is 500 to 2000. The oxygen-containing five-membered ring structure contained in the structural fragment can cross-link with graphite, change the curvature of the carbon network structure of graphite, enhance the attraction to lithium ions, facilitate lithium ion desolvation, improve the low-temperature performance of the negative electrode material, and also facilitate the doping of metal elements in the oxygen-containing five-membered ring structure, improve the electronic conductivity of the negative electrode material, thereby improving the low-temperature performance and energy density of the electrochemical device.
[0073] In some embodiments, the metal-containing compound is selected from at least one of the following compounds: C8H 10 N4Zn (abbreviated as ZIF-8), C 24 H 12 O 13 Zn4 (abbreviated as MOF-5), C4H6N2Co (abbreviated as ZIF-67), Li3PO4, LiF, C 48 H 24 O 32 Zr6 (abbreviated as UIO-66), C 24 H 16 O 32 Zr6 (abbreviated as MOF-808) or C 18 H 10 Al3O 17(abbreviated as MIL-100(Al)). After carbonization, the above-mentioned metal-containing compounds form metal elements doped in the carbon network structure, which can improve the electronic conductivity of the negative electrode material. The above-mentioned metal-containing compounds will partially remain on the surface of graphite during the carbonization process. The residues and the metal elements doped in the carbon network structure can not only improve the electronic conductivity of the negative electrode material, but also promote the desolvation ability of lithium ions and improve the low-temperature performance of the electrochemical device. For example, ZIF-8, on the basis of providing a metal Zn source, has a ligand rich in nitrogen-containing five-membered heterocyclic groups, and the negative electrode material prepared therefrom also contains some residual ligands, which can further enhance the desolvation ability of lithium ions and improve the energy density and low-temperature performance of the electrochemical device. MOF-5, on the basis of providing a metal Zn source, also contains a carboxylic acid benzene ring structure, which can improve the electron cloud density of the carbon network structure, thereby further enhancing the desolvation ability of lithium ions and improving the energy density and low-temperature performance of the electrochemical device. Similarly, ZIF-67 also has the same effect as ZIF-8. Its nitrogen-containing five-membered heterocyclic group can not only improve the desolvation ability of lithium ions, but also the nitrogen doping in its five-membered ring is more conducive to improving the electronic conductivity of the carbon network structure and improving the electronic conductivity of the negative electrode material. Li3PO4 is an excellent film-forming additive. During the process of carbonization and coating on the graphite surface, part of Li3PO4 may be formed on the surface of graphite. When the negative electrode material is used in an electrochemical device, it can improve the composition of the negative electrode material during the first round of lithium insertion, which is conducive to improving the desolvation ability of lithium ions, thereby improving the low-temperature performance of the electrochemical device. Similarly, LiF and Li3PO4 have the same effect. MOF-808, UIO-66 and MIL-100 (Al) all have stable metal centers, and their corresponding crystal structures are regular and contain nanoscale pores, which are conducive to screening lithium ion solvation and easy for lithium ions to pass through, thereby improving the desolvation ability of lithium ions. Therefore, the metal-containing compound provided in the present application can not only provide a source of metal elements and improve the conductivity of the negative electrode material, but also enhance the desolvation ability of lithium ions, thereby facilitating improving the low-temperature performance of the electrochemical device.
[0074] The negative electrode active layer also includes a binder to bind the negative electrode active material particles to facilitate the formation of a film layer, and can also improve the binding force between the negative electrode active layer and the negative electrode current collector. In some embodiments, the binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin or nylon, etc.
[0075] The negative electrode active layer may also include a conductive material, including but not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material may include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material may include but is not limited to metal powder or metal fiber, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.
[0076] Isolation film
[0077] The material and shape of the separator used in the electrochemical device of the present application are not particularly limited, and can be any technology disclosed in the prior art. In some embodiments, the separator includes a polymer or inorganic substance formed of a material that is stable to the electrolyte of the present application.
[0078] For example, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be selected.
[0079] A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. The inorganic layer includes inorganic particles and a binder, and the inorganic particles are selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer is selected from at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polyvinylidene fluoride and poly (vinylidene fluoride-hexafluoropropylene).
[0080] Electrolyte
[0081] According to some embodiments of the present application, the electrolyte includes an organic solvent, a lithium salt and an optional additive. The organic solvent in the electrolyte of the present application may be any organic solvent known in the prior art that can be used as a solvent for the electrolyte. The electrolyte used in the electrolyte according to the present application is not limited, and it can be any electrolyte known in the prior art. The additive of the electrolyte according to the present application may be any additive known in the prior art that can be used as an electrolyte additive. In some embodiments, the organic solvent includes, but is not limited to: ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate or ethyl propionate. In some embodiments, the organic solvent includes an ether solvent, for example, including at least one of 1,3-dioxolane (DO L) and ethylene glycol dimethyl ether (DME). In some embodiments, the lithium salt includes at least one of an organic lithium salt or an inorganic lithium salt. In some embodiments, the lithium salt includes, but is not limited to, lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiP O2F2), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3 SO2)2 (LiTF SI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2) (LiF SI), lithium bis(oxalatoborate) LiB(C2O4)2 (LiB OB) or lithium difluorooxalatoborate LiBF2(C2O4) (LiDFOB). In some embodiments, the additive includes at least one of fluoroethylene carbonate and adiponitrile.
[0082] Positive electrode
[0083] The positive electrode plate includes a positive current collector and a positive active layer disposed on the positive current collector. The positive current collector may be aluminum foil or nickel foil, etc., or may be any composite current collector disclosed in the prior art, such as but not limited to the current collector formed by combining the aforementioned conductive foil and the polymer substrate. The positive active layer contains a positive active material, and the positive active material includes a compound that reversibly embeds and deintercalates lithium ions (i.e., a lithiated intercalation compound). In some embodiments, the positive active material may include a lithium transition metal composite oxide. The lithium transition metal composite oxide contains lithium and at least one element selected from cobalt, manganese and nickel. In some embodiments, the positive active material may include but is not limited to lithium cobaltate, lithium nickel manganese cobaltate, lithium nickel manganese aluminum, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganese oxide, spinel lithium nickel manganese oxide and lithium titanate.
[0084] The positive electrode active layer also includes a binder to bond the positive electrode active material particles to facilitate the formation of a film layer, and at the same time, it can also improve the bonding force between the positive electrode active layer and the positive electrode current collector. In some embodiments, the binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylic (ester) styrene butadiene rubber, epoxy resin or nylon, etc. At least one of the above.
[0085] The positive electrode active layer may also include a conductive material, including but not limited to a carbon-based material, a metal-based material, a conductive polymer, or any combination thereof. In some embodiments, the carbon-based material may include but is not limited to natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, the metal-based material may include but is not limited to metal powder or metal fiber, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.
[0086] The electrochemical device is applied to an electronic device to supply power to a load in the electronic device. Moreover, the negative electrode material in the electrochemical device has excellent low temperature performance and energy density, which is beneficial to improving the service life of the electronic device and its application in a low temperature environment. Among them, the electronic device may include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor, etc.
[0087] The present application is described below by specific examples and comparative examples. Those skilled in the art should understand that the preparation methods described in the present application are only examples, and any other suitable preparation methods are within the scope of the present application.
[0088] Example 1
[0089] <Preparation of negative electrode materials>
[0090] 1. 75g of FDCA-derived bio-based polyamide (solid content 13.98%, viscosity 210,000 cp, degree of polymerization 1000-1200, containing structural fragments including ) was uniformly dissolved in 1L N,N-dimethylacetamide, and then 75g ZIF-8 powder was added and stirred at room temperature for 12h to obtain a coating agent slurry. The residual carbon mass ratio of FDCA-derived bio-based polyamide and ZIF-8 powder at 600 degrees was 1:1.
[0091] 2. Add 10 kg of artificial graphite powder into a V-type high-efficiency mixer, slowly add the coating agent slurry while stirring to evenly mix it with the graphite powder to obtain a mixed powder.
[0092] 3. The mixed powder was transferred into a rotary kiln for heat treatment. The temperature was raised to 600°C at 5°C / min in an inert atmosphere and kept at this temperature for 3 hours to obtain the negative electrode material.
[0093] <Preparation of negative electrode sheet>
[0094] The above negative electrode material, thickener sodium carboxymethyl cellulose (CMC-Na), and binder styrene-butadiene rubber (SBR) are mixed in a weight ratio of 95:2:3, and deionized water is added, and the mixture is stirred and mixed to obtain a negative electrode slurry, wherein the solid content of the negative electrode slurry is 75wt%; the negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 10μm, and dried at 120°C to obtain a negative electrode sheet with a single-sided coating of a negative electrode material layer with a coating thickness of 80μm. Repeat the above steps on the other surface of the copper foil to obtain a negative electrode sheet with a negative electrode material layer coated on both sides. Dry under vacuum conditions at 120°C for 1 hour, and then obtain a negative electrode sheet with a specification of 78mm×875mm after cold pressing, cutting, and slitting.
[0095] <Preparation of positive electrode sheet>
[0096] The positive electrode active material lithium cobalt oxide (LiCoO2), the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) are mixed in a weight ratio of 96:2:2, and N-methylpyrrolidone (NMP) is added, and the mixture is stirred and mixed to obtain a positive electrode slurry, wherein the solid content of the positive electrode slurry is 70wt%; the positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 120℃ for 1 hour to obtain a positive electrode sheet coated with a positive electrode material layer with a thickness of 60μm on one side. Repeat the above steps on the other surface of the aluminum foil to obtain a positive electrode sheet coated with a positive electrode material layer on both sides. Dry under vacuum conditions at 120℃ for 1 hour, and then after cold pressing, cutting, and slitting, a positive electrode sheet with a specification of 74mm×867mm is obtained.
[0097] <Preparation of Electrolyte>
[0098] In an argon atmosphere glove box with a water content of less than 10ppm, non-aqueous organic solvents ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC) were mixed in a weight ratio of 1:1:1, and then lithium salt lithium hexafluorophosphate (LiPF6) was added and mixed evenly to obtain an electrolyte. Based on the mass of the electrolyte, the mass percentage of lithium salt LiPF6 is 12.5%, and the balance is non-aqueous organic solvent.
[0099] <Preparation of Separator Film>
[0100] A polypropylene / polyethylene composite film with a thickness of 7 μm was used as the isolation membrane.
[0101] <Preparation of lithium-ion batteries>
[0102] The positive electrode sheet, separator, and negative electrode sheet prepared above are stacked in order, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play a role of isolation, and then wound to obtain an electrode assembly. After welding the pole ears, the electrode assembly is placed in an aluminum-plastic film packaging bag, and after drying, the electrolyte is injected, and the lithium-ion battery is obtained through vacuum packaging, standing, formation (the upper limit voltage of formation is 4.5V, the formation temperature is 70°C, and the formation standing time is 2 hours), degassing, trimming and other processes.
[0103] Example 2
[0104] Except that in step 3 of preparing the negative electrode material, the heat treatment temperature is replaced with 400 degrees, the rest is the same as Example 1.
[0105] Example 3
[0106] Except that in step 3 of preparing the negative electrode material, the heat treatment temperature is replaced with 800 degrees, the rest is the same as Example 1.
[0107] Example 4
[0108] The process was the same as in Example 1 except that in step 1 of the negative electrode material preparation, 75 g of FDCA-derived bio-based polyamide was uniformly dissolved in 1 L of N,N-dimethylacetamide and then 75 g of ZIF-67 powder was added.
[0109] Example 5
[0110] The process was the same as in Example 1 except that in step 1 of the negative electrode material preparation, 75 g of FDCA-derived bio-based polyamide was uniformly dissolved in 1 L of water and then 50 g of lithium phosphate powder was added.
[0111] Example 6
[0112] Except that in step 3 of the preparation of the negative electrode material, the heat treatment temperature is replaced with 400 degrees, the rest is the same as step 5.
[0113] Example 7
[0114] Except that in step 3 of preparing the negative electrode material, the heat treatment temperature is replaced with 800 degrees, the rest is the same as Example 5.
[0115] Example 8
[0116] The process was the same as in Example 1, except that in step 1 of the negative electrode material preparation, 75 g of FDCA-derived bio-based polyamide was uniformly dissolved in 1 L of N,N-dimethylformamide, and then 100 g of UIO-66 powder was added.
[0117] Example 9
[0118] Except that in step 3 of the preparation of the negative electrode material, the heat treatment temperature is replaced with 400 degrees, the rest is the same as Example 8.
[0119] Example 10
[0120] Except that in step 3 of preparing the negative electrode material, the heat treatment temperature is replaced with 800 degrees, the rest is the same as Example 8.
[0121] Embodiment 11
[0122] The process was the same as in Example 1 except that in step 1 of the negative electrode material preparation, 75 g of FDCA-derived bio-based polyamide was uniformly dissolved in 1 L of N,N-dimethylformamide and then 100 g of MIL-100 (Al) powder was added.
[0123] Example 12
[0124] Except that in step 3 of the preparation of the negative electrode material, the heat treatment temperature is replaced with 400 degrees, the rest is the same as Example 11.
[0125] Example 13
[0126] Except that in step 3 of the preparation of the negative electrode material, the heat treatment temperature is replaced with 800 degrees, the rest is the same as Example 11.
[0127] Embodiment 14
[0128] The process was the same as in Example 1 except that in step 1 of the negative electrode material preparation, 75 g of FDCA-derived bio-based polyamide was uniformly dissolved in 1 L of N,N-dimethylacetamide, and then 75 g of ZIF-8 powder and 50 g of lithium phosphate powder were added.
[0129] Embodiment 15
[0130] The process is the same as in Example 1 except that in step 1 of the preparation of the negative electrode material, 75 g of FDCA-derived bio-based polyamide is uniformly dissolved in 1 L of N,N-dimethylacetamide, and then 150 g of ZIF-8 powder is added and stirred at room temperature for 12 h to obtain a coating agent slurry.
[0131] Comparative Example 1
[0132] Only the graphite raw material in step 2 of preparing the negative electrode material is used as the negative electrode material without any other treatment.
[0133] Comparative Example 2
[0134] The process was the same as in Example 1, except that in step 1 of the preparation of the negative electrode material, 75 g of FDCA-derived bio-based polyamide was uniformly dissolved in 1 L of N,N-dimethylacetamide and stirred at room temperature for 12 h to obtain a coating agent slurry.
[0135] Comparative Example 3
[0136] Except that in step 3 of preparing the negative electrode material, the heat treatment temperature is replaced with 1000 degrees, the rest is the same as Example 1.
[0137] The negative electrode materials prepared in various embodiments and comparative examples and the assembled lithium-ion batteries were tested.
[0138] Test method:
[0139] Negative electrode material to be tested: Take a fully discharged lithium-ion battery, disassemble it, take out the negative electrode, soak it in ethylene carbonate (DMC) for 20 minutes, then rinse it with DMC and acetone in turn to remove the electrolyte and the surface solid electrolyte interface (SEI) film, then place it in an oven and bake it at 80℃ for 12h to obtain the treated negative electrode sheet. Use a scraper to scrape off the negative electrode material layer on the negative electrode sheet, and heat treat the powder of the scraped negative electrode material layer in a tube furnace at 350℃ for 4h under argon protection to obtain the negative electrode material.
[0140] (1) Element content test:
[0141] The mass percentage content of C, N and O elements in the negative electrode material was tested using the German Elementar element analyzer;
[0142] Microwave digestion and PE ICP-OES Optima 7000DV were used to test the mass percentage content of metal elements in the negative electrode materials.
[0143] (2) Weight loss rate test of negative electrode material:
[0144] NETZ S CH STA 449F 3Jupiter was used for thermogravimetric analysis of the material, with reference to the standard JY_T0589.1-2020 / JY_T 0589.4-2020 / JY_T 0589.5-2020 “General Rules for Thermal Analysis Methods”, using 99.99% nitrogen, a heating rate of 10°C / min, and a cut-off temperature of 800°C.
[0145] (3) Graphitization test of negative electrode materials:
[0146] The negative electrode material was tested by X-ray powder diffractometer (XRD, instrument model: Bruker D 8ADVANCE), with Cu Kα as the target material; the voltage and current were 40KV / 40mA, the scanning angle range was 5° to 80°, the scanning step length was 0.00836°, and the time for each step was 0.3s. At the same time, 15% silicon powder was added, and according to the principle of internal standard method, the peak position of silicon standard was used to calibrate the instrument and test error, so as to accurately calculate the characteristic peak position of graphite negative electrode material and obtain the graphitization degree of graphite negative electrode material.
[0147] (4) Specific surface area SSA test of negative electrode material:
[0148] In accordance with the national standard “Determination of the specific surface area of solid substances by gas adsorption BETA method” (GB / T 19587-2017), the specific surface area of the negative electrode material was tested by nitrogen adsorption method using a specific surface area analyzer (model: Tri starⅡ3020M).
[0149] (5) Particle size Dv50 test:
[0150] The particle size of the negative electrode material particles was measured using a Malvern particle size tester (model: MasterSizer 2000). 0.02 g of negative electrode material particles were added to a 50 mL clean beaker, and 20 mL of dispersant ethanol was added. Ultrasonic cleaning was performed in a 120 W ultrasonic cleaning machine for 30 min to completely disperse the negative electrode material particles in ethanol to obtain a sample dispersion. The sample dispersion was tested using a Malvern particle size tester to obtain the particle size Dv50 of the negative electrode material particles.
[0151] (6) Tap density TD test:
[0152] In accordance with the national standard GB / T 24533-2019, a density analyzer (model GeoPyc 1365) was used to test the tap density TD of the negative electrode material.
[0153] (7) Scanning electron microscope test:
[0154] In accordance with the national standard GB / T 38887-2020, the negative electrode material was tested using a scanning electron microscope model ZEI S-SEM (Sigma-02-33).
[0155] (8) Button cell co-embedded capacity test:
[0156] With reference to the national standard: GB / T 24533-2019, "Graphite Negative Electrode Materials for Lithium-ion Batteries", the negative electrode material is mixed, coated, rolled, blasted, and dried to form a negative electrode sheet (the specific process is consistent with the preparation method of the negative electrode sheet in Example 1), and a lithium sheet is used as a positive electrode sheet, assembled into a button battery for testing, but the electrolyte used is 1MLiPF6 dissolved in a three-component solvent (EC:PC:EMC=1:1:1). The button battery is kept at a constant temperature of 25°C for 12h, discharged to 5.0mV at 0.05C, discharged to 5.0mV at 50μA, and discharged to 5.0mV at 20μA. The capacity of the button battery at this time is recorded as the co-embedded lithium capacity; charged to 2.0V at 0.1C, and the capacity of the button battery at this time is recorded as the co-embedded lithium capacity.
[0157] (9) Test method for liquid phase transfer impedance (Rion) of lithium-ion batteries:
[0158] In an environment of 0°C, the lithium-ion battery was connected to the Bio-Logic VMP3 B electrochemical workstation produced by Bio-LogiC in France for testing, with a frequency range of 5mHz to 1000kHz and an amplitude of 5mV. After data collection, the impedance complex plane diagram was used to analyze the data and obtain the lithium ion liquid phase transfer impedance (Rion).
[0159] (10) Lithium-ion battery energy density ratio test:
[0160] Take 5 lithium-ion batteries from each group of all comparative examples and embodiments and take the average value. First, in an environment of 25°C, perform the first charge and discharge, perform constant current and constant voltage charging at a charging current of 0.5C until the upper limit voltage is 4.48V, then perform constant current discharge at a discharge current of 0.2C, and the discharge cut-off voltage is 3V. Calculate the energy density of each embodiment and comparative example: energy density (Wh / L) = discharge capacity (Wh) / lithium-ion battery volume size (L), and calculate the percentage increase in energy density of each embodiment relative to comparative example 1 (i.e., the percentage of energy density in comparative example 1).
[0161] (11) Lithium-ion battery -20 degrees capacity retention test:
[0162] Place the lithium-ion battery in a 25°C environment for 6 hours, and perform constant current charging (CC) on the battery at a charging rate of 1C. After charging to 4.48V, switch to constant voltage charging (CV). Stop charging when the charging current is lower than 0.05C and leave it for 5 minutes. Then discharge the battery to 3V with a constant current of 0.2C, record the 25-degree discharge capacity, and then charge the battery to 4.48V with a charging rate current of 1C according to the previous CC+CV charging mode. Place the lithium-ion battery in a -20-degree environment for 6 hours, and discharge the battery to 3V with a constant current of 0.2C, and record the -20-degree discharge capacity. Calculation formula: -20-degree capacity retention rate = [-20-degree discharge capacity / 25-degree discharge capacity] × 100%. Take 5 lithium-ion batteries for each comparative example and embodiment, and take the average value as the final result.
[0163] (12) Lithium-ion battery 0 degree cycle capacity retention rate:
[0164] In an environment of 0°C, the first charge and discharge are performed, constant current and constant voltage charging is performed at a charging current of 0.5C until the upper limit voltage is 4.48V, and then constant current discharge is performed at a discharge current of 0.5C, and the discharge cut-off voltage is 3V, and the discharge capacity A of the lithium ion battery is measured; then, 800 charge and discharge cycles are performed according to the above steps in an environment of 0°C, and the 800th lithium ion battery discharge capacity B is measured, then the lithium ion battery 0 degree cycle capacity retention rate = B / A×100%; 5 lithium ion batteries of each comparative example and embodiment are taken, and the average value is taken as the final result.
[0165] Figure 1 ] is a scanning electron microscope image of the negative electrode material in Example 1. From (a) and (b), it can be seen that a network structure is formed on the surface of the graphite, and the network structure is cross-linked with the graphite.
[0166] In the button cell test of the present application, some components that are easy to co-embed with graphite (lithium ions and part of the electrolyte solvent are co-embedded in the graphite layer), such as propylene carbonate (PC), are added to the electrolyte of the button cell. The coating effect of the coating of the graphite in the negative electrode material can be compared through the electrolyte containing PC. Comparing the negative electrode material of Example 1 and the graphite in Comparative Example 1, in the co-embedded lithium test of the button cell, in the electrolyte containing PC, the lower the co-embedded lithium capacity, the higher the reversible capacity, indicating that the more significant the desolvation ability of the negative electrode material is, the better the coating effect of the coating of the negative electrode material. This can further verify the coating effect of the negative electrode material. Figure 2 Compared with Comparative Example 1, the co-lithium embedding curve of Example 1 shows that the coating on the surface of the negative electrode material has a better coating effect, improves the desolvation ability of the negative electrode material, and can improve the low temperature performance of the electrochemical device.
[0167] Figure 3 The full battery 0 degree cycle capacity retention rate curve of the negative electrode materials in Example 1 and Comparative Example 1 is shown in FIG. Figure 3 It can be seen that after the graphite surface is coated in Example 1, the cycle capacity retention rate of the corresponding assembled full battery at low temperature is improved.
[0168] The preparation conditions of each embodiment and comparative example are shown in Table 1.
[0169] Table 1
[0170]
[0171]
[0172] Note: “ / ” in Table 1 means there is no corresponding substance or parameter.
[0173] Table 2
[0174]
[0175]
[0176] Combining Table 1 and Table 2, compared with the comparative example, after pyrolysis at different temperatures, the surface of the negative electrode material in the embodiment is coated with a coating, which significantly improves the energy density and low temperature performance of the electrochemical device. In Examples 1 to 15, the content of the same metal in the negative electrode material is different at different heat treatment temperatures, and its residual rate is also different. The higher the temperature, the lower the metal element content, and the lower the weight loss rate of the negative electrode material.
[0177] Compared with Comparative Examples 1 to 2, Examples 1 to 3 significantly improve the energy density and low-temperature performance of the electrochemical device. In Examples 1 to 3, the addition of ZIF-8 not only provides single-atom zinc doping, but its ligand 2-methylimidazole is also rich in nitrogen-containing five-membered rings, which can further improve the energy density ratio and low-temperature performance, achieving the effect of improving both energy density and low-temperature performance. Among them, in Example 1, the co-embedded lithium capacity and the 0-degree liquid phase transfer impedance were significantly reduced at a heat treatment temperature of 600°C, and the low-temperature performance of the electrochemical device was significantly improved. At this temperature, the FDCA-derived polyamide partially decomposes, and the oxygen-containing five-membered rings and amide bonds contained therein can be cross-linked with the graphite surface to form a curvature carbon network, thereby enhancing the attraction to lithium ions and inducing rapid desolvation of lithium ions. Similarly, after treatment at 600 degrees, the desolvation effect and low-temperature cycle performance of Example 4 are basically equivalent to those of Example 1.
[0178] In Examples 5 to 7, when lithium phosphate (Li3PO4) is used as a metal compound additive, it can also reduce the co-intercalation capacity of lithium and improve the energy density and low temperature performance of the electrochemical device. This is because lithium phosphate can improve the SEI film component of the negative electrode material during the first lithium intercalation, which is beneficial to improve the desolvation ability of lithium ions. At the same time, the lithium ions contained in lithium phosphate can effectively improve the first coulomb efficiency of the whole battery, thereby improving the energy density of the electrochemical device, so that the electrochemical device can improve the low temperature performance while maintaining a high energy density.
[0179] In Examples 8 to 13, different types of MOFs are used as metal compound additives. Because they have stable metal centers, they can maintain a certain crystal structure after heat treatment, which plays a role in screening solvents for the conduction of lithium ions on the surface of the negative electrode material. They can also improve the desolvation ability of lithium ions, which is beneficial to improving the low-temperature performance of the electrochemical device.
[0180] In Example 14, the surface of the negative electrode material contains two metal elements, and the electrochemical device still has good energy density and low temperature performance. In Example 15, the mass of the added metal-containing compound is changed, and at different residual carbon ratios, the electrochemical device still has good energy density and low temperature performance compared to the comparative example.
[0181] The above disclosure is only a preferred implementation mode of the present application, and certainly cannot be used to limit the present application. Therefore, equivalent changes made according to the present application are still within the scope covered by the present application.
Claims
1. A negative electrode material, characterized in that: It comprises graphite and a coating located on at least a part of the surface of the graphite, wherein the coating contains carbon, oxygen, nitrogen and metal elements, and the metal element comprises at least one of Zn, Co, Li, Zr or Al.
2. The negative electrode material according to claim 1, characterized in that Based on the mass of the negative electrode material, the mass proportion of the metal element is 0.05% to 0.2%.
3. The negative electrode material according to claim 1, characterized in that The coating contains at least one of the following structural fragments:
4. The negative electrode material according to claim 1, characterized in that In an inert atmosphere, the weight loss rate of the negative electrode material when the temperature is increased from 35° C. to 800° C. is 0.15% to 0.3%.
5. The negative electrode material according to any one of claims 1 to 4, characterized in that The negative electrode material also satisfies at least one of the following conditions: (1) Based on the mass of the negative electrode material, the mass proportion of the nitrogen element is 0.1% to 2%; (2) Based on the mass of the negative electrode material, the mass proportion of the oxygen element is 0.1% to 3%; (3) Based on the mass of the negative electrode material, the mass proportion of the carbon element is 95% to 99%.
6. The negative electrode material according to any one of claims 1 to 4, characterized in that The negative electrode material also satisfies at least one of the following conditions: (1) The graphite includes at least one of artificial graphite or natural graphite; (2) The graphitization degree of the negative electrode material is 94% to 98%; (3) The particle size Dv50 of the negative electrode material is 8 μm to 15 μm; (4) The tap density of the negative electrode material is 0.9 g / cm 3 Up to 1.1g / cm 3 ; (5) The specific surface area of the negative electrode material is 0.5 m 2 / g to 3m 2 / g.
7. A method for preparing a negative electrode material according to any one of claims 1 to 6, characterized in that: include: Dissolving biomass polyamide in a solvent, adding a metal-containing compound, and stirring to obtain a coating slurry, wherein the residual carbon mass ratio of the biomass polyamide to the metal-containing compound at the same carbonization temperature is 1:(1-5), and the metal element in the metal-containing compound comprises at least one of Zn, Co, Li, Zr or Al; adding the coating slurry to graphite and mixing to obtain an intermediate; In an inert atmosphere, the intermediate is placed at a carbonization temperature of 400° C. to 800° C. for a carbonization time of 2 h to 5 h to obtain the negative electrode material.
8. The preparation method according to claim 7, characterized in that: The biomass polyamide contains at least one of the following structural fragments: The polymerization degree n of the structural fragment is 500-2000.
9. The preparation method according to claim 8, characterized in that: The metal-containing compound is selected from at least one of the following compounds: C8H 10 N4Zn、C 24 H 12 O 13 Zn4, C4H6N2Co, Li3 PO4, LiF, C 48 H 24 O 32 Zr6、C 24 H 16 O 32 Zr6 or C 18 H 10 Al3O 17 .
10. An electrochemical device, characterized in that: The negative electrode material comprises the negative electrode material according to any one of claims 1 to 6.
11. An electronic device, characterized in that: An electrochemical device comprising the electrochemical device of claim 10.
Citation Information
Patent Citations
Preparation method of lithium battery carbon material with high stability
CN109698347A
Polymer-coated natural graphite negative electrode material as well as preparation method and application thereof
CN114914421A
Negative electrode material and preparation method and application thereof
CN115000389A
Electrochemical device and electronic device
CN115621534A
Negative electrode active material, electrochemical device, and electronic device
CN115836408A
Cited By
Fast ion conductor composite material and preparation method thereof, secondary battery and electric device
CN119852381A
A fast ion conductor composite material, a preparation method thereof, a secondary battery, and an electrical device
CN119852381B