Lithium ion battery and electronic equipment

By designing a reasonable composition of negative electrode sheet and packaging film gap and silicon-based material in lithium-ion batteries, the problem of battery cycle capacity attenuation caused by changes in silicon material volume is solved, and high energy density and long cycle life are achieved.

CN118899508APending Publication Date: 2024-11-05HONOR DEVICE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310491243.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The volume of silicon material changes greatly during charging and discharging of lithium-ion batteries, resulting in damage to the solid electrolyte interface, attenuation of circulation capacity and damage to aluminum-plastic film, making it difficult to meet the requirements of electronic equipment.

Method used

By designing a reasonable gap between the negative electrode sheet and the packaging film in a lithium-ion battery, the ductility and capacity of the negative electrode sheet are limited, and combined with appropriate silicon-based materials and electrolyte composition, we ensure that the battery avoids the extension of the electrode sheet during charging and discharging. Excessive interference with aluminum-plastic film extends the cycle life.

Benefits of technology

While increasing the energy density, it is achieved to avoid interference and cycle losses between the pole sheet and aluminum-plastic film caused by the expansion of the negative electrode, ensuring both the high capacity and long cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899508A_ABST
    Figure CN118899508A_ABST
Patent Text Reader

Abstract

The invention provides a lithium ion battery and electronic equipment, the lithium ion battery comprises a battery cell, an electrolyte and a packaging film, the battery cell and the electrolyte are located in the packaging film, and the battery cell comprises a plurality of positive pole pieces, a plurality of negative pole pieces and a plurality of diaphragms; when the battery is in a shipment state, the width of the whole battery is w0, the length of the whole battery is h0, the width of the negative pole piece is w1, the length of the negative pole piece is h1, a gap gw between the packaging film and the negative pole piece in the width direction is equal to w0-w1, a gap gh between the packaging film and the negative pole piece in the length direction is equal to h0-h1, and gw meets 0 mmlt; gwlt; gwlt; the thickness is 3 mm, and gh meets 0 mmlt; ght, ght; 5 mm; when the battery is in a fully charged state, the width of the negative pole piece is w2, the length of the negative pole piece is h2, the extension rate yw in the width direction of the negative pole piece is equal to (w2-w1) / w1, and the extension rate yh in the length direction of the negative pole piece is equal to (h2-h1) / h1; the negative pole piece comprises a silicon-based material, and when the gram volume per unit mass of the negative pole piece is a, a and yw meet 0 mAh / gram; yw * alt; a is greater than 75mAh / g, and a and yh meet 0.4 mAh / glt; yh * alt; the capacity is 120 mAh / g; wherein the specific surface area is 400 mAh / gram; a < lt >; the capacity is 1,500 mAh / g. According to the lithium ion battery, the energy density can be improved, meanwhile, the aluminum-plastic film is prevented from being damaged due to expansion of the negative electrode, and the energy density of the lithium ion battery is exerted to the maximum extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electronic technology, and in particular to a lithium-ion battery and an electronic device. Background Art

[0002] At present, consumer electronic devices such as mobile phones and laptops have become important devices in people's work and life, and they are used for longer and longer periods of time in daily work and life. As a result, people's requirements for the thinness and long battery life of these devices are constantly increasing. Correspondingly, the volume energy density (VED) of lithium-ion batteries, which are important power sources for these devices, is getting higher and higher to meet people's requirements for long battery life and thinness.

[0003] Improving the gram capacity of positive and negative electrode materials is an important measure to improve the volume energy density of batteries. The gram capacity of commonly used graphite materials is close to the theoretical limit (such as 372mAh / g), while the gram capacity of silicon (Si) materials is much higher than that of graphite materials (theoretical limit is 4200mAh / g). The application of high gram capacity silicon negative electrode can effectively improve the volume energy density of the battery cell. Silicon materials have many advantages such as moderate lithium insertion and extraction potential, abundant reserves, low price, environmental protection and non-toxicity, and mature preparation process. They are currently considered to be an ideal material to replace graphite materials as negative electrode active materials for batteries.

[0004] However, silicon materials have a huge volume effect. During the repeated lithium insertion and extraction process of the battery during charge and discharge, the volume change rate caused by expansion / contraction is as high as 400%. This causes the solid electrolyte interface (SEI) film on the surface of the silicon material to be continuously destroyed / repaired during the charge / discharge process, continuously consumes active lithium ions, and forms a byproduct layer on the surface, which directly leads to a large cycle capacity attenuation rate and thickness expansion rate of the battery. Therefore, its cycle life is not ideal and it is difficult to meet the use requirements of electronic equipment. Summary of the invention

[0005] In order to solve the above technical problems, the present application provides a lithium-ion battery and an electronic device. The lithium-ion battery can achieve a higher negative electrode plate capacity, while avoiding excessive extension of the plate due to negative electrode expansion, damage to the aluminum-plastic film due to interference between the plate and the aluminum-plastic film, and capacity and cycle losses, thereby ensuring that the battery has both high capacity and cycle performance to the greatest extent.

[0006] In a first aspect, the present application provides a lithium-ion battery, which includes: a battery cell, an electrolyte, and a packaging film. The battery cell and the electrolyte are located within the packaging film. The battery cell includes a plurality of positive electrode plates, a plurality of negative electrode plates, and a plurality of separators. The positive electrode plates and the negative electrode plates are separated by the separators, and the positive electrode plates, the separators, and the negative electrode plates are laminated layer by layer in sequence. The electrolyte is filled between the positive electrode plates, the separators, and the negative electrode plates.

[0007] When the battery is in the shipped state, the overall width of the full battery is w0, the length is h0, the width of the negative electrode plate is w1, and the length is h1. The gap gw in the width direction between the packaging film and the negative electrode plate is gw = w0 - w1, and the gap gh in the length direction is gh = h0 - h1. gw satisfies 0 mm < gw < 3 mm, and gh satisfies 0 mm < gh < 5 mm.

[0008] When the battery is in the fully charged state, the width of the negative electrode plate is w2, and the length is h2. The elongation rate yw in the width direction of the negative electrode plate is yw = (w2 - w1) / w1, and the elongation rate yh in the length direction is yh = (h2 - h1) / h1.

[0009] And the negative electrode plate contains a silicon-based material. When the specific capacity per unit mass of the negative electrode plate is a, a and yw satisfy 0 mAh / g < yw × a < 75 mAh / g, and a and yh satisfy 0.4 mAh / g < yh × a < 120 mAh / g.

[0010] Wherein, 400 mAh / g < a < 1500 mAh / g.

[0011] According to the first aspect, the present application limits the gap between the negative electrode plate of the lithium-ion battery and the packaging film, and the elongation rate and specific capacity of the negative electrode plate within a reasonable range, so as to avoid damage to the aluminum-plastic film due to the expansion of the negative electrode while increasing the energy density.

[0012] Exemplarily, the overall width of the full battery is the size of the entire battery in the first direction, the overall length of the full battery is the size of the entire battery in the second direction, the width of the negative electrode plate is the size of the negative electrode plate in the first direction, and the length of the negative electrode plate is the size of the negative electrode plate in the second direction. Among them, the first direction is perpendicular to the second direction, and the first direction is, for example, the width direction of an electronic device such as a mobile phone (i.e., the X-axis direction in the embodiment), and the second direction is, for example, the length direction of an electronic device such as a mobile phone (i.e., the Y-axis direction in the embodiment).

[0013] According to the first aspect, yw satisfies 0% < yw < 5%, and yh satisfies 0.1% < yh < 8%.

[0014] According to the first aspect, or any implementation manner of the above first aspect, the tensile strength of the current collector in the negative electrode tab when the battery is in the shipped state is f0, where f0 satisfies 300 Mpa < f0 < 600 Mpa, and 0 < yw < 3%, 0.1% < yh < 5%.

[0015] Exemplarily, f0 is 350 Mpa, 400 Mpa, 450 Mpa, 500 Mpa, 550 Mpa, etc.

[0016] According to the first aspect, or any implementation manner of the above first aspect, after 700 cycles, the tensile strength of the current collector in the negative electrode tab is f1, where f1 satisfies 80% < f1 / f0 < 100%.

[0017] According to the first aspect, or any implementation manner of the above first aspect, the packaging film is an aluminum-plastic film.

[0018] According to the first aspect, or any implementation manner of the above first aspect, the silicon-based material includes at least one of nano-silicon, silicon oxide, silicon-carbon composite material, or silicon alloy material.

[0019] According to the first aspect, or any implementation manner of the above first aspect, the positive active material of the positive electrode tab includes at least one of lithium cobaltate, lithium manganate, lithium iron phosphate, lithium nickelate, lithium nickel cobaltate, and lithium nickel cobalt manganate.

[0020] According to the first aspect, or any implementation manner of the above first aspect, the material of the separator includes at least one of polyethylene, polypropylene, and polyvinylidene fluoride.

[0021] In a second aspect, the present application provides an electronic device, including: the lithium-ion battery according to the first aspect, or any implementation manner of the above first aspect. It has the same beneficial effects as the first aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic structural diagram of the electronic device shown exemplarily;

[0023] Figure 2 It is a schematic cross-sectional view in the length direction of the stacked battery cell shown exemplarily;

[0024] Figure 3 It is a schematic cross-sectional view in the width direction of the stacked battery cell shown exemplarily;

[0025] Figure 4 It is a schematic diagram of the extension of the negative electrode tab of the gasket battery in the shipped state and the fully charged state. DETAILED DESCRIPTION OF THE EMBODIMENTS

[0026] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0027] The term "and / or" in this article is merely a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone.

[0028] The terms "first" and "second" in the description and claims of the embodiments of the present application are used to distinguish different objects rather than to describe a specific order of objects. For example, a first target object and a second target object are used to distinguish different target objects rather than to describe a specific order of target objects.

[0029] In the embodiments of the present application, words such as "exemplary" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary" or "for example" is intended to present related concepts in a specific way.

[0030] In the description of the embodiments of the present application, unless otherwise specified, the meaning of "multiple" refers to two or more than two. For example, multiple processing units refer to two or more processing units; multiple systems refer to two or more systems.

[0031] Definition of terms

[0032] Shipping state: The state of charge (SOC) of the battery cell is 70%. The battery in this state is also called a shipping state battery or a half-charged battery. The process of charging the battery to the shipping state is called half-charging.

[0033] Fully charged state: The state of charge (SOC) of the battery cell is 100%. The battery in this state is also called a fully charged battery or a fully charged battery. The process of charging the battery to the fully charged state is called full charging.

[0034] Elongation rate of negative electrode sheet: the ratio of the difference between the length of the negative electrode sheet in fully charged state and the length in shipped state to the length in shipped state, the ratio of the difference between the width of the negative electrode sheet in fully charged state and the width in shipped state to the width in shipped state.

[0035] High temperature cycle test: The test temperature is 45°C, and the battery is charged at a certain rate, such as 1C, 2C constant current charging to the upper voltage, such as 4.48V, 4.5V, etc., and charged at a constant voltage to 0.025C. After standing for 5 minutes, the battery is discharged at 0.7C to 3.0V. The capacity obtained in this step is taken as the initial capacity, and the corresponding rate charging / 0.7C discharge is performed for cycle testing. The capacity at each step is compared with the initial capacity to obtain a capacity decay curve. This application illustrates the battery cycle performance by counting the number of cycles at which the capacity decays to 80% of the initial capacity.

[0036] The present application embodiment provides an electronic device, which may be a mobile phone, a tablet computer, a personal digital assistant (PDA), a car computer, a television, a smart wearable device, or other electronic device containing a battery. The present application embodiment does not specifically limit the specific form of the above electronic device. Figure 1 As shown, for the convenience of explanation, the electronic device is taken as an example of a mobile phone.

[0037] like Figure 1 As shown, the mobile phone may include a battery 100, a display screen 200, a middle frame 300 and a rear shell 400. The display screen 200, the middle frame 300 and the rear shell 400 form a storage space for accommodating various components, and the size of the storage space can be set according to the size requirements of various components in the mobile phone. For example, the relevant components may include the above-mentioned battery 100. For the convenience of explanation, the width direction of the mobile phone is defined as the X-axis direction, the length direction of the mobile phone is defined as the Y-axis direction, and the height direction of the mobile phone is defined as the Z-axis direction.

[0038] See also Figure 2 and Figure 3 , Figure 2 Schematic diagram of a cross section of a laminated battery cell in the length direction is shown as an example. Figure 3 The cross-sectional schematic diagram of the width direction of the laminated battery cell is shown as an example, wherein the length direction of the battery cell is the Y-axis direction, and the width direction of the battery cell is the X-axis direction.

[0039] like Figure 2 and Figure 3As shown, the laminated battery 100 of the embodiment of the present application includes a battery cell 10, an electrolyte (not shown) and a packaging film 20. The battery cell 10 and the electrolyte are located in the packaging film 20. The electrolyte is a carrier for ion transmission in the battery, generally composed of lithium salts and organic solvents. The electrolyte plays a role in conducting ions between the positive and negative electrodes of the lithium battery. Different types of battery electrolytes use different compositions, which are not specifically limited and described here. The battery cell 10 includes a plurality of positive electrode sheets 11, a plurality of negative electrode sheets 13 and a plurality of separators 12. The positive electrode sheets 11, the separators 12 and the negative electrode sheets 13 are stacked layer by layer (along the Z-axis direction) in the order of positive electrode-separator-negative electrode to form the battery cell 10. The separator 12 is located between the positive electrode sheet 11 and the negative electrode sheet 13. It should be understood that the separator 12 can be a cut-off separator, that is, each layer of the separator 12 is cut off from each other, and the laminated battery using such a separator is also called a stacked laminated battery. The diaphragm 12 may also not be cut, that is, each layer of the diaphragm 12 is connected to each other to form an integral structure, which is roughly folded in a Z shape. The laminated battery using such a diaphragm is also called a folded laminated battery.

[0040] like Figure 2 and Figure 3 As shown, the length of the negative electrode sheet 13 is greater than the length of the positive electrode sheet 11, and the width of the negative electrode sheet 13 is greater than the width of the positive electrode sheet 11. Exemplarily, the length and width of the negative electrode sheet 13 are respectively 0.5 mm to 3 mm greater than the length and width of the positive electrode sheet 11, that is, the length of the negative electrode sheet 13 is 0.5 mm to 3 mm longer than the length of the positive electrode sheet 11, such as 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, or 3 mm, and the width of the negative electrode sheet 13 is 0.5 mm to 3 mm wider than the width of the positive electrode sheet 11, such as 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm or 3 mm. The length of the diaphragm 12 is greater than the length of the negative electrode plate 13, and the width of the diaphragm 12 is greater than the width of the negative electrode plate 13. Exemplarily, the length and width of the diaphragm 12 are respectively 1 to 4 mm greater than the length and width of the negative electrode 13, that is, the length of the diaphragm 12 is 1 mm to 4 mm longer than the length of the negative electrode 13, such as 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm or 4 mm, and the width of the diaphragm 12 is 1 mm to 4 mm wider than the width of the negative electrode 13, such as 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm or 4 mm.

[0041] like Figure 2 and Figure 3As shown, the cross-section of the packaging film 20 is roughly trapezoidal. The internal space of the packaging film 20 is called an inner pit, and the cross-sectional side walls in the length direction of the inner pit include a convex R corner at the bottom and a concave R corner at the top, as well as a connecting strip between the convex R corner and the concave R corner. In the embodiment of the present application, the distance between the tops of the convex R corners of the two side walls in the length direction is taken as the length of the inner pit of the packaging film, also referred to as the length h0 of the battery. The distance between the top of the convex R corner of the side wall and the negative electrode sheet 13 in the shipping state is the PA Gap in the length direction: gh = h0-h1, where h1 is the length of the negative electrode sheet in the battery shipping state.

[0042] The cross-sectional sidewall in the width direction of the inner pit includes the convex R corner and the side seal at the bottom. In the embodiment of the present application, the distance between the tops of the convex R corners of the two side walls in the width direction is used as the width of the inner pit of the packaging film, also known as the width w0 of the battery. The distance between the top of the convex R corner of the side wall and the negative electrode sheet 13 in the shipping state is the PA Gap in the width direction: gw = w0-w1, w1 is the width of the negative electrode sheet in the battery shipping state.

[0043] Illustratively, in the embodiment of the present application, the packaging film 20 comprises an aluminum-plastic film, which can be formed into a structure required by the battery by equipment such as an aluminum-plastic film forming machine.

[0044] For lithium batteries, the negative electrode sheet will expand to a certain extent in the X, Y, and Z directions during charging. For this reason, a gap PA gap is set between the packaging film and the negative electrode sheet when designing the battery to prevent the expansion of the negative electrode sheet in the X and Y directions from causing deformation of the sheet, damage to the packaging film, and other problems. Although the PA gap of conventional cells can meet the needs of graphite negative electrode cell systems, it cannot meet the needs of silicon negative electrode systems with large volume expansion. This is because: when the gram capacity a of the silicon-containing negative electrode is large (usually refers to when a exceeds the gram capacity of the graphite negative electrode of 372 mAh / g), the battery cell is fully charged, the lithium-embedded silicon-containing negative electrode expands greatly, and the negative electrode pole piece is prone to extension in the X and Y directions (i.e., the length and width directions), and as the silicon content (gram capacity of the silicon-containing negative electrode pole piece) increases, the extension in the X and Y directions becomes more serious. If the P-Agap design of the graphite battery cell is maintained, there will be interference between the negative electrode pole piece and the packaging film, which will lead to deformation of the negative electrode pole piece and damage to the packaging film, greatly reducing the safety of the battery cell, and also causing a greater cycle capacity attenuation rate and thickness expansion rate. Therefore, for high-gram capacity Si-containing negative electrode (high Si content) batteries, more PA gaps need to be designed to meet the requirements.

[0045] Figure 4 The figure shows the changes of the negative electrode sheet and the gap PA gap when the battery is shipped and fully charged. Figure 4The shipping state diagram shows the gap between the negative electrode tab and the packaging film of the battery in the P-A gap design of a conventional battery cell. The fully charged state diagram of the graphite battery cell shows the gap between the negative electrode tab and the packaging film when the graphite battery cell is in a satisfied state. The fully charged state diagram of the high-Si battery cell shows the gap between the negative electrode tab and the packaging film when the high-Si battery cell is in a satisfied state. Reference Figure 4 As can be seen from the reference, for the P-A gap design of a conventional battery cell, when applied to a high-Si battery cell, due to more serious X and Y extensions of the negative electrode tab, it is very easy to interfere with the packaging film, resulting in problems such as deformation of the negative electrode tab and damage to the packaging film, and further leading to a large cycle capacity attenuation rate and thickness expansion rate of the battery.

[0046] Based on the above description, an embodiment of the present application provides a silicon-containing negative electrode lithium-ion battery, which realizes a high-energy-density battery by reasonably designing the P-A gap, the specific capacity of the negative electrode tab, and the extension rate of the negative electrode tab, while avoiding excessive extension of the tab caused by negative electrode swelling, damage to the aluminum-plastic film caused by interference between the tab and the aluminum-plastic film, and capacity and cycle losses, thereby ensuring that the battery gives full consideration to high capacity and cycle performance to the greatest extent.

[0047] Embodiment 1

[0048] Preparation of the full battery

[0049] (1) The positive electrode active material LiCoO2, conductive carbon black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed evenly in an NMP (N-methyl-2-pyrrolidone) solvent system according to a weight ratio of 96.7:1.7:1.6, and then coated on a current collector, dried, cold-pressed, and slit to obtain a positive electrode tab. Exemplarily, the positive electrode current collector includes aluminum foil.

[0050] (2) Silicon oxide SiOx (0.5 < x < 1.5, DV50 = 5 - 10 μm), prelithiated silicon oxide, silicon-carbon negative electrode material, and graphite negative electrode material are mixed to obtain a negative electrode composite product, where the proportion of the Si-containing negative electrode material in the composite product is 0 - 100 wt%. The negative electrode active material, conductive agent acetylene black, and polyacrylic acid (PAA) are fully stirred and mixed evenly in a deionized water solvent system according to a weight ratio of 95:1.2:3.8, and then coated on a current collector, dried, cold-pressed, and slit to obtain a negative electrode tab. Exemplarily, the negative electrode current collector includes copper foil.

[0051] When coating the negative electrode active material on the copper foil above, the coating weight is 9.74 mg / cm 2 , and a certain value is selected within the range of 0 - 100 wt% for the proportion of the Si-containing negative electrode material in the composite product, so that the specific capacity a of the negative electrode tab is 450 mAh / g.

[0052] (3) Using a polyethylene (PE) porous polymer film as a separator, the positive electrode sheet, the separator, and the negative electrode sheet are stacked layer by layer in sequence to obtain a laminated battery cell.

[0053] (4) Preparation of electrolyte: In a dry oxygen environment, lithium hexafluorophosphate (LiPF6) is added to a solvent solution of propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) in a weight ratio of 1:1:1 and mixed evenly, wherein the concentration of LiPF6 is about 1.15 mol / L, and then 12 wt% of fluoroethylene carbonate (FEC) is added and mixed evenly to obtain an electrolyte.

[0054] (4) The battery cell is packaged into the inner pit of the packaging film, and after drying, the electrolyte is injected and packaged, and a full battery is obtained after formation, degassing, and trimming.

[0055] By controlling the gap PA gap between the negative electrode plate and the packaging film, the width of the full battery after half charge is w0=15~70mm, the length is h0=20~100mm, the width of the negative electrode plate is w1=12~68mm, the length is h1=15~95mm, the gap PA gap is: gw=1.0mm, gh=1.8mm, and after full charge, the width of the negative electrode plate is w2, the length is h2, the elongation of the negative electrode plate is yw=(w2-w1) / w1=0.4%, yh=(h2-h1) / h1=1.5%, and yw×a=1.8mAh / g, yh×a=6.75mAh / g.

[0056] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0057] It should be understood that the materials of the above-mentioned electrolyte and diaphragm are exemplary. In other embodiments of the present application, the electrolyte may also be one or more of EC, DMC, EMC, DEC, VC, and PS, wherein EC is ethylene carbonate, Ethylenecarbonate; DMC is dimethyl carbonate, Dimethyl carbonate; EMC is ethyl methyl carbonate, Ethyl MethylCarbonate; DEC is diethyl carbonate, Diethyl carbonate; VC is vinylene carbonate, Vinylenecarbonate; PS is polystyrene, Polystyrene or more. The diaphragm may also be a composite structure composed of PE, ceramics, and glue coating or other structures.

[0058] Example 2

[0059] The difference from Example 1 is that the gap PA gap between the negative electrode sheet and the packaging film is: gw = 0.9 mm, gh = 1.6 mm, that is, the gap in the length direction becomes smaller, and the gap in the width direction also becomes smaller. The gram capacity a of the negative electrode sheet is the same as that in Example 1, which is 450 mAh / g, and the elongation of the negative electrode sheet is the same as that in Example 1, that is, yw = (w2-w1) / w1 = 0.4%, yh = (h2-h1) / h1 = 1.5%, and yw×a = 1.8 mAh / g, yh×a = 6.75 mAh / g.

[0060] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0061] Example 3

[0062] The difference from Example 1 is that the gap PA gap between the negative electrode sheet and the packaging film is: gw = 1.1 mm, gh = 1.9 mm, that is, the gap in the length direction becomes larger, and the gap in the width direction also becomes larger. The gram capacity a of the negative electrode sheet is the same as that in Example 1, which is 450 mAh / g, and the elongation of the negative electrode sheet is the same as that in Example 1, that is, yw = (w2-w1) / w1 = 0.4%, yh = (h2-h1) / h1 = 1.5%, and yw×a = 1.8 mAh / g, yh×a = 6.75 mAh / g.

[0063] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0064] Example 4

[0065] The difference from Example 1 is that the tensile strength f0 of the current collector in the negative electrode sheet increases when the battery is shipped, for example, f0 increases from 100 MPa to 400 MPa, and the gap PA gap between the negative electrode sheet and the packaging film is controlled so that the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode sheet is w1, and the length is h1, and the gap PA gap is: gw=1.0mm, gh=1.8mm, which is the same as the gap PA gap in Example 1, and after full charge, the width of the negative electrode sheet is w2, and the length is h2, and the elongation of the negative electrode sheet is yw=(w2-w1) / w1=0.2%, yh=(h2-h1) / h1=1.00%, and yw×a=0.9mAh / g, yh×a=4.5mAh / g.

[0066] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0067] Example 5

[0068] The difference from Example 1 is that silicon oxide SiOx (0.5 < x < 1.5, DV50 = 5 - 10 μm), prelithiated silicon oxide, silicon-carbon anode material and graphite anode material are mixed to obtain a negative electrode composite, where the proportion of the Si-containing anode material in the composite is 0 - 100 wt%. After the negative electrode active material, conductive agent acetylene black, and polyacrylic acid (PAA) are fully stirred and mixed evenly in a deionized water solvent system according to a weight ratio of 95:1.2:3.8, they are coated on a current collector, dried, cold-pressed, and slit to obtain a negative electrode sheet. Exemplarily, the negative electrode current collector includes a copper foil.

[0069] When coating the negative electrode active material on the copper foil above, the coating weight is 9.74 mg / cm 2 , and a definite value is selected within the range of 0 - 100 wt% for the proportion of the Si-containing anode material in the composite, such that the specific capacity a of the negative electrode sheet is 600 mAh / g.

[0070] By controlling the gap P - A gap between the negative electrode sheet and the packaging film, the width of the fully charged battery is w0, the length is h0, the width of the negative electrode sheet is w1, the length is h1, and the gap P - A gap is: gw = 1.3 mm, gh = 2.2 mm. And after full charge, the width of the negative electrode sheet is w2, the length is h2, and the elongation rates of the negative electrode sheet are yw = (w2 - w1) / w1 = 1.00%, yh = (h2 - h1) / h1 = 2.00%, and yw × a = 6 mAh / g, yh × a = 12 mAh / g.

[0071] After obtaining the above lithium-ion full battery, battery performance tests are carried out, including battery cycle performance tests, and the test results are shown in Table 1 for details.

[0072] Example 6

[0073] The difference from Example 5 is that the gap P - A gap between the negative electrode sheet and the packaging film is: gw = 1.2 mm, gh = 2 mm, that is, the gap in the length direction becomes smaller, and the gap in the width direction also becomes smaller. The specific capacity a of the negative electrode sheet is the same as that in Example 5, which is 600 mAh / g, and the elongation rates of the negative electrode sheet are the same as those in Example 5, that is, yw = (w2 - w1) / w1 = 1.00%, yh = (h2 - h1) / h1 = 2.00%, and yw × a = 6 mAh / g, yh × a = 12 mAh / g.

[0074] After obtaining the above lithium-ion full battery, battery performance tests are carried out, including battery cycle performance tests, and the test results are shown in Table 1 for details.

[0075] Example 7

[0076] It is different from Example 5 in that the tensile strength f0 of the current collector in the negative electrode tab at the time of battery shipment is increased. For example, f0 is increased from 100 Mpa to 400 Mpa. By controlling the gap P-A gap between the negative electrode tab and the packaging film, the width of the fully charged battery is w0, the length is h0, the width of the negative electrode tab is w1, the length is h1, and the gap P-A gap is: gw = 1.1 mm, gh = 1.9 mm. After full charge, the width of the negative electrode tab is w2, the length is h2, the elongation rate of the negative electrode tab is yw = (w2 - w1) / w1 = 0.80%, yh = (h2 - h1) / h1 = 1.90%, and yw × a = 4.8 mAh / g, yh × a = 11.4 mAh / g.

[0077] After obtaining the above lithium-ion full battery, battery performance tests are carried out, including battery cycle performance tests. The test results are shown in Table 1 for details.

[0078] Example 8

[0079] It is different from Example 1 in that silicon oxide SiOx (0.5 < x < 1.5, DV50 = 5 - 10 μm), prelithiated silicon oxide, silicon-carbon anode material and graphite anode material are mixed to obtain a negative electrode composite product, where the proportion of the Si-containing anode material in the composite product is 0 - 100 wt%. After the negative electrode active material, conductive agent acetylene black, and polyacrylic acid (PAA) are fully stirred and mixed evenly in a deionized water solvent system according to a weight ratio of 95:1.2:3.8, they are coated on the current collector, dried, cold-pressed, and slit to obtain a negative electrode tab. Exemplarily, the negative electrode current collector includes copper foil.

[0080] When coating the negative electrode active material on the copper foil above, the coating weight is 9.74 mg / cm 2 , and a definite value is selected within the range of 0 - 100 wt% for the proportion of the Si-containing anode material in the composite product, so that the specific capacity a of the negative electrode tab is 850 mAh / g.

[0081] By controlling the gap P-A gap between the negative electrode tab and the packaging film, the width of the fully charged battery is w0, the length is h0, the width of the negative electrode tab is w1, the length is h1, and the gap P-A gap is: gw = 1.5 mm, gh = 2.5 mm. After full charge, the width of the negative electrode tab is w2, the length is h2, the elongation rate of the negative electrode tab is yw = (w2 - w1) / w1 = 1.30%, yh = (h2 - h1) / h1 = 2.30%, and yw × a = 11.05 mAh / g, yh × a = 19.55 mAh / g.

[0082] After obtaining the above lithium-ion full battery, battery performance tests are carried out, including battery cycle performance tests. The test results are shown in Table 1 for details.

[0083] Example 9

[0084] The difference from Example 8 is that the gap P - A gap between the negative electrode plate and the packaging film is: gw = 1.7 mm, gh = 2.8 mm, that is, the gap in the length direction becomes larger, and the gap in the width direction also becomes larger. The specific capacity a of the negative electrode plate is the same as that in Example 8, which is 850 mAh / g, and the elongation rate of the negative electrode plate is the same as that in Example 8, that is, yw = (w2 - w1) / w1 = 1.30%, yh = (h2 - h1) / h1 = 2.30%, and yw × a = 11.05 mAh / g, yh × a = 19.55 mAh / g.

[0085] After obtaining the above lithium - ion full cell, battery performance tests are carried out, including battery cycle performance tests. The test results are shown in Table 1 for details.

[0086] Example 10

[0087] The difference from Example 8 is that the tensile strength f0 of the current collector in the negative electrode plate at the time of battery shipment increases. For example, f0 increases from 100 Mpa to 400 Mpa. By controlling the gap P - A gap between the negative electrode plate and the packaging film, the width of the full cell after half - charge is w0, the length is h0, the width of the negative electrode plate is w1, the length is h1, and the gap P - A gap is: gw = 1.3 mm, gh = 2.3 mm. And after full charge, the width of the negative electrode plate is w2, the length is h2, the elongation rate of the negative electrode plate is yw = (w2 - w1) / w1 = 1.10%, yh = (h2 - h1) / h1 = 2.00%, and yw × a = 9.35 mAh / g, yh × a = 17 mAh / g.

[0088] After obtaining the above lithium - ion full cell, battery performance tests are carried out, including battery cycle performance tests. The test results are shown in Table 1 for details.

[0089] Example 11

[0090] The difference from Example 1 is that silicon oxide SiOx (0.5 < x < 1.5, DV50 = 5 - 10 μm), pre - lithiated silicon oxide, silicon - carbon negative electrode material and graphite negative electrode material are mixed to obtain a negative electrode composite product, where the proportion of the Si - containing negative electrode material in the composite product is 0 - 100 wt%. After the negative electrode active material, conductive agent acetylene black, and polyacrylic acid (PAA) are fully stirred and mixed evenly in a deionized water solvent system according to a weight ratio of 95:1.2:3.8, they are coated on the current collector, dried, cold - pressed, and slit to obtain a negative electrode plate. Exemplarily, the negative electrode current collector includes copper foil.

[0091] When coating the negative electrode active material on the copper foil above, the coating weight is 9.74 mg / cm 2, control the proportion of Si negative electrode material in the composite product to select a certain value within 0 to 100wt%, so that the gram capacity a of the negative electrode plate is 1000mAh / g.

[0092] By controlling the gap PA gap between the negative electrode plate and the packaging film, the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode plate is w1, and the length is h1, and the gap PA gap is: gw=1.6mm, gh=2.7mm, and after full charge, the width of the negative electrode plate is w2, and the length is h2, the elongation of the negative electrode plate is yw=(w2-w1) / w1=1.50%, yh=(h2-h1) / h1=2.60%, and yw×a=15mAh / g, yh×a=26mAh / g.

[0093] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0094] Example 12

[0095] The difference from Example 11 is that the gap PA gap between the negative electrode plate and the packaging film is: gw = 1.7 mm, gh = 2.8 mm, that is, the gap in the length direction becomes larger, and the gap in the width direction also becomes larger. The gram capacity a of the negative electrode plate is the same as that of Example 11, which is 1000 mAh / g, and the elongation of the negative electrode plate is the same as that of Example 11, that is, yw = (w2-w1) / w1 = 1.50%, yh = (h2-h1) / h1 = 2.60%, and yw×a = 15 mAh / g, yh×a = 26 mAh / g.

[0096] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0097] Embodiment 13

[0098] The difference from Example 11 is that the tensile strength f0 of the current collector in the negative electrode sheet increases when the battery is shipped, for example, f increases from 100 MPa to 400 MPa, and the gap PA gap between the negative electrode sheet and the packaging film is controlled so that the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode sheet is w1, and the length is h1, and the gap PA gap is: gw=1.5mm, gh=2.5mm, and after full charge, the width of the negative electrode sheet is w2, and the length is h2, and the elongation of the negative electrode sheet is yw=(w2-w1) / w1=1.40%, yh=(h2-h1) / h1=2.40%, and yw×a=14mAh / g, yh×a=24mAh / g.

[0099] After obtaining the above lithium-ion full battery, battery performance tests are carried out, including battery cycle performance tests. The test results are shown in Table 1 in detail.

[0100] Example 14

[0101] The difference from Example 1 is that silicon oxide SiOx (0.5 < x < 1.5, DV50 = 5 - 10 μm), prelithiated silicon oxide, and silicon-carbon anode materials are mixed with graphite anode materials to obtain a negative electrode composite product, where the proportion of Si-containing anode materials in the composite product is 0 - 100 wt%. After the negative electrode active materials, conductive agent acetylene black, and polyacrylic acid (PAA) are fully stirred and mixed evenly in a deionized water solvent system according to a weight ratio of 95:1.2:3.8, they are coated on the current collector, dried, cold-pressed, and slit to obtain a negative electrode sheet. Exemplarily, the negative electrode current collector includes copper foil.

[0102] When coating the negative electrode active materials on the copper foil above, the coating weight is 9.74 mg / cm 2 , and a definite value is selected within the range of 0 - 100 wt% for the proportion of Si-containing anode materials in the composite product, such that the specific capacity a of the negative electrode sheet is 1200 mAh / g.

[0103] By controlling the gap P-A gap between the negative electrode sheet and the packaging film, the width of the full battery after half charge is w0, the length is h0, the width of the negative electrode sheet is w1, the length is h1, and the gap P-A gap is: gw = 1.7 mm, gh = 2.8 mm. And after full charge, the width of the negative electrode sheet is w2, the length is h2, the elongation rate of the negative electrode sheet is yw = (w2 - w1) / w1 = 1.70%, yh = (h2 - h1) / h1 = 2.80%, and yw × a = 20.4 mAh / g, yh × a = 33.6 mAh / g.

[0104] After obtaining the above lithium-ion full battery, battery performance tests are carried out, including battery cycle performance tests. The test results are shown in Table 1 in detail.

[0105] Example 15

[0106] The difference from Example 14 is that the gap P-A gap between the negative electrode sheet and the packaging film is: gw = 1.8 mm, gh = 2.9 mm, that is, the gap in the length direction becomes larger, and the gap in the width direction also becomes larger. The specific capacity a of the negative electrode sheet is the same as that in Example 14, which is 1200 mAh / g, and the elongation rate of the negative electrode sheet is the same as that in Example 14, that is, yw = (w2 - w1) / w1 = 1.70%, yh = (h2 - h1) / h1 = 2.80%, and yw × a = 20.4 mAh / g, yh × a = 33.6 mAh / g.

[0107] After obtaining the above lithium-ion full battery, battery performance tests are carried out, including battery cycle performance tests. The test results are shown in Table 1 in detail.

[0108] Example 16

[0109] The difference from Example 14 is that the tensile strength f0 of the current collector in the negative electrode sheet at the time of battery shipment increases. For example, f increases from 100 Mpa to 400 Mpa. By controlling the gap P-A gap between the negative electrode sheet and the packaging film, the width of the full battery after half charge is w0, the length is h0, the width of the negative electrode sheet is w1, the length is h1, and the gap P-A gap is: gw = 1.5 mm, gh = 2.6 mm. And after full charge, the width of the negative electrode sheet is w2, the length is h2, the elongation rate of the negative electrode sheet is yw = (w2 - w1) / w1 = 1.60%, yh = (h2 - h1) / h1 = 2.70%, and yw × a = 19.2 mAh / g, yh × a = 32.4 mAh / g.

[0110] After obtaining the above lithium-ion full battery, battery performance tests are carried out, including battery cycle performance tests. The test results are shown in Table 1 in detail.

[0111] Example 17

[0112] The difference from Example 1 is that silicon oxide SiOx (0.5 < x < 1.5, DV50 = 5 - 10 μm), prelithiated silicon oxide, and silicon-carbon anode materials are mixed with graphite to obtain a negative electrode composite product, where the proportion of the Si-containing anode material in the composite product is 0 - 100 wt%. After the negative electrode active material, conductive agent acetylene black, and polyacrylic acid (PAA) are fully stirred and mixed evenly in a deionized water solvent system according to a weight ratio of 95:1.2:3.8, they are coated on the current collector, dried, cold-pressed, and slit to obtain a negative electrode sheet. Exemplarily, the negative electrode current collector includes copper foil.

[0113] When coating the negative electrode active material on the copper foil above, the coating weight is 9.74 mg / cm 2 , and a definite value is selected within the range of 0 - 100 wt% for the proportion of the Si-containing anode material in the composite product, so that the specific capacity a of the negative electrode sheet is 1500 mAh / g.

[0114] By controlling the gap PA gap between the negative electrode plate and the packaging film, the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode plate is w1, and the length is h1, and the gap PA gap is: gw=1.9mm, gh=3mm, and after full charge, the width of the negative electrode plate is w2, and the length is h2, the elongation of the negative electrode plate is yw=(w2-w1) / w1=1.80%, yh=(h2-h1) / h1=2.90%, and yw×a=27mAh / g, yh×a=43.5mAh / g.

[0115] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0116] Embodiment 18

[0117] The difference from Example 17 is that the gap PA gap between the negative electrode plate and the packaging film is: gw = 2 mm, gh = 3.1 mm, that is, the gap in the length direction becomes larger, and the gap in the width direction also becomes larger. The gram capacity a of the negative electrode plate is the same as that of Example 17, which is 1500 mAh / g, and the elongation of the negative electrode plate is the same as that of Example 17, that is, yw = (w2-w1) / w1 = 1.80%, yh = (h2-h1) / h1 = 2.90%, and yw×a = 27 mAh / g, yh×a = 43.5 mAh / g.

[0118] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0119] Embodiment 19

[0120] The difference from Example 17 is that the tensile strength f0 of the current collector in the negative electrode sheet increases when the battery is shipped, for example, f increases from 100 MPa to 400 MPa, and the gap PA gap between the negative electrode sheet and the packaging film is controlled so that the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode sheet is w1, and the length is h1, and the gap PA gap is: gw=1.7mm, gh=2.8mm, and after full charge, the width of the negative electrode sheet is w2, and the length is h2, and the elongation of the negative electrode sheet is yw=(w2-w1) / w1=1.70%, yh=(h2-h1) / h1=2.80%, and yw×a=25.5mAh / g, yh×a=42mAh / g.

[0121] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0122] Comparative Example 1

[0123] The difference from Example 1 is that by controlling the gap PA gap between the negative electrode pole piece and the packaging film, the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode pole piece is w1, and the length is h1, the gap PA gap is: gw=1.0mm, gh=1.8mm, and after full charge, the width of the negative electrode pole piece is w2, the length is h2, the elongation of the negative electrode pole piece is yw=(w2-w1) / w1=6.00%, yh=(h2-h1) / h1=9.00%, and yw×a=27mAh / g, yh×a=40.5mAh / g.

[0124] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0125] Comparative Example 2

[0126] The difference from Example 1 is that by controlling the gap PA gap between the negative electrode pole piece and the packaging film, the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode pole piece is w1, and the length is h1, the gap PA gap is: gw=0.8mm, gh=1.5mm, and after full charge, the width of the negative electrode pole piece is w2, the length is h2, the elongation of the negative electrode pole piece is yw=(w2-w1) / w1=0.40%, yh=(h2-h1) / h1=1.50%, and yw×a=1.8mAh / g, yh×a=6.75mAh / g.

[0127] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0128] Comparative Example 3

[0129] The difference from Example 1 is that by controlling the gap PA gap between the negative electrode pole piece and the packaging film, the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode pole piece is w1, and the length is h1, the gap PA gap is: gw=0.8mm, gh=1.5mm, and after full charge, the width of the negative electrode pole piece is w2, the length is h2, the elongation of the negative electrode pole piece is yw=(w2-w1) / w1=0.2%, yh=(h2-h1) / h1=1.00%, and yw×a=0.9mAh / g, yh×a=4.5mAh / g.

[0130] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0131] Comparative Example 4

[0132] The difference from Example 1 is that by controlling the gap PA gap between the negative electrode pole piece and the packaging film, the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode pole piece is w1, and the length is h1, the gap PA gap is: gw=3.3mm, gh=5.5mm, and after full charge, the width of the negative electrode pole piece is w2, the length is h2, the elongation of the negative electrode pole piece is yw=(w2-w1) / w1=0.4%, yh=(h2-h1) / h1=1.50%, and yw×a=1.8mAh / g, yh×a=6.75mAh / g.

[0133] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0134] Comparative Example 5

[0135] The difference from Example 5 is that by controlling the gap PA gap between the negative electrode pole piece and the packaging film, the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode pole piece is w1, and the length is h1, the gap PA gap is: gw=1.3mm, gh=2.2mm, and after full charge, the width of the negative electrode pole piece is w2, and the length is h2, the elongation of the negative electrode pole piece is yw=(w2-w1) / w1=6.00%, yh=(h2-h1) / h1=9.00%, and yw×a=36mAh / g, yh×a=54mAh / g.

[0136] After obtaining the above-mentioned lithium-ion full battery, a battery performance test was performed, including a battery cycle performance test. The test results are detailed in Table 1.

[0137] Comparative Example 6

[0138] The difference from Example 5 is that by controlling the gap PA gap between the negative electrode pole piece and the packaging film, the width of the full battery after half charge is w0, and the length is h0, the width of the negative electrode pole piece is w1, and the length is h1, the gap PA gap is: gw=1.3mm, gh=2.2mm, and after full charge, the width of the negative electrode pole piece is w2, and the length is h2, the elongation of the negative electrode pole piece is yw=(w2-w1) / w1=13.00%, yh=(h2-h1) / h1=21.00%, and yw×a=78mAh / g, yh×a=126mAh / g.

[0139] After obtaining the above-mentioned lithium-ion full battery, the battery performance test was carried out, including the battery cycle performance test. The test results are shown in Table 1

[0140] Table 1

[0141]

[0142]

[0143] As can be seen from Table 1, Example 1: When the gram capacity of the negative electrode sheet is 450mAh / g, and the gap gw is 1mm, the gap gh is 1.8mm, the elongation yw in the width direction of the negative electrode sheet is 0.4%, and the elongation yh in the length direction of the negative electrode sheet is 1.5%, the P-Agap is sufficiently designed (that is, even if the negative electrode sheet is extended in the X and Y directions, the PA gap design can make the negative electrode sheet and the packaging film not interfere), and the cycle performance is met. Example 2: The type of Si material is the same as that of Example 1, and the gram capacity is the same, so the elongation is consistent with that of Example 1. The PA gap design is reduced (that is, the gap is reduced), and the cycle performance can be met, and the VED is improved. Example 3: The type of Si material is the same as that of Example 1, and the gram capacity is the same, so the elongation is consistent with that of Example 1. The PA gap design is further sufficient (that is, the gap is increased), which can improve the cycle performance, but the VED is reduced. Example 4: When the tensile strength of the negative electrode current collector is relatively strong, the elongation of the electrode sheet can be reduced, thereby improving the cycle performance.

[0144] Example 5: The gram capacity of the negative electrode plate is increased to 600mAh / g, and the elongation of the plate changes (such as increases), such as the elongation yw of the negative electrode plate in the width direction is 1.00%, and the elongation yh of the negative electrode plate in the length direction is 2.00%. Correspondingly, the P-Agap design changes, such as the gap gw is 1.3mm, and the gap gh is 2.2mm, to meet the cycle performance. Example 6: The type of Si material is the same as that of Example 5, and the gram capacity is the same, so the elongation is also consistent with that of Example 5. The PA gap design is reduced (that is, the gap is reduced), which can also meet the cycle performance, and the VED is improved. Example 7: When the tensile strength of the negative electrode current collector is strong, the elongation of the plate can be reduced, and then the PA gap design can be reduced, and the cycle performance can be improved.

[0145] Example 8: The gram capacity of the negative electrode plate is increased to 850 mAh / g, and the elongation of the plate changes (such as increases), such as the elongation yw of the negative electrode plate in the width direction is 1.30%, and the elongation yh of the negative electrode plate in the length direction is 2.30%. Correspondingly, the P-Agap design changes, such as the gap gw is 1.5 mm, and the gap gh is 2.5 mm, to meet the cycle performance. Example 9: The type of Si material is the same as that of Example 8, and the gram capacity is the same, so the elongation is also consistent with that of Example 8. The PA gap design is increased (that is, the gap is increased), which meets the cycle performance, but the VED is reduced. Example 10: When the tensile strength of the negative electrode current collector is strong, the elongation of the plate can be reduced, and then the PA gap design can be reduced, and the cycle performance can be improved.

[0146] Example 11: The gram capacity of the negative electrode plate is increased to 1000mAh / g, and the elongation of the plate changes (such as increases), such as the elongation yw of the negative electrode plate in the width direction is 1.50%, and the elongation yh of the negative electrode plate in the length direction is 2.60%. Correspondingly, the P-Agap design changes, such as the gap gw is 1.6mm, and the gap gh is 2.7mm, to meet the cycle performance. Example 12: The type of Si material is the same as that of Example 11, and the gram capacity is the same, so the elongation is also consistent with that of Example 11. The PA gap design is increased (that is, the gap is increased), which meets the cycle performance, but the VED is reduced. Example 13: When the tensile strength of the negative electrode current collector is strong, the elongation of the plate can be reduced, and then the PA gap design can be reduced, and the cycle performance can be improved.

[0147] Example 14: The gram capacity of the negative electrode plate is increased to 1200mAh / g, and the elongation of the plate changes (such as increases), such as the elongation yw of the negative electrode plate in the width direction is 1.70%, and the elongation yh of the negative electrode plate in the length direction is 2.80%. Correspondingly, the P-Agap design changes, such as the gap gw is 1.7mm, and the gap gh is 2.8mm, to meet the cycle performance. Example 15: The type of Si material is the same as that of Example 14, and the gram capacity is the same, so the elongation is also consistent with that of Example 14, and the PA gap design is increased (that is, the gap is increased), which meets the cycle performance, but the VED is reduced. Example 16: When the tensile strength of the negative electrode current collector is strong, the elongation of the plate can be reduced, and then the PA gap design can be reduced, and the cycle performance can be improved.

[0148] Example 17: The gram capacity of the negative electrode plate is increased to 1500mAh / g, and the elongation of the plate changes (such as increases), such as the elongation yw of the negative electrode plate in the width direction is 1.80%, and the elongation yh of the negative electrode plate in the length direction is 2.90%. Correspondingly, the P-Agap design changes, such as the gap gw is 1.9mm, and the gap gh is 3mm, to meet the cycle performance. Example 18: The type of Si material is the same as that of Example 17, and the gram capacity is the same, so the elongation is also consistent with that of Example 17. The PA gap design is increased (that is, the gap is increased), which meets the cycle performance, but the VED is reduced. Example 19: When the tensile strength of the negative electrode current collector is strong, the elongation of the plate can be reduced, and then the PA gap design can be reduced, and the cycle performance can be improved.

[0149] It can be seen from Comparative Example 1 that although the gram capacity of the negative electrode plate is the same as that in Example 1, due to the different types of Si materials, for example, the negative electrode plate in Comparative Example 1 is made of a negative electrode material with larger expansion, which makes the elongation of the negative electrode plate larger. If the PA gap design remains unchanged, such as the gap gw is 1 mm and the gap gh is 1.8 mm, that is, the PA gap design is insufficient, resulting in poor cycle.

[0150] It can be seen from Comparative Example 2 that although the type and gram capacity of the negative electrode Si material are the same as those in Example 1, that is, the elongation of the negative electrode is also the same, if the PA gap is reduced, that is, the PA gap design is insufficient, it will also lead to cycle attenuation.

[0151] It can be seen from Comparative Example 3 that although the type and gram capacity of the negative electrode Si material are the same as those in Example 4, that is, the elongation of the negative electrode is also the same, if the PA gap is reduced, that is, the PA gap design is insufficient, it will also lead to cycle attenuation.

[0152] It can be seen from Comparative Example 4 that although the type and gram capacity of the negative electrode Si material are the same as those in Example 1, that is, the elongation of the negative electrode is also the same, if the PA gap is increased, that is, the PA gap is sufficiently designed, the cycle performance is better, but the VED loss is larger.

[0153] It can be seen from Comparative Example 5 that although the gram capacity of the negative electrode plate is the same as that of Example 5, due to the different types of Si materials, for example, the negative electrode plate in Comparative Example 5 is a negative electrode material with larger expansion, which makes the elongation of the negative electrode plate larger. If the PA gap design remains unchanged, such as the gap gw is 1.3 mm, and the gap gh is 2.2 mm, that is, the PA gap design is insufficient, resulting in interference between the packaging film (such as aluminum-plastic film) and the negative electrode plate, deformation of the battery cell, and film peeling of the plate.

[0154] It can be seen from Comparative Example 6 that although the gram capacity of the negative electrode plate is the same as that of Example 5, due to the different types of Si materials, for example, the negative electrode plate in Comparative Example 5 is a negative electrode material with larger expansion, which makes the elongation of the negative electrode plate very large. If the PA gap design remains unchanged, such as the gap gw is 1.3 mm, and the gap gh is 2.2 mm, that is, the PA gap design is insufficient, resulting in interference between the packaging film (such as aluminum-plastic film) and the negative electrode plate, deformation of the battery cell, film peeling of the plate, and tearing of the Cu current collector.

[0155] It should be noted that the gram capacity of other negative electrode sheets is the same as the above rules and will not be listed here one by one.

[0156] In summary, through the analysis of the above embodiments and comparative examples, it can be seen that by reasonably designing the P-A gap, the specific capacity of the negative electrode sheet, and the elongation rate of the negative electrode sheet, such as the specific capacity a of the negative electrode sheet satisfies: 400 mAh / g < a < 1500 mAh / g, the P-A gap satisfies 0 mm < gw < 3 mm, and 0 mm < gh < 5 mm; the elongation rate of the negative electrode sheet satisfies 0% < yw < 5%, and 0.1% < yh < 1.8%; and a and yw satisfy 0 mAh / g < yw × a < 75 mAh / g, and a and yh satisfy 0.4 mAh / g < yh × a < 120 mAh / g, a battery with high energy density can be obtained, while avoiding problems such as excessive elongation of the electrode sheet caused by negative electrode swelling, damage to the aluminum-plastic film caused by interference between the electrode sheet and the aluminum-plastic film, and capacity and cycle loss, thereby ensuring that the battery takes into account high capacity and cycle performance to the greatest extent.

[0157] As described above, the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application has been described in detail with reference to the foregoing embodiments, those of ordinary skill in the art should understand that: they can still modify the technical solutions described in the foregoing embodiments, or perform equivalent replacements for some of the technical features; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A lithium ion battery, characterized in that: It includes a battery cell, an electrolyte, and a packaging film. The battery cell and the electrolyte are located inside the packaging film. The battery cell includes a plurality of positive electrode plates, a plurality of negative electrode plates, and a plurality of separators. The positive electrode plates and the negative electrode plates are separated by the separators, and the positive electrode plates, the separators, and the negative electrode plates are laminated layer by layer in sequence. The electrolyte is filled between the positive electrode plates, the separators, and the negative electrode plates; When the lithium-ion battery is in the shipped state, the overall width of the full battery is w0, the length is h0, the width of the negative electrode plate is w1, the length is h1, and the gap gw in the width direction between the packaging film and the negative electrode plate is gw = w0 - w1, and the gap gh in the length direction is gh = h0 - h1. gw satisfies 0mm < gw < 3mm, and gh satisfies 0mm < gh < 5mm; When the lithium-ion battery is in the fully charged state, the width of the negative electrode plate is w2, the length is h2, and the elongation rate yw in the width direction of the negative electrode plate is yw = (w2 - w1) / w1, and the elongation rate yh in the length direction is yh = (h2 - h1) / h1; The negative electrode plate contains a silicon-based material. When the specific capacity per unit mass of the negative electrode plate is a, a and yw satisfy 0mAh / g < yw×a < 75mAh / g, and a and yh satisfy 0.4mAh / g < yh×a < 120mAh / g; Among them, 400mAh / g < a < 1500mAh / g.

2. The lithium-ion battery according to claim 1, characterized in that yw satisfies 0% < yw < 5%, and yh satisfies 0.1% < yh < 8%.

3. The lithium-ion battery according to claim 1, characterized in that When the battery is in the shipped state, the tensile strength of the current collector in the negative electrode plate is f0, and f0 satisfies 100Mpa < f0 < 600Mpa, and 0 < yw < 3%, 0.1% < yh < 5%.

4. The lithium-ion battery according to claim 3, characterized in that: After 700 cycles, the tensile strength of the current collector in the negative electrode plate is f1, and it satisfies 60% < f1 / f0 < 100%.

5. The lithium-ion battery according to claim 1, characterized in that: The packaging film is an aluminum-plastic film.

6. The lithium ion battery according to any one of claims 1 to 5, characterized in that: The silicon-based material includes at least one of nano-silicon, silicon oxide, silicon-carbon composite material, or silicon alloy material.

7. The lithium ion battery according to any one of claims 1 to 5, characterized in that: The positive active material of the positive electrode plate includes at least one of lithium cobaltate, lithium manganate, lithium iron phosphate, lithium nickelate, lithium nickel cobaltate, and lithium nickel cobalt manganate.

8. The lithium ion battery according to any one of claims 1 to 4, characterized in that: The material of the separator includes at least one of polyethylene, polypropylene, and polyvinylidene fluoride.