Preparation process of low-temperature-resistant battery
By baking and using low-temperature electrolyte in a high vacuum environment, combining specific materials such as magnification lithium cobalt oxide and nanoparticle modified graft polymer, the problem of instability of lithium-ion batteries in low-temperature environments is solved, and the problem of instability of lithium-ion batteries is achieved. The normal working performance of the battery in severe cold areas improves the low-temperature working efficiency.
Patent Information
- Application Number
- CN202410929576.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure BDA0004939233280000061 
Figure BDA0004939233280000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of low-temperature resistant battery technology, and in particular to a preparation process of a low-temperature resistant battery. Background Art
[0002] In the new energy era, lithium-ion batteries have been widely used. People have higher requirements for the charging and discharging performance of lithium-ion batteries in low-temperature environments, and hope to apply lithium-ion batteries to the cold northern regions or the wild, power vehicles or energy storage fields.
[0003] However, the current research on the low-temperature characteristics of lithium-ion batteries is significantly lagging behind. Conventional lithium battery products are only suitable for room temperature or an ambient temperature range of -10℃ to 60℃. When the ambient temperature is lower than -20℃, lithium-ion batteries can hardly discharge electricity or can only discharge a small amount of electricity, which cannot meet the normal working requirements of electrical equipment, so there is room for improvement. Summary of the invention
[0004] In order to improve the low temperature working performance of the battery, the present application provides a preparation process of a low temperature resistant battery.
[0005] The present application provides a preparation process for a low-temperature resistant battery using the following technical solution: A preparation process of a low temperature resistant battery comprises the following steps: The positive electrode sheet, the negative electrode sheet and the separator are wound to form a core, tested for short circuit, and after passing the test, they are loaded into an aluminum plastic film for packaging, tested again for short circuit, and after passing the test, angle pressing and vacuum baking are performed to obtain a semi-finished battery cell; Low-temperature electrolyte is injected into the semi-finished battery cell, and after vacuum packaging, formation and secondary packaging are carried out, and low-temperature resistant batteries are obtained after capacity division.
[0006] By baking in a high vacuum environment, the moisture in the semi-finished core can be fully removed, the stability of the electrolyte components can be improved, and thus the performance of the battery can be improved; by using low-temperature electrolyte, the working performance of the battery in a low-temperature environment can be greatly improved to meet the use needs in extremely cold areas.
[0007] Preferably, the preparation material of the positive electrode sheet includes rate-type lithium cobalt oxide.
[0008] Rate-type lithium cobalt oxide has high charge and discharge performance, stable structural performance, can improve the energy density of the battery, and efficiently convert energy.
[0009] Preferably, the separator is 1.5-2.5 mm wider than the positive electrode sheet, and the negative electrode sheet is 1-2 mm wider than the positive electrode sheet.
[0010] The winding structure ensures effective coating of the diaphragm on the negative electrode and the negative electrode on the positive electrode, eliminating the occurrence of short circuits and improving product production efficiency and product consistency.
[0011] Preferably, the low-temperature electrolyte comprises 10-20 parts of lithium hexafluorophosphate, 1-2 parts of a film-forming additive and 60-80 parts of a low-temperature solvent.
[0012] Film-forming additives help form the SEI film, which can improve the stability and density of the SEI film, so that the battery can maintain good working performance in a low-temperature environment and perform normal discharge work; low-temperature solvents have a low crystallization point and good ionic conductivity, can maintain low viscosity under low temperature conditions, and have high ion transfer efficiency, so that the battery maintains good low-temperature working performance.
[0013] Preferably, the raw materials for preparing the film-forming additive include nanoparticle-modified graft polymer and ionic liquid.
[0014] By compounding nanoparticle-modified grafted polymers and ionic liquids to obtain film-forming additives, the stability and density of the SEI film can be improved, thereby improving the low-temperature performance of the battery. Ionic liquids have good electrochemical properties and high safety. By grafting ionic liquids on the surface of nanoparticle-modified grafted polymers, the diffusion of lithium ions in the battery can be accelerated, the conductivity of the electrolyte can be improved, and the low-temperature working performance of the battery can be improved.
[0015] Preferably, the raw materials for preparing the nanoparticle-modified graft polymer include modified mesoporous alumina, polyethylene oxide and polysiloxane.
[0016] Modified mesoporous alumina is modified to improve its dispersibility and compatibility. Modified mesoporous alumina is dispersed in polymers, which can inhibit the crystallization of polymers and improve the conductivity of nanoparticle-modified grafted polymers. Polysiloxane has a low glass transition temperature and good chemical stability, which can improve the stability of nanoparticle-modified grafted polymers, promote the formation of SEI films with good stability and density, inhibit the formation of lithium dendrites, help the transfer of lithium ions, improve conductivity, and thus improve the low-temperature performance of the battery.
[0017] Preferably, the mass ratio of the modified mesoporous alumina, polyethylene oxide and polysiloxane is 0.4:1:(0.2-0.3).
[0018] The low-temperature resistant battery prepared according to the above mass ratio has good low-temperature working performance.
[0019] Preferably, the low temperature solvent includes 1,3-dioxolane, dimethyl carbonate and diethylene diether.
[0020] The low-temperature solvent obtained by compounding 1,3-dioxolane, dimethyl carbonate and diethylene diether has good low-temperature performance. These three solvents have high dielectric constants and low viscosities, which help to improve ion conductivity and battery discharge efficiency, thereby improving the low-temperature performance of the battery.
[0021] Preferably, the mass ratio of dimethyl carbonate, 1,3-dioxolane and diethylene diether is 1:(2-3):0.5.
[0022] The battery prepared according to the above mass ratio has good low-temperature performance.
[0023] In summary, the present application includes at least one of the following beneficial technical effects: 1. By baking in a high vacuum environment, the moisture in the semi-finished core can be fully removed, the stability of the electrolyte components can be improved, and the performance of the battery can be improved; by using low-temperature electrolyte, the working performance of the battery in a low-temperature environment can be greatly improved to meet the use needs in extremely cold areas.
[0024] 2. Film-forming additives help form the SEI film, which can improve the stability and density of the SEI film, so that the battery can maintain good working performance in a low temperature environment and perform normal discharge work; low-temperature solvents have a low crystallization point and good ionic conductivity, can maintain low viscosity under low temperature conditions, and have high ion transfer efficiency, so that the battery maintains good low-temperature working performance. DETAILED DESCRIPTION
[0025] The present application discloses a preparation process of a low temperature resistant battery. The present application is further described in detail below in conjunction with the examples: Example 1 Preparation of Nano-ion Modified Graft Polymers 20 kg of aluminum isopropoxide was dispersed in 40 L of ethanol to obtain an aluminum source dispersion, 20 kg of template P123 (CAS No.: 106392-12-5) was added to the aluminum source dispersion, and stirred at a speed of 500 r / min until completely dissolved, nitric acid was used to adjust the pH to 5, and the stirring was continued at a speed of 500 r / min for 30 min, and then placed in an 80°C blast drying oven for 8 h to obtain a dried solid, and the dried solid was ground and placed in a box-type resistance furnace at 2°C / min The temperature was raised to 600°C at a rate of 200 r / min, and calcined for 4 h in an air atmosphere. The calcined solid was taken out and tableted with a powder tablet press. The tablets were ground with a mortar and passed through a 500-mesh sieve to obtain mesoporous alumina. 8 kg of mesoporous alumina and 2 kg of 3-glycidyloxypropyltrimethoxysilane (CAS No.: 2530-83-8) were mixed and dispersed in 20 L of ethanol, and the mixture was stirred and reacted at a speed of 200 r / min for 2 h to obtain modified mesoporous alumina. After filtering, the mixture was dried in an oven at 80°C for 6 h to obtain modified mesoporous alumina.
[0026] 2.5 kg of modified mesoporous alumina is dispersed in 5 L of toluene to obtain an alumina dispersion; 1.25 kg of polysiloxane (CAS No.: 63148-57-2), 6.25 kg of polyethylene oxide (CAS No.: 68441-17-8) and 10 kg of toluene are mixed and dispersed, 20 mg of chloroplatinic acid catalyst is added dropwise to obtain a reactant, the alumina dispersion is added dropwise to the reactant, and the addition is completed within 1 hour. The reactant is stirred at a speed of 500 r / min, and reacted for 6 hours under nitrogen protection to obtain a product, the product is precipitated in n-hexane three times to remove impurities, and the solvent is removed by reduced pressure distillation to obtain a nano-ion modified graft polymer.
[0027] Preparation of film-forming additives 5 kg of nano-ion modified graft polymer and 5 kg of 1-vinyl-3-ethylimidazolium bromide (CAS No.: 81517-60-4) were mixed and dispersed in acetonitrile, and the mixture was stirred at a speed of 200 r / min for 12 hours to obtain a crude product. The crude product was rotary evaporated to remove the solvent and then dried in a high vacuum oven at 95° C. for 24 hours to obtain a film-forming additive.
[0028] Preparation of low temperature resistant batteries The positive electrode sheet, the negative electrode sheet and the separator are wound to form a core, and tested for short circuit. After passing the test, aluminum-plastic film is put into the core for packaging, and the short circuit is tested again. After passing the test, the corner is pressed, and then the core is placed in a high vacuum oven for vacuum baking to obtain a semi-finished battery cell; 10kg of lithium hexafluorophosphate, 1kg of film-forming additive and 60kg of low-temperature solvent are mixed, heated and stirred at 40°C and a speed of 200r / min to obtain an electrolyte; the mass ratio of 1,3-dioxolane, dimethyl carbonate and diethylene diether in the above electrolyte is 1:2:0.5; the low-temperature electrolyte is injected into the semi-finished battery cell, and after vacuum packaging, it is formed and repackaged, and a low-temperature resistant battery is obtained after capacity division.
[0029] Example 2 Preparation of Nano-ion Modified Graft Polymers Disperse 20 kg of aluminum isopropoxide in 40 L of ethanol to obtain an aluminum source dispersion, add 20 kg of template P123 to the aluminum source dispersion, stir at 500 r / min until completely dissolved, adjust the pH to 5 with nitric acid, continue stirring at 500 r / min for 30 min, then put it in an 80°C forced air drying oven for 8 h to obtain a dried solid, grind the dried solid and put it in a box-type resistance furnace and heat it to 600°C at a rate of 2°C / min, calcine it in an air atmosphere for 4 h, take out the calcined solid and press it with a powder tablet press, grind it with a mortar and pass it through a 500-mesh sieve to obtain mesoporous alumina; mix 8 kg of mesoporous alumina and 2 kg of 3-glycidyloxypropyltrimethoxysilane and disperse them in 20 L of ethanol, stir and react at 200 r / min for 2 h to obtain modified mesoporous alumina, filter and dry it in an oven at 80°C for 6 h to obtain modified mesoporous alumina.
[0030] 2.35 kg of modified mesoporous alumina is dispersed in 5 L of toluene to obtain an alumina dispersion; 1.77 kg of polysiloxane, 5.88 kg of polyethylene oxide and 10 kg of toluene are mixed and dispersed, 20 mg of chloroplatinic acid catalyst is added dropwise to obtain a reactant, the alumina dispersion is added dropwise to the reactant, and the addition is completed within 1 hour. The reactant is stirred at a speed of 500 r / min, and reacted for 6 hours under nitrogen protection to obtain a product. The product is precipitated in n-hexane three times to remove impurities, and the solvent is removed by reduced pressure distillation to obtain a nano-ion modified graft polymer.
[0031] Preparation of film-forming additives 5 kg of nano-ion modified graft polymer and 5 kg of 1-vinyl-3-ethylimidazolium bromide were dispersed in acetonitrile, stirred at 200 r / min for 12 h to obtain a crude product, the crude product was rotary evaporated to remove the solvent and dried in a high vacuum oven at 95° C. for 24 h to obtain a film-forming additive.
[0032] Preparation of low temperature resistant batteries The positive electrode sheet, the negative electrode sheet and the separator are wound to form a core, and tested for short circuit. After passing the test, an aluminum-plastic film is placed in the core for packaging. After the short circuit is tested again, the core is pressed after passing the test, and then the core is placed in a high vacuum oven for vacuum baking to obtain a semi-finished battery cell; 20 kg of lithium hexafluorophosphate, 2 kg of film-forming additives and 80 kg of low-temperature solvent are mixed, heated and stirred at 40°C and a speed of 200 r / min to obtain an electrolyte; the mass ratio of 1,3-dioxolane, dimethyl carbonate and diethylene diether in the above electrolyte is 1:3:0.5; the low-temperature electrolyte is injected into the semi-finished battery cell, and after vacuum packaging, it is formed and repackaged, and a low-temperature resistant battery is obtained after capacity division.
[0033] Example 3 Preparation of Nano-ion Modified Graft Polymers Disperse 20 kg of aluminum isopropoxide in 40 L of ethanol to obtain an aluminum source dispersion, add 20 kg of template P123 to the aluminum source dispersion, stir at 500 r / min until completely dissolved, adjust the pH to 5 with nitric acid, continue stirring at 500 r / min for 30 min, then put it in an 80°C forced air drying oven for 8 h to obtain a dried solid, grind the dried solid and put it in a box-type resistance furnace and heat it to 600°C at a rate of 2°C / min, calcine it in an air atmosphere for 4 h, take out the calcined solid and press it with a powder tablet press, grind it with a mortar and pass it through a 500-mesh sieve to obtain mesoporous alumina; mix 8 kg of mesoporous alumina and 2 kg of 3-glycidyloxypropyltrimethoxysilane and disperse them in 20 L of ethanol, stir and react at 200 r / min for 2 h to obtain modified mesoporous alumina, filter and dry it in an oven at 80°C for 6 h to obtain modified mesoporous alumina.
[0034] 2.29 kg of modified mesoporous alumina is dispersed in 5 L of toluene to obtain an alumina dispersion; 2 kg of polysiloxane, 5.71 kg of polyethylene oxide and 10 kg of toluene are mixed and dispersed, 20 mg of chloroplatinic acid catalyst is added dropwise to obtain a reactant, the alumina dispersion is added dropwise to the reactant, the addition is completed within 1 hour, the reactant is stirred at a speed of 500 r / min, and reacted for 6 hours under nitrogen protection to obtain a product, the product is precipitated in n-hexane three times to remove impurities, and the solvent is removed by reduced pressure distillation to obtain a nano-ion modified graft polymer.
[0035] Preparation of film-forming additives 5 kg of nano-ion modified graft polymer and 5 kg of 1-vinyl-3-ethylimidazolium bromide were dispersed in acetonitrile, stirred at 200 r / min for 12 h to obtain a crude product, the crude product was rotary evaporated to remove the solvent and dried in a high vacuum oven at 95° C. for 24 h to obtain a film-forming additive.
[0036] Preparation of low temperature resistant batteries The positive electrode sheet, the negative electrode sheet and the separator are wound to form a core, and tested for short circuit. After passing the test, an aluminum-plastic film is placed in the core for packaging. After the short circuit is tested again, the core is pressed after passing the test, and then the core is placed in a high vacuum oven for vacuum baking to obtain a semi-finished battery cell; 15 kg of lithium hexafluorophosphate, 1.5 kg of film-forming additives and 70 kg of low-temperature solvent are mixed, heated and stirred at 40°C and a speed of 200 r / min to obtain an electrolyte; the mass ratio of 1,3-dioxolane, dimethyl carbonate and diethylene diether in the above electrolyte is 1:2.5:0.5; the low-temperature electrolyte is injected into the semi-finished battery cell, and after vacuum packaging, it is formed and repackaged, and a low-temperature resistant battery is obtained after capacity division.
[0037] Example 4 Example 4 is based on Example 3. The only difference between Example 4 and Example 3 is that in Example 4, the amount of modified mesoporous alumina is 2.42 kg, the amount of polyethylene oxide is 6.06 kg, and the amount of polysiloxane is 1.52 kg.
[0038] Example 5 Example 5 is based on Example 3. The only difference between Example 5 and Example 3 is that in Example 5, the amount of modified mesoporous alumina is 2.22 kg, the amount of polyethylene oxide is 5.56 kg, and the amount of polysiloxane is 2.22 kg.
[0039] Example 6 Example 6 is based on Example 3. The only difference between Example 6 and Example 3 is that the mass ratio of 1,3-dioxolane, dimethyl carbonate and diethylene diether in the low-temperature solvent in Example 6 is 1:1.5:0.5.
[0040] Example 7 Example 7 is based on Example 3. The only difference between Example 7 and Example 3 is that the mass ratio of 1,3-dioxolane, dimethyl carbonate and diethylene diether in the low-temperature solvent in Example 7 is 1:3.5:0.5.
[0041] Example 8 Example 8 is based on Example 3. The only difference between Example 8 and Example 3 is that in Example 8, the rate-type lithium cobalt oxide used as the material for preparing the positive electrode sheet is replaced with lithium cobalt oxide.
[0042] Example 9 Example 9 is based on Example 3. The only difference between Example 9 and Example 3 is that in Example 9, the modified mesoporous alumina in the step of preparing the nanoparticle-modified graft polymer is replaced by mesoporous alumina.
[0043] Example 10 Example 10 is based on Example 3. The only difference between Example 10 and Example 3 is that in Example 10, no polysiloxane is added when preparing the nanoparticle-modified graft polymer.
[0044] Embodiment 11 Example 11 is based on Example 3. The only difference between Example 11 and Example 3 is that in Example 11, no ionic liquid is added in the step of preparing the film-forming additive.
[0045] Example 12 Example 12 is based on Example 3. The only difference between Example 12 and Example 3 is that in Example 12, the low-temperature solvent is replaced by ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate in a volume ratio of 3:4:3.
[0046] Comparative Example 1 Comparative Example 1 is based on Example 3, and the only difference between Comparative Example 1 and Example 3 is that the high vacuum oven in Comparative Example 1 is replaced by a conventional vacuum oven.
[0047] Performance testing The prepared low-temperature resistant battery was charged to 4.45V at 1C constant current and constant voltage at 25°C, with a cut-off current of 0.05C, and discharged to 3.0V at a rate of 1C, and the 1C discharge capacity at 25°C was recorded; then charged to 4.45V at 1C constant current and constant voltage, with a cut-off current of 0.05C, and after standing in a -40°C environment for 8h, discharged to 2.5V at a constant current of 0.5C, and the 0.5C discharge capacity at -40°C was recorded. The discharge efficiency and battery energy density of the low-temperature resistant battery at -40°C were calculated, and the discharge efficiency = 0.5C discharge capacity at -40°C / 1C discharge capacity at 25°C * 100%. Each sample was tested three times, and the average value was taken after measurement. The results are recorded in Table 1.
[0048] Table 1 Test results of discharge efficiency and battery energy density of low temperature resistant batteries It can be seen from Table 1 that the discharge efficiency of Examples 1-3 is greater than 68.9%, and the battery energy density is greater than 181Wh / kg, which shows that the low-temperature-resistant battery prepared in the present application has good low-temperature performance.
[0049] It can be seen from Table 1 that the only difference between Examples 4 and 5 and Example 3 is that the mass ratio of modified mesoporous alumina, polyethylene oxide and polysiloxane in Example 4 is 0.4:1:0.25, and the mass ratio of modified mesoporous alumina, polyethylene oxide and polysiloxane in Example 5 is 0.4:1:0.4. The discharge efficiency in Examples 4 and 5 is less than 67.2%, and the battery energy density is less than 179Wh / kg. The discharge efficiency in Example 3 is 75.4%, and the battery energy density is 187Wh / kg. Compared with Example 3, the low-temperature performance of the battery in Examples 4 and 5 is reduced. This is because the ratio of modified mesoporous alumina, polyethylene oxide and polysiloxane is not within the specified range. Too much or too little polysiloxane affects the ability of the electrolyte to transport lithium ions, thereby affecting the conductivity, so that the low-temperature performance of the battery is reduced.
[0050] As can be seen from Table 1, the only difference between Examples 6 and 7 and Example 3 is that the mass ratio of 1,3-dioxolane, dimethyl carbonate and diethylene diether in the low-temperature solvent in Example 6 is 1:1.5:0.5, and the mass ratio of 1,3-dioxolane, dimethyl carbonate and diethylene diether in the low-temperature solvent in Example 7 is 1:3.5:0.5. The discharge efficiency in Examples 6 and 7 is less than 65.7%, and the battery energy density is less than 175Wh / kg. Compared with Example 3, the low-temperature performance of the battery in Examples 6 and 7 is reduced. This is because the ratio of dioxolane, dimethyl carbonate and diethylene diether is not within the specified range. The ratio of the low-temperature solvent affects the ability of the electrolyte to transport lithium ions and the viscosity under low-temperature conditions. The low-temperature solvent that destroys the ratio decreases the ion transmission efficiency in a low-temperature environment, thereby reducing the low-temperature performance of the battery.
[0051] It can be seen from Table 1 that the only difference between Example 8 and Example 3 is that in Example 8, the rate-type lithium cobalt oxide of the positive electrode sheet preparation material is replaced by lithium cobalt oxide, the discharge efficiency in Example 8 is 62.4%, and the battery energy density is 169Wh / kg. Compared with Example 3, Example 8 has a reduced low-temperature performance of the battery. This is because the rate-type lithium cobalt oxide is replaced by lithium cobalt oxide, the charge and discharge performance of lithium cobalt oxide is reduced, the structural stability is reduced compared to the high-rate lithium cobalt oxide, the energy density of the battery is reduced, and thus the low-temperature performance of the battery is reduced.
[0052] As can be seen from Table 1, the only difference between Examples 9, 10, and 11 and Example 3 is that in Example 9, the modified mesoporous alumina in the step of preparing the nanoparticle-modified grafted polymer is replaced by mesoporous alumina, in Example 10, no polysiloxane is added when preparing the nanoparticle-modified grafted polymer, and in Example 11, no ionic liquid is added in the step of preparing the film-forming additive. The discharge efficiency in Examples 9, 10, and 11 is less than 61.5%, and the battery energy density is less than 168Wh / kg. Compared with Example 3, the low-temperature performance of the battery in Examples 9, 10, and 11 is reduced. This is because the preparation components of the film-forming additive are replaced. The modified mesoporous alumina is replaced by mesoporous alumina, and the dispersibility of the mesoporous alumina is reduced, which in turn affects the film-forming performance and lithium ion transport performance. Without adding polysiloxane or ionic liquid, the stability of the film-forming additive is reduced, which affects the formation of the SEI film, thereby reducing the low-temperature performance of the battery.
[0053] As can be seen from Table 1, the only difference between Example 12 and Example 3 is that in Example 12, the low-temperature solvent is replaced with ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate in a volume ratio of 3:4:3. The discharge efficiency in Example 12 is 55.7%, and the battery energy density is 159Wh / kg. Compared with Example 3, Example 12 has a decreased low-temperature performance of the battery. This is because the low-temperature solvent is replaced with a composite solvent of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate, and the carbonate series solvent has poor low-temperature performance. Under low-temperature conditions, the viscosity increases and the ion transfer efficiency decreases, thereby reducing the low-temperature performance of the battery.
[0054] It can be seen from Table 1 that the only difference between Comparative Example 1 and Example 3 is that the high vacuum oven is replaced by a conventional vacuum oven in Comparative Example 1, the discharge efficiency in Comparative Example 1 is 51.1%, and the battery energy density is 151Wh / kg. Compared with Example 3, the low-temperature performance of the battery in Comparative Example 1 is significantly reduced. This is because the high vacuum oven is replaced by a conventional vacuum oven, which reduces the effect of removing moisture from the battery cell, affects the stability of the electrolyte, and thus the low-temperature performance of the battery is significantly reduced.
[0055] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A preparation process for a low temperature resistant battery, characterized in that: The steps include: The positive electrode sheet, the negative electrode sheet and the separator are wound to form a core, tested for short circuit, and after passing the test, they are loaded into an aluminum plastic film for packaging, tested again for short circuit, and after passing the test, angle pressing and vacuum baking are performed to obtain a semi-finished battery cell; Low-temperature electrolyte is injected into the semi-finished battery cell, and after vacuum packaging, formation and secondary packaging are carried out, and low-temperature resistant batteries are obtained after capacity division.
2. The preparation process of a low temperature resistant battery according to claim 1, characterized in that: The preparation material of the positive electrode sheet includes rate-type lithium cobalt oxide.
3. The preparation process of a low temperature resistant battery according to claim 1, characterized in that: The separator is 1.5-2.5 mm wider than the positive electrode sheet, and the negative electrode sheet is 1-2 mm wider than the positive electrode sheet.
4. The process for preparing a low temperature resistant battery according to claim 1, characterized in that: The low-temperature electrolyte comprises 10-20 parts of lithium hexafluorophosphate, 1-2 parts of a film-forming additive and 60-80 parts of a low-temperature solvent.
5. The process for preparing a low temperature resistant battery according to claim 4, characterized in that: The raw materials for preparing the film-forming additive include nano-particle-modified graft polymer and ionic liquid.
6. The process for preparing a low temperature resistant battery according to claim 5, characterized in that: The raw materials for preparing the nanoparticle modified graft polymer include modified mesoporous aluminum oxide, polyethylene oxide and polysiloxane.
7. The process for preparing a low temperature resistant battery according to claim 6, characterized in that: The mass ratio of the modified mesoporous alumina, polyethylene oxide and polysiloxane is 0.4:1:(0.2-0.3).
8. The process for preparing a low temperature resistant battery according to claim 4, characterized in that: The low temperature solvents include 1,3-dioxolane, dimethyl carbonate and diethylene diether.
9. The process for preparing a low temperature resistant battery according to claim 8, characterized in that: The mass ratio of the dimethyl carbonate, 1,3-dioxolane and diethylene diether is 1:(2-3):0.5.