Manganese titanate-containing fischer-tropsch catalysts and methods of making and using same
By forming manganese titanate on titanium dioxide-supported catalyst and cobalt treatment, the existing Fischer-Tropsch catalysts are solved, and a high stability and selectivity catalyst is achieved, suitable for efficient formation of chain hydrocarbons and Low oxygenated compounds.
Patent Information
- Application Number
- CN202280092381.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-23
- Filing Date
- 2022-12-22
- Publication Date
- 2024-11-05
AI Technical Summary
The existing Fischer-Tropsch catalysts are prone to sintering and degradation at high temperatures, resulting in a decrease in catalytic activity and selectivity, and it is difficult to control the formation of high proportions of chain hydrocarbons and low proportions of oxygen-containing compounds.
Using titanium dioxide-supported catalyst precursor, by depositing manganese on the support and converting it into manganese titanate (MnTiO3), reducing treatment at high temperatures to form a catalyst with high stability and selectivity, and at a suitable temperature and atmosphere. Cobalt impregnation and calcination are carried out to adjust the structure and properties of the catalyst.
The stability and activity of the catalyst are improved, the selectivity of oxygen-containing compounds is reduced, the selectivity of chain hydrocarbon products is maintained, the life of the catalyst is extended, and the construction cost of the reactor is reduced.
Smart Images

Figure BDA0005005795530000141 
Figure BDA0005005795530000142 
Figure BDA0005005795530000143
Abstract
Description
[0001] Public background Technical Field
[0002] The present disclosure relates to a Fischer-Tropsch catalyst containing manganese titanate, a preparation method thereof and uses thereof. Background Art
[0003] The conversion of synthesis gas (i.e. a mixture of carbon monoxide and hydrogen, also known as syngas) to hydrocarbons by the Fischer-Tropsch process has been known for decades, but has historically lagged behind other hydrocarbon synthesis technologies. The growing importance of alternative energy sources has led to a renewed interest in the Fischer-Tropsch (FT) process because it enables a direct and environmentally acceptable route to high quality fuels and feedstock chemicals.
[0004] The FT process is known for producing straight chain hydrocarbons for fuels, as well as oxygenates that can be used for fuels and also serve as valuable feedstock chemicals. Hydrocarbon fuels derived from the FT process are generally better able to meet increasingly stringent environmental regulations than conventional refinery-produced fuels because FT-derived fuels generally have lower levels of sulfur, nitrogen, and aromatic compounds that contribute to potent pollutants such as SO2, NO x The resulting alcohols and other oxygenates can also be used as reagents in other processes, such as in the synthesis of lubricants.
[0005] Various transition metals have been identified as having catalytic activity for the conversion of synthesis gas to hydrocarbons and their oxygenated derivatives. In particular, cobalt, nickel and iron have been studied, usually in combination with support materials, the most common of which are alumina, silica and carbon.
[0006] In a typical preparation of a supported cobalt-containing FT synthesis catalyst, a solid support material is contacted with a solution of a soluble cobalt compound, such as cobalt nitrate. The impregnated support is then calcined and / or oxidized to form a cobalt oxide, typically one or more of CoO, Co2O3 or Co3O4, sometimes in combination with an oxide of one or more promoters. Such oxides typically have poor FT catalytic activity and must be reduced to form a preferred catalytically active cobalt metal species. The properties of the cobalt metal formed in combination with an optional promoter can have a significant effect on catalyst activity and selectivity. In addition, certain catalyst compositions are known to sinter and degrade over time to impair catalyst performance.
[0007] Therefore, there is a need to develop improved Fischer-Tropsch catalysts and methods for their preparation. Summary of the invention
[0008] The inventors have developed a catalyst composition and method for making the same that enables high manganese loadings and low oxygenate selectivity. This results in improved catalyst stability and activity while maintaining control over the selectivity of the Fischer-Tropsch reaction, for example, to provide a desired high proportion of paraffins and a low proportion of oxygenates such as alcohols. Advantageously, the catalyst precursor can be prepared ex situ and then, in certain embodiments, followed by a subsequent cobalt impregnation step to produce the Fischer-Tropsch catalyst.
[0009] Thus, in one aspect, the present disclosure provides a titanium dioxide supported Fischer-Tropsch catalyst precursor comprising manganese in the range of 1 wt% to 50 wt% calculated as manganese (0); wherein at least 10 atomic % of the manganese is in the form of manganese titanate (i.e., MnTiO3) as measured by x-ray diffraction, and preferably at least 25%, more preferably at least 50%, and most preferably at least 75% of the manganese is in the form of MnTiO3. Any unconverted manganese species may be in the form of manganese oxides, such as MnO, Mn2O3, Mn3O4, MnO2, but may also be in the form of MnTi2O4 or Mn2TiO4 spinel.
[0010] In another aspect, the present disclosure provides a method of producing a titania-supported Fischer-Tropsch catalyst support, such as a catalyst support precursor as otherwise described herein, the method comprising:
[0011] providing a first support precursor comprising a manganese salt disposed on a titania support, wherein the first catalyst precursor is free of cobalt; and optionally calcining in an oxygen-containing atmosphere;
[0012] The support precursor is contacted with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a titania-supported Fischer-Tropsch catalyst precursor in which at least 10 atomic % of the manganese is present as MnTiO 3 .
[0013] Other aspects of the disclosure will be apparent to those skilled in the art using alternative techniques to X-ray diffraction, such as beamline X-ray adsorption techniques (EXAFS / XANES) or beamline X-ray diffraction as a more accurate method of observing and quantifying the phases formed.
[0014] In another aspect, the present disclosure provides for producing a titanium dioxide-supported Fischer-Tropsch catalyst precursor, the method comprising:
[0015] a) providing a first catalyst support precursor comprising a manganese salt disposed on a titanium dioxide support, wherein the first catalyst precursor does not contain cobalt; and optionally calcining the first catalyst support precursor in an oxygen-containing atmosphere;
[0016] b) contacting the first catalyst support precursor with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a titania-supported Fischer-Tropsch catalyst precursor in which at least 10 atomic % of the manganese is present as MnTiO 3 ,
[0017] c) contacting the catalyst precursor with a decomposable cobalt salt and calcining at a temperature in the range of 200° C. to 450° C. in an oxygen-containing atmosphere;
[0018] d) reducing the catalyst precursor with a reducing gas at a temperature of no greater than 350° C. to form a titania-supported Fischer-Tropsch catalyst, wherein at least 10 atomic % of the manganese of the final catalyst is present as MnTiO 3 .
[0019] In another aspect, the present disclosure provides a method for producing a Fischer-Tropsch catalyst, the method comprising:
[0020] providing a Fischer-Tropsch catalyst precursor as otherwise described herein;
[0021] impregnating the catalyst precursor with a decomposable cobalt salt;
[0022] The impregnated catalyst precursor is calcined at a temperature in the range of 200°C to 450°C.
[0023] In another aspect, the present disclosure provides a method for producing hydrocarbons, the method comprising contacting a supported Fischer-Tropsch catalyst containing manganese titanate containing at least 1 wt. % cobalt and 1 wt. % manganese, such as a catalyst as otherwise described herein, or a catalyst prepared by a method as otherwise described herein, with a gaseous reaction mixture comprising H2 and CO in a ratio ranging from 1:1 to 3:1, wherein the method has a selectivity to alcohols of not more than 10% (e.g., not more than 8%, or not more than 6%, or not more than 5%).
[0024] In another aspect, the present disclosure provides a method for controlling the selectivity of a Fischer-Tropsch catalyst, the method comprising:
[0025] (i) providing a titanium dioxide-supported Fischer-Tropsch synthesis catalyst precursor comprising manganese in an amount of at least 1 wt % calculated as manganese (0); and
[0026] (ii) contacting the catalyst with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a second catalyst precursor in which at least 10 atomic % of the manganese is present as MnTiO 3 ;
[0027] (iii) impregnating the second catalyst precursor with a cobalt salt;
[0028] (iv) calcining at a temperature in the range of 200°C to 450°C;
[0029] (v) contacting the calcined catalyst with a reducing gas at a temperature of no greater than 350° C. (e.g., no greater than 300° C.) to produce a Fischer-Tropsch catalyst, wherein
[0030] The selectivity of the Fischer-Tropsch catalyst to alcohols is no more than 50% of the selectivity of an equivalent catalyst to alcohols contacted with the reducing gas in step (ii) at a temperature of 300° C. for the same amount of time. For example, the performance of the catalysts under FT conditions such as 30 barg and a H2:CO ratio of 2:1 is compared, wherein the temperature or flow rate is adjusted to match the conversion to 40-60%.
[0031] Other aspects of the present disclosure will be apparent to those skilled in the art based on the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a schematic diagram of a reactor suitable for the process described herein, wherein a reducing gas is fed (101) onto a catalyst bed (120) for conversion to MnTiO3. Optionally, the outlet gas (104) may be recycled back into the feed (103).
[0033] Figure 2 X-ray diffraction patterns of three catalyst support examples in which MnTiO3 was formed are shown.
[0034] Figure 3 Shown are X-ray diffraction patterns of support materials calcined in air vs. treated with hydrogen.
[0035] Figure 4 X-ray diffraction of the reduced support impregnated with cobalt and calcined, and the air calcined analogue showing loss of the crystal structure of the MnTiO3 phase. DETAILED DESCRIPTION
[0036] The present disclosure relates in various aspects to Fischer-Tropsch catalyst compositions comprising manganese titanate. Generally, the addition of a promoter has the effect of changing the selectivity and activity of the catalyst. For example, in a typical cobalt-containing Fischer-Tropsch catalyst, manganese (as MnO x The presence of manganese in the form of manganese has the effect of increasing the selectivity to oxygenates such as alcohols relative to hydrocarbons. However, the inventors have noted that the inclusion of manganese in the Fischer-Tropsch catalyst can provide several advantageous effects, including reduced thermal sintering and catalyst damage, increased catalyst life stability, increased chain growth capacity and low methane selectivity. Therefore, the inventors have sought a method to separate these technical effects, such as providing low oxygenate selectivity, while maintaining increased catalyst stability.
[0037] Surprisingly, the inventors have found that at least a portion of the manganese deposited on the titanium dioxide carrier is converted into manganese titanate to produce a catalyst material having reduced oxygen-containing compound selectivity but maintaining improved catalyst stability. The carrier loaded with manganese titanate can be prepared non-in situ, and these properties can be substantially maintained throughout the catalyst life. In various embodiments as described herein, this conversion is achieved by high temperature treatment of the manganese species deposited on the titanium dioxide carrier so that the manganese species is at least partially converted into manganese titanate (i.e., MnTiO3). Without wishing to be bound by theory, it is currently believed that manganese titanate contributes to favorable structural properties while being largely inert to the Fischer-Tropsch synthesis reaction. Therefore, the disclosed catalyst and its method of manufacture are surprisingly able to obtain certain beneficial qualities of manganese inclusions while maintaining the ability to adjust the selectivity of the catalyst to paraffin products.
[0038] In addition, it has been surprisingly found that the manganese titanate phase formed due to hydrogen reduction at greater than 350°C is reversible. In addition, it has been determined that calcination in air can be used to at least partially decompose the MnTiO3 phase back to manganese oxide. These processes advantageously enable precise adjustment of the MnTiO3 and manganese oxide content to adjust the catalyst properties. Therefore, in some embodiments, the method as otherwise described herein further comprises calcining the support, catalyst precursor or catalyst containing MnTiO3 in air. For example, calcination can be to convert at least a portion of the MnTiO3 into MnO (e.g., at least 10 atomic % or at least 20 atomic %).
[0039] Advantageously, the catalyst prepared as described herein can be manufactured in two steps, wherein the formation of manganese titanate is carried out separately from the cobalt impregnation. This enables the ex situ formation of manganese titanate. Since the formation of manganese titanate requires a temperature of at least 350° C., manganese conversion can be carried out in a separate dedicated reactor. After the cobalt impregnation, calcination and final reduction can be carried out at lower temperatures in a typical reactor lacking metallurgy dedicated to high temperature operation. This can reduce the capital cost in the reactor configuration.
[0040] Of particular note is the re-reduction of the catalyst in the presence of cobalt, where the reduction process can be completed at less than 350°C so that the cobalt oxide is reduced and reforms the manganese titanate phase, thereby avoiding the need to reach the high temperatures required for the original MnTiO3 phase formation.
[0041] Accordingly, in one aspect, the present disclosure provides a titanium dioxide-supported Fischer-Tropsch catalyst precursor comprising a titanium dioxide carrier; and manganese in a range of 1 wt % to 50 wt % calculated as manganese (0) disposed on the titanium dioxide carrier; wherein at least 10 atomic % of the manganese is in the form of manganese titanate (i.e., MnTiO3) as measured by x-ray diffraction.
[0042] The titanium dioxide supported Fischer-Tropsch catalyst precursor is formed prior to the addition of cobalt. Thus, in various embodiments as otherwise described herein, the catalyst precursor does not contain cobalt. For example, in certain embodiments, the catalyst precursor does not contain cobalt, copper or iron. In specific embodiments, the catalyst precursor does not contain other transition metals other than titanium and manganese.
[0043] The percentage of manganese in the form of manganese titanate can be adjusted by the technician according to the present disclosure. It is not intended to be bound by theory, but it is believed that increasing the proportion of manganese in the form of manganese titanate will reduce the oxygen-containing compound selectivity of the catalyst. For example, in various embodiments as described in addition herein, as measured by X-ray diffraction, at least 15 atomic % (e.g., at least 20 atomic %, or at least 30 atomic %, or at least 40 atomic %) of manganese is in the form of MnTiO3. In various embodiments as described in addition herein, as measured by X-ray diffraction, at least 50 atomic % (e.g., at least 60 atomic %, or at least 70 atomic %, or at least 80 atomic %) of manganese is in the form of MnTiO3. In various embodiments as described in addition herein, as measured by x-ray diffraction, at least 90 atomic % (e.g., at least 95 atomic % or at least 98 atomic %) of manganese is in the form of MnTiO3. A person of ordinary skill in the art can provide reduction conditions (e.g., by increasing time and / or temperature) to provide the desired ratio of manganese titanate based on the disclosure herein.
[0044] However, in some embodiments, it may be advantageous to provide a portion of the manganese in a form other than manganese titanate. For example, one of ordinary skill in the art may select synthesis conditions so that a portion of the manganese remains as a catalytically active species, such as MnO. Accordingly, in some embodiments as otherwise described herein, no more than 99 atomic % (e.g., no more than 95 atomic %, or no more than 90 atomic %, or no more than 85 atomic %, or no more than 80 atomic %) of the manganese is in the form of MnTiO3 as measured by X-ray diffraction. In various embodiments as otherwise described herein, less than 5 atomic % of the manganese is in the form of MnO as measured by X-ray diffraction. For example, in certain embodiments, less than 3 atomic %, or less than 2 atomic %, or less than 1.5 atomic % of the manganese is in the form of MnO as measured by X-ray diffraction or a suitable X-ray technique.
[0045] Catalyst compositions and catalyst precursor compositions described herein include manganese in various loadings selected by those of ordinary skill in the art. Manganese loading is determined as the total amount of manganese present in all manganese-containing species (including, for example, manganese titanate, manganese oxide, and manganese metal). In various embodiments as described herein in addition, manganese is present in an amount of at least 0.5% by weight. For example, in a particular embodiment, manganese is present in an amount of at least 1% by weight (e.g., at least 1.5% by weight or at least 2% by weight). Advantageously, the present invention allows for relatively high manganese loadings while controlling the effect of manganese on the selectivity of Fischer-Tropsch synthesis products. Therefore, the technician will recognize that the upper limit of manganese loading is impractical. For example, in some embodiments, manganese is present in an amount of not more than 50% by weight, such as not more than 40% by weight, or not more than 30% by weight in the catalyst composition or catalyst precursor. In various embodiments as described herein in addition, manganese is present in an amount in the range of 1% by weight to 15% by weight, such as 1-10% by weight, or 1-8% by weight, or 1-5% by weight. In various embodiments as further described herein, manganese is present in an amount in the range of 2 to 50 wt %, for example 2-30 wt %, or 2-20 wt %, or 2-15 wt %. In various embodiments as further described herein, manganese is present in an amount in the range of 4 to 30 wt %, for example 4-20 wt % or 4-15 wt %. In various embodiments as further described herein, manganese is present in an amount in the range of 5 to 25 wt %, for example 5-15 wt %, or 5-12 wt %, or 5-10 wt %. Manganese loading is calculated as manganese (0).
[0046] Advantageously, manganese (regardless of their form, such as metal, oxide or mixed oxide) is disposed on a titania support. The titania support includes at least 50% by weight of titania. In various embodiments as described herein in addition, the titania support comprises at least 80% by weight of titania, such as at least 85% by weight or at least 90% by weight of titania. In various embodiments, the titania support comprises at least 95% by weight of titania, such as at least 98% by weight of titania. In some embodiments, the titania support is substantially entirely titania (e.g., titania except for negligible impurities). In various specific embodiments, the titania support comprises not more than 5% by weight (e.g., not more than 1% by weight or not more than 0.5% by weight) of silica, alumina, ceria, zirconium oxide and zinc oxide in total. The titania support can be provided in various forms, such as as extrudates, powders or microspheres.
[0047] Without wishing to be bound by theory, it is presently believed that at least a portion of the manganese titanate forms a solid solution with the titanium dioxide support. Thus, when discussing the composition of the support herein, the proportions are understood to exclude any manganese titanate species.
[0048] The term "disposed on" does not imply a particular arrangement. The inventors recognize that the cobalt and manganese may be "disposed on" the titania support in a variety of ways, such as by impregnation (eg, incipient wetness technique), precipitation, or coextrusion techniques.
[0049] In another aspect, the present disclosure provides a method of producing a titanium dioxide-supported Fischer-Tropsch catalyst precursor, such as a catalyst as otherwise described herein, the method comprising:
[0050] providing a support precursor comprising a manganese salt disposed on a titania support;
[0051] The support precursor is contacted with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a titania-supported Fischer-Tropsch catalyst precursor in which at least 10 atomic % of the manganese is present as MnTiO 3 .
[0052] The inventors have determined that a high temperature reduction process can produce a catalyst support suitable for subsequent impregnation with cobalt. The resulting catalyst has a relatively high selectivity for paraffins and a low selectivity for oxygen-containing compounds such as alcohols. Thus, the catalyst can enjoy the structural benefits of the presence of manganese without the sometimes undesirable formation of alcohols. The inventors have associated this with the formation of a manganese titanate phase (MnTiO3).
[0053] Thus, contact of the first catalyst precursor with the reducing gas can be carried out at various temperatures for at least a time sufficient to provide the desired level of manganese titanate. In various embodiments as otherwise described herein, contact with the reducing gas is carried out for a time of at least 10 minutes, such as at least 30 minutes or at least 1 hour. In various embodiments, contact with the reducing gas is carried out for a time of 10 minutes to 24 hours, such as 30 minutes to 24 hours, or 1-24 hours.
[0054] The inventors have found that high temperature is essential for the production of manganese titanate phase. Therefore, as described above, the reduction temperature is at least 350°C. However, higher temperatures can be used advantageously. For example, in various embodiments as further described herein, the contact of the first catalyst precursor with the reducing gas is carried out at a temperature of at least 360°C, such as at least 370°C, or at least 380°C, or at least 390°C. In various embodiments as further described herein, the contact of the first catalyst precursor with the reducing gas is carried out at a temperature of at least 400°C, such as at least 410°C or at least 420°C. In various embodiments as further described herein, the contact of the first catalyst precursor with the reducing gas is carried out at a temperature of at least 430°C, such as at least 440°C or at least 450°C. In various embodiments, the contact of the first catalyst precursor with the reducing gas is carried out at a temperature of not more than 800°C, such as not more than 700°C. In various embodiments, the contact of the first catalyst precursor with the reducing gas is carried out at a temperature of not more than 650°C.
[0055] The high temperature reduction as described herein is operated at a temperature higher than most other Fischer-Tropsch processes. Reaching such temperatures generally requires a dedicated reactor with upgraded metallurgy to reduce the chance of reactor damage. Therefore, it may be desirable to perform the high temperature reduction in a reactor specifically designed for this purpose. Therefore, in certain embodiments as further described herein, the high temperature reduction is performed in a first reactor. Subsequently, in some embodiments, the Fischer-Tropsch catalyst precursor can be removed from the first reactor and introduced into a second reactor for subsequent processing steps.
[0056] In various embodiments as described herein in addition, the reducing gas comprises H2, CO or a mixture thereof. For example, in a particular embodiment, H2 and / or CO are present in the reducing gas in the range of 10% by volume to 100% by volume. For example, in certain embodiments, H2 is present in the reducing gas in the range of 20% by volume to 100% by volume, or 30% by volume to 100% by volume, or 40% by volume to 100% by volume, or 50% by volume to 100% by volume. In various embodiments, the reducing gas may further comprise an inert gas, such as N2 or CO2, in an amount not greater than 90% by volume, such as not greater than 80% by volume, or 70% by volume, or 60% by volume. In various embodiments, the reducing gas is a mixture of H2 and N2.
[0057] The contacting of the first catalyst precursor with the reducing gas can be carried out at various pressures, for example in the range of 0 to 40 barg. In certain embodiments, it may be desirable to use a low pressure. In various such embodiments, the contacting of the first catalyst precursor with the reducing gas can be carried out at a pressure in the range of 0 to 15 barg, for example 0 to 10 barg, or 0 to 5 barg, or 0 to 2 barg.
[0058] As described above, those skilled in the art select the ideal relative amount of manganese titanate for the catalyst. The relative amount of manganese in the form of manganese titanate can be adjusted by the technician according to the present disclosure by changing the conditions of the contacting step, for example to provide any relative amount mentioned above. Generally, higher temperatures, longer times and higher partial pressures of reducing agents (e.g., hydrogen) will provide a higher conversion rate of manganese salts to manganese titanate. In various embodiments as described herein in addition, as measured by X-ray diffraction, at least 10 atomic % (e.g., at least 15 atomic %, or at least 20 atomic %, or at least 30 atomic %, or at least 40 atomic %) of the manganese of the manganese salt of the first catalyst precursor is converted into manganese titanate.
[0059] In various embodiments, the high temperature reduction may be performed to convert a majority of the manganese of the manganese oxide to manganese titanate. Thus, in various embodiments as further described herein, at least 50 atomic % (e.g., at least 60 atomic %, or at least 70 atomic %, or at least 80 atomic %) of the manganese of the manganese oxide of the first catalyst precursor is converted to manganese titanate as measured by X-ray diffraction. In various embodiments as further described herein, at least 90 atomic % (e.g., at least 95 atomic % or at least 98 atomic %) of the manganese of the manganese oxide of the first catalyst precursor is converted to manganese titanate as measured by X-ray diffraction.
[0060] However, as described above, in some cases it may be desirable to leave a portion of the manganese in the form of manganese oxide. Thus, in some embodiments, at least 1 atomic % (e.g., at least 0.5 atomic %, or at least 1 atomic %, or at least 2 atomic %, or at least 5 atomic %) of the manganese in the manganese oxide remains in the form of manganese oxide after high temperature reduction.
[0061] The first catalyst precursor for high temperature reduction can be provided by a person of ordinary skill in the art. Many methods for producing supported transition metal catalysts are known in the art. For example, the impregnation method is described in International Patent Application Nos. PCT / EP2015 / 080745 and PCT / EP2018 / 053350, each of which is incorporated herein by reference in its entirety.
[0062] The reduction temperature after the cobalt addition can be adjusted by the skilled person. Generally, it is desirable to reduce at least a portion of the cobalt to cobalt (0) as a catalytically active Fischer-Tropsch species. Therefore, the reduction of the catalyst precursor with a reducing gas can be carried out at a temperature of not more than 340°C, for example, not more than 330°C, or 320°C, or 310°C, or 300°C. In various embodiments, the reduction is carried out at a temperature of at least 200°C.
[0063] The catalyst compositions described herein may include various loadings of cobalt as selected by one of ordinary skill in the art. In various embodiments as otherwise described herein, cobalt is present in an amount ranging from 5 wt % to 25 wt % (e.g., calculated as cobalt (0), in the range of 7-35 wt %, or 10-35 wt %, or 5-25 wt %, or 7-25 wt %, or 10-25 wt %, or 5-20 wt %, or 7-20 wt %, or 10-20 wt %).
[0064] It is known that Fischer-Tropsch catalysis with shaped particles such as extrudates is beneficial, particularly in the case of fixed catalyst bed reactor systems. For example, it is known that, for catalyst particles of a given shape, a reduction in the size of the catalyst particles in a fixed bed results in a corresponding increase in the pressure drop across the bed. Thus, relatively large shaped particles result in a smaller pressure drop across the catalyst bed in the reactor than a corresponding powdered or granular supported catalyst. Shaped particles, such as extrudates, also typically have greater strength and experience less wear, which is particularly valuable in fixed bed arrangements where bulk crush strength must be very high. Thus, in certain embodiments as otherwise described herein, the titania support is in the form of an extrudate.
[0065] "Impregnation" mentioned herein is intended to mean that the support material is contacted with one or more solutions of, for example, cobalt-containing compounds or manganese-containing compounds as required before drying to achieve the precipitation of cobalt-containing compounds and / or manganese-containing compounds. Impregnation with one or more substantially dissolved solutions of cobalt-containing compounds and / or manganese-containing compounds ensures good dispersion of cobalt-containing compounds and manganese-containing compounds on the support material, and is therefore preferred. This is in contrast to the use of partially dissolved cobalt-containing compounds and / or partially dissolved manganese-containing compounds, for example, in a "solid solution" or suspension, in which the dispersion level of cobalt-containing compounds and manganese-containing compounds on the surface of the support material and in the pores can fluctuate according to the precipitation properties on the support material. In addition, compared with a solid solution, the use of one or more completely dissolved solutions of cobalt-containing compounds and / or manganese-containing compounds has a smaller effect on the resulting morphology and stacked crushing strength of the extrudate formed thereafter. Nevertheless, in the case of using one or more solid solutions of partially undissolved cobalt-containing compounds and / or manganese-containing compounds, the benefits of the method of the present disclosure can also be achieved.
[0066] In the case where a powder or granules of the support material is contacted with one or more solutions of a cobalt-containing compound and / or a manganese-containing compound, the amount of solution used preferably corresponds to an amount of liquid suitable for achieving a mixture having a consistency suitable for further processing, for example for shaping by extrusion. In this case, complete removal of the solvent of the impregnation solution can be carried out after the formation of the shaped particles, such as extrudates.
[0067] Suitable cobalt-containing compounds are those which are thermally decomposable to cobalt oxides after calcination and which are preferably completely soluble in the impregnation solution. Preferred cobalt-containing compounds are cobalt nitrates, acetates or acetylacetonates, most preferably cobalt nitrates, such as cobalt nitrate hexahydrate. Halides are preferably avoided as these have been found to be detrimental.
[0068] Suitable manganese-containing compounds are those which are thermally decomposable after calcination and are preferably completely soluble in the impregnation solution. Preferred manganese-containing compounds are manganese nitrates, acetates or acetylacetonates, most preferably manganese acetates.
[0069] The solvent of the impregnation solution can be an aqueous solvent or a non-aqueous organic solvent. Suitable non-aqueous organic solvents include, for example, alcohols (e.g., methanol, ethanol and / or propanol), ketones (e.g., acetone), liquid alkanes and ethers. Alternatively, an aqueous organic solvent, such as an aqueous alcohol solvent, can be used. Preferably, the solvent of the impregnation solution is an aqueous solvent.
[0070] After impregnation of the support material, the impregnation solution is usually dried to achieve precipitation of the cobalt-containing compound and / or the manganese-containing compound onto the support material, and preferably also removes the binding solvent (e.g., water) of the impregnation solution. Therefore, drying does not, for example, result in complete decomposition of the cobalt- or manganese-containing compound or otherwise result in a change in the oxidation state of the cobalt- or manganese-containing compound. It will be appreciated that in an embodiment in which extrusion is performed, complete drying and removal of the solvent (e.g., binding solvent) of the impregnation solution can be performed, for example, after forming the shaped particles by extrusion. Drying is suitably performed at a temperature of 50° C. to 150° C., preferably 75° C. to 125° C. Suitable drying times are, for example, 5 minutes to 72 hours. Drying can be suitably performed in a drying oven or box furnace, for example, under an inert gas flow, at an elevated temperature.
[0071] The supported Co-Mn Fischer-Tropsch synthesis catalyst used in the method of the present disclosure may additionally include one or more promoters, dispersing aids or binders. Promoters may be added to promote the reduction of cobalt oxide to cobalt metal, preferably at lower temperatures. Preferably, the one or more promoters are selected from ruthenium, palladium, platinum, rhodium, rhenium, chromium, nickel, iron, molybdenum, manganese, tungsten, zirconium, gallium, thorium, lanthanum, cerium, copper and mixtures thereof. Promoters are generally used with a cobalt / promoter atomic ratio of up to 250:1, more preferably up to 125:1, more preferably up to 25:1, and most preferably 10:1. In one or more preferred embodiments, the one or more promoters are present in the resulting cobalt-containing Fischer-Tropsch synthesis catalyst in an amount of 0.1 wt % to 3 wt % by element based on the total weight of the supported synthesis catalyst. In the embodiment in which manganese is added as a promoter, this is understood to be manganese other than manganese added during the impregnation process. In one or more preferred embodiments, the cobalt-containing Fischer-Tropsch synthesis catalyst does not contain one or more promoters. For example, in some embodiments as otherwise described herein, the cobalt-containing Fischer-Tropsch synthesis catalyst comprises a transition metal, wherein the transition metal consists of Co, Mn, and Ti.
[0072] In certain embodiments as otherwise described herein, the catalyst support precursor is prepared by a process comprising the steps of:
[0073] impregnating a titania support material with a decomposable manganese salt to form an impregnated titania support material; and
[0074] The impregnated titania support material is calcined at a temperature in the range of 200°C to 450°C.
[0075] Advantageously, the catalysts of the present disclosure and methods for making the same are capable of producing catalysts having high manganese loadings and, when used in the Fischer-Tropsch synthesis, ideally low alcohol selectivity. Thus, in another aspect, the present disclosure provides a method for producing hydrocarbons, the method comprising contacting a titanium dioxide-supported Fischer-Tropsch catalyst, such as a catalyst as otherwise described herein, or a catalyst prepared by a method as otherwise described herein, the method comprising contacting a titanium dioxide-supported Fischer-Tropsch catalyst containing at least 1 wt % cobalt and at least 1 wt % manganese, such as a catalyst as otherwise described herein, or a catalyst prepared by a method as otherwise described herein with a gaseous reaction mixture containing H2 and CO in a ratio ranging from 1:1 to 3:1, wherein the method has a selectivity to alcohols of no more than 10%. For example, in various embodiments as otherwise described herein, the method has a selectivity to alcohols of no more than 8%, or no more than 6%, or even no more than 5%. In various such embodiments, the catalyst comprises at least 2 wt % manganese, such as at least 4 wt % or even at least 7 wt % or even at least 10 wt % or even at least 15 wt % manganese.
[0076] The Fischer-Tropsch process as otherwise described herein may also have an advantageous high C 5+ Selectivity. For example, in certain embodiments, the method has at least 75%, such as at least 80%, or at least 85%, or at least 90% C 5+ Selectivity. A Fischer-Tropsch process as otherwise described herein may also have an advantageously low selectivity to methane. For example, in certain embodiments, the process has a methane selectivity of no greater than 6%, such as no greater than 5%, or 4%, or 3%.
[0077] Conventional Fischer-Tropsch temperatures can be used to prepare liquid hydrocarbons according to the present disclosure using the catalysts described herein. For example, the contact temperature of a mixture of hydrogen and gaseous carbon oxides (e.g., in the form of a synthesis gas mixture) with a supported cobalt-manganese Fischer-Tropsch catalyst can be suitably in the range of 100 to 400°C, such as 100 to 350°C, or 100 to 300°C, or 100 to 250°C, or 150 to 400°C, or 150 to 350°C, or 150 to 300°C, or 150 to 250°C. In certain embodiments, the contact is carried out at a temperature of not more than 350°C, such as not more than 325°C, or not more than 300°C, or not more than 280°C, or not more than 260°C. The contact pressure (i.e., the pressure of the Fischer-Tropsch reaction) may be suitably in the range of 10 to 100 bara (1 to 10 MPa), such as 15 to 75 bara (1.5 to 7.5 MPa), or 20 to 50 bara (2.0 to 5.0 MPa) in certain embodiments. For example, in certain embodiments, the contact is carried out at a pressure of no more than 7.5 MPa absolute pressure.
[0078] In a specific embodiment, the temperature of the Fischer-Tropsch reaction is in the range of 150 to 350° C., more preferably 180 to 300° C., and most preferably 200 to 260° C. In a preferred embodiment, the pressure of the Fischer-Tropsch reaction is in the range of 10 to 100 bar (1 to 10 MPa), more preferably 10 to 60 bar (1 to 6 MPa), and most preferably 20 to 45 bar (2 to 4.5 MPa).
[0079] As discussed, the present disclosure provides a method for controlling the selectivity of a Fischer-Tropsch synthesis catalyst. Accordingly, in another aspect, the present disclosure provides a method for controlling the selectivity of a Fischer-Tropsch catalyst, the method comprising:
[0080] (i) providing a titania-supported Fischer-Tropsch synthesis catalyst precursor comprising manganese in an amount of at least 1 wt. % calculated as manganese (0) (e.g. a catalyst precursor as otherwise described herein); and
[0081] (ii) contacting the catalyst with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a second catalyst precursor in which at least 10 atomic % of the manganese is present as MnTiO 3 ;
[0082] (iii) impregnating the second catalyst precursor with a cobalt salt;
[0083] (iv) calcining at a temperature in the range of 200°C to 450°C;
[0084] (v) contacting the calcined catalyst with a reducing gas at a temperature of not more than 300° C. to produce a Fischer-Tropsch catalyst, wherein
[0085] The selectivity of the Fischer-Tropsch catalyst to alcohols is no more than 50% of the selectivity to alcohols of an equivalent catalyst contacted with the reducing gas at a temperature of 300° C. for the same amount of time in step (ii).
[0086] For example, in certain embodiments as further described herein, the alcohol selectivity of the resulting reduced catalyst is no greater than 35% (e.g., no greater than 20%) of the alcohol selectivity of the equivalent catalyst reduced at a temperature of 300° C. In addition to alcohol selectivity, C 5+ Thus, in certain embodiments as further described herein, the C 5+ The selectivity is greater than that of the same catalyst reduced at 300°C (e.g., C 5+ In this regard, selectivity may be determined under FT conditions, for example, comparing catalyst performance under FT conditions, such as 30 barg and a H2:CO ratio of 2:1, wherein temperature or flow is adjusted to match conversion to 40-60%.
[0087] As described in more detail below, various reaction systems can be used to implement the methods described herein, and those of ordinary skill in the art will adapt conventional systems as needed. An example of a reaction system for implementing the methods of the present disclosure is shown schematically in Figure 1 The reactor 110 is loaded with a reduced catalyst 120. Synthesis gas is introduced through inlet 101, and hydrocarbon products are removed through outlet 104 for further processing. Unreacted synthesis gas and optional light hydrocarbons can be removed through a suitable recycle outlet and recycled back to inlet 101 through recycle feed 103.
[0088] The CO conversion is defined as moles of CO used / moles of CO fed x 100. 5+ The hydrocarbon selectivity is defined as the 5+ Moles of CO to hydrocarbons / moles of CO converted x 100. Alcohol selectivity is defined as moles of CO attributed to alcohols / moles of CO converted x 100.
[0089] Unless otherwise stated, the temperatures mentioned in the examples are applied temperatures, not catalyst / bed temperatures. Unless otherwise stated, the pressures mentioned in the examples are absolute pressures.
[0090] The method of the present disclosure will now be further described with reference to the following examples which are presented by way of illustration only.
[0091] In certain embodiments, the term cobalt salt or manganese salt, the term "salt" includes, but is not limited to, nitrates, acetates, hydroxides, oxides, carbonates, citrates, chlorides, and sulfates.
[0092] Example
[0093] The following examples illustrate specific embodiments of the methods of the present disclosure and various uses thereof. They are for illustrative purposes only and should not be considered to limit the scope of the present disclosure.
[0094] Example 1: Manganese loading and reduction temperature screening
[0095] Three titanium dioxide supported Fischer-Tropsch catalyst precursors were prepared with metal loadings of 50 wt%, 30 wt% and 10 wt% MnO. These catalyst precursors were prepared by mixing titanium dioxide (P25) with a decomposable manganese salt such as manganese acetate tetrahydrate or manganese nitrate and calcining at a temperature of at least 450°C to form MnO. Subsequently, they were reduced in H2 at atmospheric pressure at 500°C for 12 hours:
[0096] Table 1
[0097]
[0098] The above support was then impregnated with a cobalt salt (cobalt nitrate hexahydrate) to form the following catalyst:
[0099] Table 2
[0100]
[0101] Subsequently, the above catalyst 6 was used for Fischer-Tropsch synthesis in comparison with a Co-Mn catalyst that had not undergone high temperature reduction and a cobalt catalyst that did not contain manganese. -1 Fischer-Tropsch synthesis was carried out at a synthesis gas space velocity and a synthesis gas ratio of 1.8 H2:CO:
[0102] Table 3
[0103]
[0104]
[0105] As observed above, Catalyst 6 of the present invention exhibited a smaller alcohol selectivity of only 1.4%, compared to 17.3% observed for an equivalent catalyst that had not undergone high temperature reduction. Interestingly, the alcohol selectivity of Catalyst 6 was even less than the 2.3% selectivity observed for Catalyst 8, which did not contain manganese. Thus, high temperature reduction in this manner is an effective way to alter alcohol and oxygenate selectivity.
[0106] Example 2: Formation of manganese titanate
[0107] Figure 2 X-ray diffraction analysis is shown for Supports 1, 2, and 3. In particular, all three supports formed a MnTiO3 phase, with 50% of the manganese present as MnTiO3 as shown in Table 4. Figure 3 Shows the effect of calcination in air vs. hydrogen, Figure 4 X-ray diffraction of the reduced support impregnated with cobalt and calcined and the air calcined analog showing loss of the crystal structure of the MnTiO3 phase. In situ X-ray diffraction showed that the lost MnTiO3 crystal structure can be regained at temperatures below 350°C.
[0108] Table 4
[0109]
[0110] These catalysts with 10% cobalt, 0-10% manganese on titania were reduced and analyzed by X-ray absorption spectroscopy (XAS, EXAFS, XANES) to demonstrate the formation of MnTiO3 and metallic cobalt. Tables 5 and 6 show the formation of Mn-Mn and Mn-Ti bonds consistent with a titanate phase, while cobalt metal and cobalt oxides are the only cobalt phases observed. In addition, the average coordination number (CN) was observed to deviate significantly from that expected for manganese oxides and approach the lower coordination number expected for a titanate phase.
[0111] Table 5 EXAFS fitting results for 10%Co-5%Mn / TiO2 at the Mn edge
[0112]
[0113] Table 6 EXAFS fitting results for 10%Co-10%Mn / TiO2 at the Mn edge
[0114]
[0115] Various exemplary embodiments of the present disclosure include, but are not limited to, the embodiments listed in the claims recited below, which may be combined in any number and in any combination that are not technically or logically contradictory.
[0116] Embodiment 1. A titanium dioxide supported Fischer-Tropsch catalyst precursor comprising:
[0117] a titania support, and manganese in a range of 1 wt % to 50 wt % calculated as manganese (0) disposed on the titania support;
[0118] At least 10 atomic % of the manganese is in the form of MnTiO3 to form a catalyst support.
[0119] Embodiment 2. The catalyst precursor of Embodiment 1, wherein the catalyst precursor is free of cobalt (eg, free of cobalt, copper, or iron).
[0120] Embodiment 3. The catalyst precursor of Embodiment 1 or Embodiment 2, wherein at least 15 atomic % (e.g., at least 20 atomic %, or at least 30 atomic %, or at least 40 atomic %) of the manganese is in the form of MnTiO3.
[0121] Embodiment 4. The catalyst precursor of Embodiment 1 or Embodiment 2, wherein at least 50 atomic % (e.g., at least 60 atomic %, or at least 70 atomic %, or at least 80 atomic %, at least 90 atomic %, at least 95 atomic %, or at least 98 atomic %) of the manganese is in the form of MnTiO3.
[0122] Embodiment 5. The catalyst precursor of any of Embodiments 1-4, wherein at least 0.1 atomic % of the manganese is in the form of MnO (e.g., at least 0.5 atomic %, or at least 1 atomic %, or at least 2 atomic %, or at least 5 atomic %).
[0123] Embodiment 6. The catalyst precursor of any of Embodiments 1-5, wherein manganese is present in an amount ranging from 1 wt% to 50 wt%, such as 1-30 wt%, or 1-20 wt%, or 1-15 wt%, 2 wt% to 40 wt%, 2-20 wt%, or such as 4 wt% to 35 wt%, such as 4-30 wt%, or 4-20 wt%, 7 wt% to 25 wt%, such as 7-20 wt%.
[0124] Embodiment 7. The catalyst precursor of any of Embodiments 1-6, wherein the titania support comprises at least 80 wt% titania, e.g., at least 85 wt% or at least 90 wt% titania, at least 95 wt% titania, e.g., at least 98 wt% titania or at least 99 wt% titania.
[0125] Embodiment 8. The catalyst precursor of any of Embodiments 1-7, wherein the support material comprises no greater than 5 wt% (e.g., no greater than 1 wt%, or no greater than 0.5 wt%) of the total amount of silica, alumina, ceria, zirconia, and zinc oxide.
[0126] Embodiment 9. The catalyst precursor of any of Embodiments 1-8, wherein the support material is in the form of extrudates, powders, granules, or microspheres.
[0127] Embodiment 10. The catalyst precursor of any one of Embodiments 1-9, wherein the catalyst precursor is made by impregnation technique, chemical deposition or spray drying.
[0128] Embodiment 11. A method for producing a titanium dioxide-supported Fischer-Tropsch catalyst precursor (e.g., a catalyst precursor of any one of Embodiments 1-10), the method comprising:
[0129] providing a first catalyst precursor comprising a manganese oxide disposed on a titania support, wherein the support precursor is free of cobalt; and
[0130] The first catalyst precursor is contacted with the reducing gas at a temperature of at least 350° C. for a time sufficient to provide a second catalyst precursor wherein at least 10 atomic % of the manganese is present as MnTiO 3 .
[0131] Embodiment 12. The method of Embodiment 11, wherein the contact with the reducing gas is carried out for 10 minutes to 24 hours, such as 30 minutes to 24 hours, or 1-24 hours.
[0132] Embodiment 13. The method of any one of Embodiments 11-12, wherein the reducing gas comprises H2, CO, or a mixture thereof, wherein the reducing gas is present at 10 volume % to 100 volume % of the reducing gas.
[0133] Embodiment 14. The method of any one of Embodiments 11-13, wherein the contact with the reducing gas is carried out at a temperature of at least 360°C (e.g., at least 370°C, or at least 380°C, or at least 390°C, at least 400°C (e.g., at least 410°C, or at least 420°C, at least 440°C, or at least 450°C).
[0134] Embodiment 15. The method of any of Embodiments 11-14, wherein the contacting with the reducing gas is carried out at a temperature not greater than 800°C, eg, not greater than 700°C or not greater than 600°C.
[0135] Embodiment 16. The method of any one of claims 11-15, wherein the contacting with the reducing gas is carried out at a pressure in the range of 0 barg to 40 barg.
[0136] Embodiment 17. The method of any of Embodiments 11-16, wherein at least 10 atomic % (e.g., at least 15 atomic %, or at least 20 atomic %, or at least 30 atomic %, or at least 40 atomic %) of the manganese in the support precursor is converted to manganese titanate.
[0137] Embodiment 18. The method of any of Embodiments 11-17, wherein at least 50 atomic % (e.g., at least 60 atomic %, or at least 70 atomic %, or at least 80 atomic % or at least 90 atomic %, or at least 95 atomic %) of the manganese in the support precursor is converted to manganese titanate.
[0138] Embodiment 19. The method of any one of Embodiments 11-18, wherein the first catalyst precursor is prepared by a method comprising the steps of:
[0139] impregnating a titanium dioxide support material with a decomposable manganese salt; and
[0140] The impregnated titania support material is calcined at a temperature in the range of 200°C to 450°C.
[0141] Embodiment 20. A method for producing a Fischer-Tropsch catalyst, the method comprising:
[0142] Providing a Fischer-Tropsch catalyst precursor according to any one of claims 1 to 10 (or prepared according to any one of claims 11 to 19);
[0143] impregnating the catalyst precursor with a decomposable cobalt salt;
[0144] The impregnated catalyst precursor is calcined at a temperature in the range of 200°C to 450°C.
[0145] Embodiment 21. The method of Embodiment 20, wherein cobalt is present in the prepared catalyst in an amount in the range of 5 wt% to 25 wt% (e.g., in the range of 7-35 wt%, or 10-35 wt%, or 5-25 wt%, or 7-25 wt%, or 10-25 wt%, or 5-20 wt%, or 7-20 wt%, or 10-20 wt%, calculated as cobalt(0)).
[0146] Embodiment 22. A Fischer-Tropsch catalyst prepared by the method of Embodiment 20 or Embodiment 21.
[0147] Embodiment 23. A method for producing hydrocarbons, comprising contacting a supported Fischer-Tropsch catalyst containing MnTiO3 (e.g., the catalyst of Embodiment 22, or a catalyst made according to the method of Embodiment 20 or 21) with a gaseous reaction mixture comprising H2 and CO in a ratio ranging from 1:1 to 3:1, wherein the method has a selectivity for alcohols of not more than 20% (e.g., not more than 10%, or not more than 8%, or not more than 6%).
[0148] Embodiment 24. The method of Embodiment 23, wherein the catalyst comprises at least 2 wt % manganese, eg, at least 4 wt % or even at least 7 wt %.
[0149] Embodiment 25. The method of embodiment 23 or embodiment 24, wherein the method has a C of at least 75% (e.g., at least 80%, or at least 85%, or at least 90%). 5+ Selective.
[0150] Embodiment 26. The method of any of Embodiments 23-25, wherein the method has a methane selectivity of no greater than 15% (eg, no greater than 10%, or 8%).
[0151] Embodiment 27. A method of controlling the selectivity of a Fischer-Tropsch catalyst, the method comprising:
[0152] (i) providing a titanium dioxide-supported Fischer-Tropsch synthesis catalyst precursor comprising manganese in an amount of at least 1 wt % calculated as manganese (0); and
[0153] (ii) contacting the catalyst with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a second catalyst precursor in which at least 10 atomic % of the manganese is present as MnTiO 3 ;
[0154] (iii) impregnating the second catalyst precursor with a cobalt salt;
[0155] (iv) calcining at a temperature in the range of 200°C to 450°C;
[0156] (v) contacting the calcined catalyst with a reducing gas at a temperature of no greater than 300° C. to produce a Fischer-Tropsch catalyst; wherein
[0157] The selectivity of the Fischer-Tropsch catalyst to alcohols is no more than 50% of the selectivity to alcohols of an equivalent catalyst contacted with the reducing gas at a temperature of 300° C. for the same amount of time in step (ii).
[0158] Embodiment 28. The method of Embodiment 27, wherein the alcohol selectivity of the resulting reduced catalyst is no greater than 35% (eg, no greater than 20%) of the alcohol selectivity of an equivalent catalyst.
[0159] Embodiment 29. The method of Embodiment 27 or Embodiment 28, wherein the C of the obtained Fischer-Tropsch catalyst is 5+ The selectivity is greater than that of the same catalyst (e.g., C 5+ Selectivity of at least 110%).
[0160] Embodiment 30. A method for producing a supported Fischer-Tropsch catalyst, comprising:
[0161] a) providing a first catalyst support precursor comprising a manganese salt disposed on a titanium dioxide support, wherein the first catalyst precursor is free of cobalt; and optionally calcining in an oxygen-containing atmosphere to form a support precursor;
[0162] b) contacting the first catalyst support precursor with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a titania-supported Fischer-Tropsch catalyst precursor in which at least 10 atomic % of manganese is present as MnTiO 3 ;
[0163] c) contacting the catalyst precursor with a decomposable cobalt salt and calcining at a temperature in the range of 200° C. to 450° C. in an oxygen-containing atmosphere; wherein the MnTiO 3 phase is at least partially decomposed;
[0164] d) reducing the catalyst precursor with a reducing gas at a temperature of no greater than 350° C. to form a titania-supported Fischer-Tropsch catalyst, wherein at least 10 atomic % of the manganese of the final catalyst is present as MnTiO 3 .
[0165] Embodiment 31. The catalyst precursor of Embodiment 30, wherein step b is carried out at above 350°C, preferably above 400°C, more preferably above 450°C, and most preferably above 500°C.
[0166] Embodiment 32. The catalyst precursor of Embodiment 30 or Embodiment 31, wherein step d is carried out at less than 350°C, preferably less than 320°C, more preferably less than 300°C, and most preferably greater than 280°C.
[0167] The details shown herein are provided as examples and only for the purpose of illustrative discussion of certain embodiments of the present disclosure, and are given in order to provide the most useful and understandable description of the principles and concepts of the various embodiments of the present disclosure. In this regard, no attempt is made to display the details related to the methods of the present disclosure to a level of detail necessary for a basic understanding of the methods described herein, and the descriptions made in conjunction with the examples make it clear to those skilled in the art how several forms of the methods of the present disclosure can be specifically implemented in practice. Therefore, before describing the disclosed methods and apparatus, it is to be understood that the aspects described herein are not limited to specific embodiments, apparatuses, or configurations, and therefore can certainly vary. It is also to be understood that the terms used herein are only for the purpose of describing specific aspects, and are not intended to be limiting unless specifically defined herein.
[0168] The terms “a” and “an” and “the” and similar referents used in the context of describing the methods of the present disclosure (especially in the context of the following embodiments and claims) should be construed to cover both the singular and the plural, unless otherwise indicated herein or clearly contradicted by context.
[0169] Unless otherwise specified herein or clearly contradictory to the context, all methods described herein can be performed in any suitable order of steps. The use of any and all examples or exemplary wordings (e.g., "such as") provided herein is intended only to better illustrate the methods of the present disclosure rather than to impose limitations on the scope of the present disclosure. The wording in the specification should not be interpreted as indicating that any unclaimed element is essential to the practice of the methods of the present disclosure.
[0170] Unless the context clearly requires otherwise, throughout the specification and claims, the words "comprising" and the like should be interpreted in an inclusive sense rather than an exclusive or exhaustive sense; that is, in the sense of "including but not limited to". Words using the singular or plural number also include the plural and singular, respectively. In addition, when used in this application, the words "herein", "above" and "hereafter" and words of similar meaning shall refer to this application as a whole and not to any particular part of this application.
[0171] As will be appreciated by those of ordinary skill in the art, each embodiment disclosed herein may comprise, consist essentially of, or consist of its specific specified elements, steps, ingredients, or components. As used herein, the transitional term "comprising" is meant to include, but is not limited to, and allows for the inclusion of unspecified elements, steps, ingredients, or components, even in major amounts. The transitional phrase "consisting of" does not include any unspecified elements, steps, ingredients, or components. The transitional phrase "consisting essentially of" limits the scope of the embodiment to the specified elements, steps, ingredients, or components and those that do not substantially affect the embodiment.
[0172] All percentages, ratios and proportions herein are by weight unless otherwise specified.
[0173] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the disclosure are approximations, the numerical values set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0174] The grouping of alternative elements or embodiments of the present disclosure should not be construed as limiting. Each group member may be mentioned and claimed individually or in any combination with other members of the group or other elements found herein. It is estimated that one or more members in the group may join the group or delete from the group for convenience and / or patentability reasons. When any such addition or deletion occurs, this specification is considered to contain the modified group, so the written description of all Markush groups used in the appended claims is met.
[0175] Some embodiments of various aspects of the present disclosure are described herein, including the best mode known to the inventors for implementing the methods described herein. Of course, the changes to these described embodiments will be apparent to those of ordinary skill in the art after reading the above description. The technician will utilize such changes as appropriate, so the method of the present disclosure can be implemented differently from the specific description herein. Therefore, the scope of the present disclosure includes all modifications and equivalents of the subject items listed in the claims attached hereto as permitted by applicable law. In addition, unless otherwise specified herein or clearly contradictory to the context, the present disclosure covers any combination of the above-mentioned elements under all possible changes thereof.
[0176] As used herein, the phrase "at least a portion" is used to mean at least a desired fractional amount, up to a full possible amount.
[0177] Finally, it is to be understood that the various embodiments herein illustrate the method of the present disclosure. Other modifications that may be employed are within the scope of the present disclosure. Therefore, by way of example and not limitation, alternative configurations of the method may be utilized according to the teachings herein. Therefore, the method of the present disclosure is not limited to being exactly as shown and described.
Claims
1. A titanium dioxide supported Fischer-Tropsch catalyst precursor, comprising: Titanium dioxide support, and a titanium dioxide support Manganese in the range of 1 wt. % to 50 wt. % calculated as manganese (0); At least 10 atomic % of the manganese is in the form of MnTiO3 to form a catalyst support.
2. The catalyst precursor of claim 1, wherein the catalyst precursor is cobalt-free (eg, free of cobalt, copper, or iron).
3. A catalyst precursor according to claim 1 or claim 2, wherein at least 15 atomic % (e.g., at least 20 atomic %, or at least 30 atomic %, or at least 40 atomic %) of the manganese is in the form of MnTiO3.
4. A catalyst precursor according to claim 1 or claim 2, wherein at least 50 atomic % (e.g., at least 60 atomic %, or at least 70 atomic %, or at least 80 atomic %, at least 90 atomic %, at least 95 atomic %, or at least 98 atomic %) of the manganese is in the form of MnTiO3.
5. The catalyst precursor of any one of claims 1 to 4, wherein at least 0.1 atomic % of the manganese is in the form of MnO (e.g., at least 0.5 atomic %, or at least 1 atomic %, or at least 2 atomic %, or at least 5 atomic %).
6. The catalyst precursor according to any one of claims 1 to 5, wherein manganese is present in an amount ranging from 1 wt% to 50 wt%, such as 1-30 wt%, or 1-20 wt%, or 1-15 wt%, 2 wt% to 40 wt%, 2-20 wt%, or such as 4 wt% to 35 wt%, such as 4-30 wt%, or 4-20 wt%, 7 wt% to 25 wt%, such as 7-20 wt%.
7. The catalyst precursor according to any one of claims 1 to 6, wherein the titania support comprises at least 80 wt% titania, such as at least 85 wt% or at least 90 wt% titania, at least 95 wt% titania, such as at least 98 wt% titania or at least 99 wt% titania.
8. A method for producing a titanium dioxide-supported Fischer-Tropsch catalyst precursor (e.g., a catalyst precursor according to any one of claims 1 to 7), the method comprising: providing a first catalyst precursor comprising a manganese oxide disposed on a titania support, wherein the support precursor is free of cobalt; and The first catalyst precursor is contacted with the reducing gas at a temperature of at least 350° C. for a time sufficient to provide a second catalyst precursor wherein at least 10 atomic % of the manganese is present as MnTiO 3 .
9. A method for producing a Fischer-Tropsch catalyst, the method comprising: Providing a Fischer-Tropsch catalyst precursor according to any one of claims 1 to 7 (or prepared according to claim 8); impregnating the catalyst precursor with a decomposable cobalt salt; The impregnated catalyst precursor is calcined at a temperature in the range of 200°C to 450°C.
10. The method of claim 9, wherein cobalt is present in the prepared catalyst in an amount in the range of 5 wt% to 25 wt% (e.g., in the range of 7-35 wt%, or 10-35 wt%, or 5-25 wt%, or 7-25 wt%, or 10-25 wt%, or 5-20 wt%, or 7-20 wt%, or 10-20 wt%, calculated as cobalt (0)).
11. A Fischer-Tropsch catalyst prepared by the method according to claim 9 or claim 10.
12. A method for producing hydrocarbons, comprising contacting a supported Fischer-Tropsch catalyst containing MnTiO3 (e.g., a catalyst according to claim 11, or a catalyst prepared according to claim 9 or claim 10) containing at least 1 wt.% cobalt and 1 wt.% manganese with a gaseous reaction mixture comprising H2 and CO in a ratio ranging from 1:1 to 3:1, wherein the method has a selectivity to alcohols of not more than 20% (e.g., not more than 10%, or not more than 8%, or not more than 6%).
13. A method for controlling the selectivity of a Fischer-Tropsch catalyst, the method comprising: (i) providing a titanium dioxide-supported Fischer-Tropsch synthesis catalyst precursor comprising manganese in an amount of at least 1 wt % calculated as manganese (0); and (ii) contacting the catalyst with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a second catalyst precursor in which at least 10 atomic % of the manganese is present as MnTiO 3 ; (iii) impregnating the second catalyst precursor with a cobalt salt; (iv) calcining at a temperature in the range of 200°C to 450°C; (v) contacting the calcined catalyst with a reducing gas at a temperature of not more than 300° C. to produce a Fischer-Tropsch catalyst, wherein The selectivity of the Fischer-Tropsch catalyst to alcohols is no more than 50% of the selectivity to alcohols of an equivalent catalyst contacted with the reducing gas at a temperature of 300° C. for the same amount of time in step (ii).
14. The method according to claim 13, wherein the alcohol selectivity of the obtained reduced catalyst is no more than 35% (eg no more than 20%) of the alcohol selectivity of an equivalent catalyst.
15. The method according to claim 13 or claim 14, wherein the C of the obtained Fischer-Tropsch catalyst is 5+ The selectivity is greater than that of the same catalyst (e.g., C 5+ Selectivity of at least 110%).
16. A method for producing a supported Fischer-Tropsch catalyst, the method comprising: a) providing a first catalyst support precursor comprising a manganese salt disposed on a titania support, wherein the first catalyst precursor is free of cobalt; and optionally calcining in an oxygen-containing atmosphere to form a support precursor; b) contacting the first catalyst support precursor with a reducing gas at a temperature of at least 350° C. for a time sufficient to provide a titania-supported Fischer-Tropsch catalyst precursor in which at least 10 atomic % of manganese is present as MnTiO 3 ; c) contacting the catalyst precursor with a decomposable cobalt salt and calcining in an oxygen-containing atmosphere at a temperature in the range of 200° C. to 450° C., wherein the MnTiO 3 phase is at least partially decomposed; d) reducing the catalyst precursor with a reducing gas at a temperature of no greater than 350° C. to form a titania-supported Fischer-Tropsch catalyst, wherein at least 10 atomic % of the manganese of the final catalyst is present as MnTiO 3 .
17. A catalyst precursor according to claim 15 or claim 16, wherein step d is carried out at less than 350°C, preferably less than 320°C, more preferably less than 300°C, most preferably greater than 280°C.
Citation Information
Patent Citations
Method of preparing catalyst support from a waste catalyst
CN101087652A
Fischer-tropsch catalyst support and catalyst
US20080262114A1
Titania carrier for supporting catalyst, manganese oxide-titania catalyst comprising the same, apparatus and method for manufacturing the titania carrier and manganese oxide-titania catalyst, and method for removing nitrogen oxides
US20140004027A1
Thermochemical generation of hydrogen and oxygen from water
US4276279A
Fischer-tropsch catalyst support and catalyst
WO2008087147A1