Laminated polyester film
By forming a resin layer X with vinyl alcohol residues and thiophene residues on the polyester film and combining the resin layer Y with siloxane bonds, the problem of antistatic agent leaking at high temperatures is solved, and antistatic properties are achieved and improve heat resistance, suitable for bonded products and industrial processing processes.
Patent Information
- Application Number
- CN202380025639.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-29
- Filing Date
- 2023-03-06
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-03-06
AI Technical Summary
In the case of a laminated film that imparts antistatic properties to the release layer, there are problems of antistatic agent leakage and process contamination when heating is applied.
A laminated polyester film is adopted, which has a resin layer X on at least one surface of the polyester film, including Compound A with vinyl alcohol residues and Compound B with thiophene residues, and a solid component middle ring of the resin layer X The oxygen content is 5 mg/g or more and 100 mg/g or less, the total organic component is 90 mass % or more, the sum of vinyl alcohol residues, thiophene residues and epoxy compounds is 90 mass % or more, and the degree of polymerization is 50 or more, and the degree of polymerization is 50 or more, and the The adhesion M(X) is ≥90%, and the resin layer X and the resin layer Y are formed by the online coating method, and the surface resistivity of the resin layer Y remains within an excellent range after heat treatment.
A layered polyester film with excellent antistatic and heat resistance is achieved, which can suppress oligomer leakage under high temperature conditions, improve the heat resistance and antistatic properties of the film, and is suitable as a protective film for adhesive products and Films for processing industrial products.
Smart Images

Figure BDA0005028761140000151 
Figure BDA0005028761140000161 
Figure BDA0005028761140000171
Abstract
Description
Technical Field
[0001] The present invention relates to a laminated polyester film having excellent antistatic properties and heat resistance. Background Art
[0002] Polyester films have excellent properties such as mechanical properties, electrical properties, dimensional stability, transparency, and chemical resistance, and are therefore widely used as magnetic recording materials, optical materials, and industrial materials.
[0003] In addition, in recent years, as a protective film for the adhesive layer in the adhesive product, a process film in the processing process of various industrial products, the demand for a film having excellent heat resistance to the heat applied in the processing process of various industrial products has increased for demoulding properties, antistatic properties, and various industrial products. In this case, a film that imparts antistatic properties to the demoulding layer has been disclosed (Patent Document 1). In addition, in order to impart heat resistance, a film that provides a base layer between a demoulding film that has been imparted with antistatic properties and a substrate of a polyester film has been disclosed (Patent Document 2).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-66888
[0007] Patent Document 2: Japanese Patent Application Publication No. 2014-141557 Summary of the invention
[0008] Problems to be solved by the invention
[0009] However, in the case of a laminated film in which antistatic properties are imparted to a release layer, when heat is applied to the film, there are problems such as the antistatic agent contained in the release layer oozing out, deterioration of antistatic properties, or contamination of the process.
[0010] Means of solving the problem
[0011] In order to solve the above problems, the laminated polyester film of the present invention adopts the following constitution. That is,
[0012] <1> A laminated polyester film comprising a resin layer X on at least one surface of a polyester film, wherein the resin layer X contains at least a compound A having a vinyl alcohol residue and a compound B having a thiophene residue.
[0013] <2> The laminated polyester film according to <1>, wherein the epoxy group content in the solid content of the resin layer X measured from the laminated polyester film under specific extraction and analysis conditions is 5 mg / g or more and 100 mg / g or less.
[0014] <3> The laminated polyester film according to <1> or <2>, wherein the total amount of organic components in the solid content of the resin layer X extracted under specific extraction conditions is 90% by mass or more, assuming that the converted mass of the resin layer X of the laminated polyester film is 100% by mass.
[0015] <4> The laminated polyester film according to any one of <1> to <3>, wherein the total content of the compound A having a vinyl alcohol residue, the compound B having a thiophene residue, and the epoxy compound C in 100% by mass of the resin layer X is 90% by mass or more.
[0016] <5> The laminated polyester film according to any one of <1> to <4>, wherein the degree of polymerization of the compound A is 50 or more and 1,000 or less.
[0017] <6> The laminated polyester film according to any one of <1> to <5>, wherein the adhesion M(X) of the resin layer X satisfies the following conditions:
[0018] M(X)≥90(%).
[0019] <7> The method for producing a laminated polyester film according to <1> or <2>, which comprises, in this order, a step of coating the coating agent for forming the resin layer X on a polyester film and a step of stretching the polyester film.
[0020] <8> The laminated polyester film according to any one of <1> to <6>, comprising a polyester film, the resin layer X, and a resin layer Y in this order.
[0021] <9> The laminated polyester film according to <8>, wherein the surface resistivity of the surface of the resin layer Y satisfies the following formula (1) and formula (2),
[0022] (1)10 6 ≤Ω (0) ≤10 10
[0023] (2)Ω (150) / Ω (0) <50
[0024] Among them, Ω (0) represents the surface resistivity (Ω / sq) of the resin layer Y before heat treatment, Ω (150) It shows the surface resistivity (Ω / sq) of the surface of the resin layer Y after heat treatment at 150°C for 60 minutes.
[0025] <10> The laminated polyester film according to <8> or <9>, wherein the surface free energy of the resin layer Y is 30 mN / m or less.
[0026] <11> The laminated polyester film according to any one of <8> to <10>, wherein the resin layer Y is a resin having a compound having a siloxane bond as a main component.
[0027] <12> The laminated polyester film according to any one of <8> to <11>, wherein the water contact angle on the resin layer Y side satisfies the following formula (3) and formula (4),
[0028] (3) 0°≤HYa≤80°
[0029] (4) 10°≤|HYp-HYa|≤100°
[0030] Here, HYp represents the water contact angle on the resin layer Y side of the laminated polyester film, and HYa represents the water contact angle on the resin layer Y side of the laminated polyester film after the laminated polyester film is immersed in pure water at 25° C. for 5 minutes.
[0031] <13> The laminated polyester film according to any one of <8> to <12>, wherein a change in haze after heat treatment at 150°C for 60 minutes (hereinafter, sometimes referred to as “Δ haze”) is 10% or less.
[0032] <14> The laminated polyester film according to any one of <8> to <13>, wherein the solvent durability of the surface of the resin layer Y measured according to JIS L 0849 (2013) (friction tester type II) is 50% or more and 100% or less.
[0033] <15> The laminated polyester film according to any one of <8> to <14>, which is used as a process film in a product manufacturing process.
[0034] Effects of the Invention
[0035] According to the present invention, there can be provided a laminated polyester film which is excellent in antistatic properties and heat resistance and which is suitable for use as a protective film for a pressure-sensitive adhesive layer in pressure-sensitive adhesive products and a process film in the processing steps of various industrial products. DETAILED DESCRIPTION
[0036] The present invention will be described in detail below with reference to specific examples.
[0037] The present invention relates to a laminated polyester film having one or more layers arranged on at least one surface of the polyester film. The polyester referred to in the present invention is a substance having a dicarboxylic acid constituent component and a diol constituent component. It should be noted that, in the present specification, the constituent component represents the smallest unit that can be obtained by hydrolyzing the polyester. As the dicarboxylic acid constituent component constituting the polyester, terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 1,8-naphthalene dicarboxylic acid, 4,4'-diphenyl dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid and other aromatic dicarboxylic acids, or their ester derivatives can be cited.
[0038] In addition, as the diol constituent components constituting the above polyester, there can be mentioned aliphatic diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, alicyclic diols such as cyclohexanedimethanol and spirodiol, and substances formed by connecting a plurality of the above diols, etc. Among them, from the perspective of mechanical properties and transparency, it is preferred to use polyethylene terephthalate (PET), polyethylene 2,6-naphthalate (PEN), substances formed by copolymerizing isophthalic acid, naphthalene dicarboxylic acid and part of the dicarboxylic acid component of PET, and polyesters formed by copolymerizing cyclohexanedimethanol, spirodiol, diethylene glycol and part of the diol component of PET.
[0039] The laminated polyester film of the present invention preferably has a resin layer X on at least one surface of the polyester film, wherein the resin layer X contains at least a compound A having a vinyl alcohol residue and a compound B having a thiophene residue.
[0040] Since the compound B is conductive, antistatic properties can be exhibited by making the resin layer X contain the compound B. In addition, since the compound A has a plurality of electron-rich hydroxyl groups, it can interact with the π-type conjugated electrons of the compound B, improve the fluidity of the rigid compound B, and improve the film-forming property of the resin layer X. As a result of the improved film-forming property of the resin layer X, the compound B can be uniformly present in the surface layer of the polyester film, the surface resistivity of the laminated polyester film is sufficiently reduced, and the antistatic property of the laminated polyester film can be improved. In addition, as a result of the improved film-forming property of the resin layer X, the resin layer X can uniformly cover the surface of the polyester film. As a result, when the film is heat-treated, the oligomers contained in the polyester film can be suppressed from seeping out on the surface of the resin layer X, and a laminated film with less haze change caused by heating, i.e., high heat resistance, can be made.
[0041] In the film of the present invention, the resin layer X contains compound A and compound B, and the fluidity of compound B is improved. As a result, the generation of fine defects in the resin layer X, such as fine coating leaks and microcracks, can be suppressed, and the oligomers contained in the polyester film can be suppressed from seeping out to the surface of the resin layer X, and in particular, a laminated film with high heat resistance can be prepared.
[0042] The compound A having a vinyl alcohol residue as mentioned herein refers to an ion containing polyvinyl alcohol as a source when a laminated polyester film is measured by the method described below. In addition, the compound B having a thiophene residue as mentioned herein refers to an ion containing polythiophene as a source when a laminated polyester film is measured by the method described below.
[0043] As the compound B having a thiophene residue, a polythiophene compound can be preferably used. Polythiophene compounds are generally π-electron conjugated compounds, and because they have conductivity, compound B can exhibit the antistatic properties of the resin layer X. As polythiophene compounds, for example, compounds having a structure in which the positions at positions 3 and 4 of the thiophene ring are substituted can be used. Furthermore, compounds having oxygen atoms bonded to carbon atoms at positions 3 and 4 of the thiophene ring can be preferably used. Substances having hydrogen atoms or carbon atoms directly bonded to the carbon atom are sometimes not easily dispersed in water. The above-mentioned compounds can be manufactured, for example, by the methods disclosed in Japanese Patent Publication No. 2000-6324, European Patent No. 602713, and U.S. Patent No. 5391472, but can also be methods other than these.
[0044] For example, after obtaining 3,4-ethylenedioxythiophene using an alkali metal salt of 3,4-dihydroxythiophene-2,5-dicarboxylate as a starting material, potassium persulfate and ferric sulfate and the previously obtained 3,4-ethylenedioxythiophene are introduced into an aqueous solution of polystyrenesulfonic acid and reacted to obtain a composition in which an acidic polymer such as polystyrenesulfonic acid and a polythiophene such as poly(3,4-ethylenedioxythiophene) are composited. By composited with an acidic polymer, the acidic function of the acidic polymer can also function as a dopant for polythiophene, which is related to the improvement of antistatic properties, and therefore is preferred.
[0045] In addition, as the aqueous coating composition containing poly-3,4-ethylenedioxythiophene and polystyrenesulfonic acid, a product sold as "Baytron" P by HC Starck (Germany) or the like can be used.
[0046] On the other hand, as an acidic polymer, for example, polymer carboxylic acid, polymer sulfonic acid, polyvinyl sulfonic acid, etc. can be cited. As a polymer carboxylic acid, for example, polyacrylic acid, polymethacrylic acid, polymaleic acid can be exemplified. In addition, as a polymer sulfonic acid, for example, polystyrene sulfonic acid can be exemplified. From the perspective of antistatic properties, polystyrene sulfonic acid is particularly preferred. It should be noted that these acidic polymers can take the form of partially neutralized salts. In addition, they can also be used in the form of copolymerization with other copolymerizable monomers, such as acrylates, methacrylates, styrene, etc. There is no particular restriction on the molecular weight of polymer carboxylic acids and polymer sulfonic acids. From the perspective of the stability and antistatic properties of the coating agent, the weight average molecular weight is preferably 1,000 or more and 1,000,000 or less, and more preferably 5,000 or more and 150,000 or less. In addition, within the range that does not hinder the characteristics of the invention, a portion of alkali metal salts such as lithium salts and sodium salts, ammonium salts, etc. can be included. It is believed that in the case of a salt neutralized with a polyanion, it will also act as a dopant. This is because, for polystyrene sulfonic acid and its ammonium salt, which act as extremely strong acids, the equilibrium shifts to the acidic side due to the progress of equilibrium reaction after neutralization.
[0047] As the compound A having a vinyl alcohol residue mentioned here, polyvinyl alcohol can be preferably used. Since polyvinyl alcohol has a plurality of electron-rich hydroxyl groups, it interacts with the π-type conjugated electrons of the above-mentioned polythiophenes to improve the fluidity of the rigid polythiophene molecular chain. As a result, when the resin layer X is provided in the film-forming of the polyester film by using an online coating method for coating, the coating property of the resin layer X is improved, and the stretching followability is improved. Such film-forming properties can be improved. As a result of the improved film-forming properties, the polythiophene compound is uniformly present in the surface layer of the polyester film as a conductive resin, so that the surface resistivity of the laminated polyester film is reduced, and the antistatic property of the laminated polyester film is improved. In addition, the film-forming properties of the resin layer X are improved. As a result, when the resin layer X is formed by an online coating method, the resin layer X can uniformly cover the surface of the polyester film. As a result, for example, when the laminated polyester film having the resin layer X is heat-treated, the oligomers contained in the polyester film rarely seep out on the surface of the resin layer X, which can improve the heat resistance.
[0048] The saponification degree of polyvinyl alcohol is preferably 70 to 100, more preferably 80 to 100. Polyvinyl alcohol has hydroxyl groups and acetic acid groups as side chains, and a higher saponification degree indicates a greater amount of hydroxyl groups. Therefore, the higher the saponification degree, the easier it is to obtain the above-mentioned effect.
[0049] The degree of polymerization of compound A is preferably 50 to 1,000, more preferably 100 to 800, and even more preferably 300 to 600. Within the above preferred range, the fluidity of the rigid polythiophene molecular chain can be improved, coating properties are improved, and lamination becomes easy.
[0050] In addition, as the side chain of the polyvinyl alcohol resin used as the resin layer X, it is also a preferred embodiment to use a copolymerized polyvinyl alcohol copolymerized with a functional group other than a hydroxyl group and an acetic acid group. It is particularly preferred to introduce a hydrophilic functional group, such as a 1,2-ethylene glycol group, a carboxyl group, a sodium sulfonate group, etc. As for the copolymerization amount, it is preferably 1 mol% or more and 20 mol% or less, and more preferably 3 mol% or more and 10 mol% or less relative to the entire polyvinyl alcohol resin. When the copolymerization amount is within the above preferred range, the coating property is good and lamination becomes easy.
[0051] The laminated polyester film of the present invention preferably has an epoxy group content in the solid content of the resin layer X measured from the laminated polyester film under the following specific extraction and analysis conditions of 5 mg / g or more and 100 mg / g or less.
[0052] <Extraction conditions>
[0053] Cut 0.5m 2 The laminated polyester film was cut and placed in a flask with 80 mL of water, and layer X was extracted while ultrasonic cleaning was performed at 40 kHz and an output of 360 W for 30 minutes. The obtained aqueous solution was filtered to remove impurities, and then the solvent was removed by freeze drying to obtain a solid component.
[0054] <Analysis conditions>
[0055] The obtained solid components were extracted with heavy water and measured under the following conditions: 1 HNMR: The epoxy group was quantified based on the peak area derived from the obtained epoxy group.
[0056] Device: ECZ-600R (manufactured by JEOL Resonance Co., Ltd.)
[0057] Measurement method: Single pulse
[0058] Measurement frequency: 600.17MHz
[0059] Pulse width: 5.88μs
[0060] Chemical shift standard: TSP (sodium 3-trimethylsilylpropionate-2,2,3,3-d) 4 (0ppm)
[0061] Total times: 16 times
[0062] Measurement temperature: 20℃
[0063] Sample speed: 15Hz
[0064] When obtaining the spectrum, a known amount of sodium 3-(trimethylsilyl) propionate (TSP) was added as an internal standard. From the obtained spectrum, the peak area Ea observed at 2.7 ppm derived from the epoxy group and the peak area Ta observed at 0 ppm derived from the internal standard were calculated. The amount of epoxy groups equivalent to Ea was calculated from the ratio of Ea to Ta and the amount of the added standard sample, and was taken as the amount of epoxy groups in layer X.
[0065] Examples of the state in which the epoxy group content in the solid content of the resin layer X determined by the above method is less than 5 mg / g include a state in which the resin layer X does not contain an epoxy compound, a state in which the crosslinking reaction by the crosslinking agent or the binder proceeds excessively even if the epoxy compound is contained, or a state in which the resin layer X is insoluble in water.
[0066] The epoxy group content in the solid component of the resin layer X obtained by the above method is 5 mg / g or more, so that the film-forming property of the resin layer X is improved, the compound B can be more uniformly present in the surface layer of the polyester film, the surface resistivity of the laminated polyester film is reduced, and the antistatic property of the laminated polyester film can be improved. In addition, when the polyester film is immersed in water, water easily penetrates into the resin layer X, and the resin layer X is easily removed by water extraction and the film is cleaned. In addition, by making the epoxy group content in the solid component of the resin layer X obtained by the above method 100 mg / g or less, the film-forming property of the resin layer X can be improved.
[0067] In order to make the epoxy group content in the solid content of the resin layer X of the laminated polyester film of the present invention within the above range, it is a preferred embodiment to further contain an epoxy compound (compound C) in addition to compound A and compound B. As compound C, for example, sorbitol polyglycidyl ethers, polyglycerol polyglycidyl ethers, polyethylene glycol diglycidyl ethers, polyhydroxyalkane polyglycidyl ethers, etc. can be used. For example, the epoxy compounds "Denacol" (EX-611, EX-614, EX-614B, EX-512, EX-521, EX-421, EX-313, EX-810, EX-830, EX-850, etc.) manufactured by Nagase Chemtex Co., Ltd., diepoxy / polyepoxy compounds (SR-EG, SR-8EG, SR-GLG, etc.) manufactured by Sakamoto Pharmaceutical Industries, Ltd., and the epoxy crosslinking agent "EPICLON" (EM-85-75W, CR-5L) manufactured by DIC Corporation can be preferably used. Among them, water-soluble substances are preferred.
[0068] The epoxy compound has a three-membered ring containing an oxygen atom, so the electrons of the oxygen atom easily interact with other molecules. In the film of the present invention, the epoxy compound interacts with the compound B having a thiophene residue contained in the resin layer X to improve the fluidity of the rigid polythiophene molecular chain. As a result, when the resin layer X is provided in the film formation of the polyester film by coating using an online coating method, the film formation of the resin layer X can be improved by improving the coating property of the resin layer X and improving the stretching followability. As a result of the improved film formation of the resin layer X, the polythiophene compound as a conductive resin is uniformly present in the surface layer of the polyester film, thereby reducing the surface resistivity of the laminated polyester film and improving the antistatic property of the laminated polyester film.
[0069] Furthermore, as a result of the improved fluidity of the resin layer X, when the polyester film of the present invention is immersed in water, water easily permeates into the resin layer X. Therefore, the compound A having a vinyl alcohol residue contained in the resin layer X dissolves in water, and as a result, the resin layer X can be extracted with water. Since the resin layer X can be extracted with water, the resin layer X can be washed with water or the like to recover only the polyester film and reuse it.
[0070] In order to improve the fluidity of the resin layer X, the molecular weight of the compound C is 10,000 or less, preferably 5,000 or less, and more preferably 1,000 or less.
[0071] In order to improve the fluidity of the resin layer X and improve the extractability with water, when the converted mass of the resin layer X of the laminated polyester film of the present invention is set to 100 mass%, the total organic component amount in the solid content of the resin layer X extracted under the following specific extraction conditions is preferably 90 mass% or more.
[0072] <Extraction conditions>
[0073] Cut 0.5m 2 The laminated polyester film was cut and placed in a flask with 80 mL of water, and the resin layer X was extracted while ultrasonic cleaning was performed at 40 kHz and an output of 360 W for 30 minutes. The obtained aqueous solution was filtered to remove impurities, and then the solvent was removed by freeze drying to obtain a solid component.
[0074] It should be noted that the converted mass of the resin layer X mentioned here is obtained by measuring the thickness of the resin layer X by the method described later, calculating the volume of the resin layer X, and then accumulating the density of the organic component, that is, the density 1.0. That is, the percentage of the value obtained by dividing the mass of the solid content of the resin layer X obtained by the above-mentioned specific extraction method by the converted mass of the resin layer X is preferably 90% by mass or more.
[0075] By adopting this embodiment, it is possible to extract the resin layer X with water. Thereby, the resin layer X can be washed with water or the like, and only the polyester film can be recovered and reused.
[0076] In order to set the total amount of organic components extracted under the above extraction conditions within the above range, the resin layer X preferably does not contain a resin having a crosslinking point with other components represented by urethane resins, polyester resins, acrylic resins, etc., so-called binder resins having N (nitrogen) elements and carbonyl groups. In the case of not containing a binder resin containing an N element and a carbonyl group having a crosslinking point with other components, for example, it is difficult to form a crosslinking structure with the compound A in the present invention, and no hydrophobicity is formed, so the resin layer X can be extracted under the above conditions.
[0077] That is, in order to be able to extract the resin layer X under the above conditions, the laminated polyester film of the present invention, in 100% by mass of the above-mentioned resin layer X, the total content of the compound A having a vinyl alcohol residue, the compound B having a thiophene residue and the epoxy compound C is preferably 90% by mass or more, the total content of the compounds A to C is more preferably 95% by mass or more, further preferably 98% by mass or more, and particularly preferably 99% by mass or more.
[0078] In addition, the ratio of compound A to compound C contained in the resin layer X in the laminated polyester film of the present invention is preferably 10 parts by mass or more and 300 parts by mass or less of compound C relative to 100 parts by mass of compound A. More preferably, it is 20 parts by mass or more and 180 parts by mass or less. When the ratio of compound A to compound C contained in the resin layer X is within the above preferred range, a film having excellent antistatic properties and excellent extractability of the resin layer X in water is formed.
[0079] The resin layer X in the present invention preferably has adhesion M(X) that satisfies the following conditions.
[0080] M(X)≥90(%)
[0081] In the present invention, the adhesiveness M(X) of the resin layer X is measured as follows.
[0082] A 5 cm square film with a resin layer X was cut with a load of 10 g to form a grid of 0.5 cm square. A 31B tape manufactured by Nitto Denko Co., Ltd. was attached to the cut portion and then peeled off. The number of grids where the resin layer X was not transferred to the tape side was counted and expressed as a percentage.
[0083] The fact that the adhesion M(X) of the resin layer X satisfies the above range means that the adhesion between the resin layer X and the polyester film is high. By adopting this embodiment, the heat resistance of the laminated polyester film can be improved. As a method for making the adhesion M(X) of the resin layer X within the above range, a method in which the resin layer X contains compound A and compound B to improve film forming properties can be preferably cited. In addition, as a method for forming the resin layer X, a so-called online coating method having a step of coating the above-mentioned resin layer X-forming coating agent on a polyester film and a step of stretching the polyester film in sequence is also a preferred embodiment. In the online coating method, since the resin layer X is formed while stretching the polyester film, as the polyester film is stretched, the area of the contact surface between the polyester film and the resin layer X becomes larger, thereby improving the adhesion. As a result, M(X) can be set within the above range.
[0084] The laminated polyester film of the present invention preferably comprises a polyester film, the above-mentioned resin layer X, and a resin layer Y in this order. The resin layer Y is located on the outermost layer of the laminated polyester film and is a functional layer that exhibits the performance as a laminated polyester film. By laminating the resin layer Y on the outermost layer via the resin layer X having antistatic properties, the resin layer Y exhibits antistatic properties, and when the laminated film of the present invention is subjected to heat in the process, it is possible to suppress process contamination caused by the seepage of components contained in the resin layer X, such as components exhibiting antistatic properties, or to suppress the reduction of the function as a laminated film. In addition, when the polyester film of the present invention is used as a process film, the resin layer Y is preferably formed of a resin having mold release properties. As the resin having mold release properties, organic silicon compounds having a compound having a siloxane bond as a main component, compounds having a long-chain alkyl group, and compounds having fluorine can be listed. Here, the so-called resin layer Y having a compound having a siloxane bond as a main component means that the part having a siloxane bond contains 80 mol% or more in the compound. Among them, organic silicon compounds (organopolysiloxanes) having a compound having a highly hydrophobic siloxane bond as a main component are preferred, and resins composed of curable organic silicon compounds can be particularly preferably used. As resins composed of curable organic silicon compounds, there can be cited "addition reaction type" in which organic hydrogen polysiloxane and organic polysiloxane containing alkenyl groups are cured by heating using a platinum catalyst, "condensation reaction type" in which organic hydrogen polysiloxane and organic polysiloxane containing hydroxyl groups at the end are cured by heating using an organic tin catalyst, "UV curing type" in which a photopolymerization initiator is added to organic polysiloxane containing acryloyl groups or methacryloyl groups, or organic polysiloxane containing alkenyl groups and organic polysiloxane containing mercapto groups and cured by irradiation with UV light, and "cationic polymerization type" in which an epoxy group is cured by photo-ring opening using an onium salt initiator. In particular, when a resin having a vinyl alcohol residue is used in the resin layer X, an addition reaction type organopolysiloxane in which an organohydrogenpolysiloxane and an organopolysiloxane containing an alkenyl group are cured by heating using a platinum catalyst is preferred for the reasons described below. From the perspective of hydrophobicity and compound production, dimethylpolysiloxane is preferred as the organopolysiloxane.
[0085] In the laminated polyester film of the present invention, the surface resistivity of the surface of the resin layer Y preferably satisfies the following formula (1) and formula (2).
[0086] (1)10 6 ≤Ω (0) ≤10 10
[0087] (2)Ω (150) / Ω (0) <50
[0088] In formula (1) and formula (2), Ω (0) represents the surface resistivity (Ω / sq) of the resin layer Y before heat treatment, Ω(150) It shows the surface resistivity (Ω / sq) of the surface of the resin layer Y after heat treatment at 150°C for 60 minutes.
[0089] By making Ω (0) When the above formula (1) is satisfied, the antistatic property is sufficient, and when the laminated polyester film is used as a process film, the mold release object can be easily peeled off from the film. On the other hand, since the conductivity does not become too high, it can be suppressed from becoming a major cause of short circuit when used in various processes.
[0090] By making Ω (150) / Ω (0) When the above range is used, the antistatic property of the surface of the resin layer Y of the laminated polyester film of the present invention is less damaged by heat. When the laminated polyester film of the present invention is used as a process film, the influence of heating during the process is less, so it can be used as a variety of process films, which is preferred.
[0091] In order to satisfy the above formula (2), the amount of the antistatic agent contained in the resin layer Y as the outermost layer forming the laminated polyester film is less than 0.1% by mass relative to the resin layer Y, and it is particularly preferred that it is substantially free of antistatic agent. The antistatic agent referred to herein refers to a material that exhibits antistatic properties by being contained in the resin layer Y, and examples thereof include ion-conductive polymer compounds such as ammonium compounds, polyether compounds, sulfonic acid compounds, and betaine compounds, and π-electron conjugated polymer compounds such as polyacetylene, polyphenylene, polyaniline, polypyrrole, polyisothiophthalene, and polythiophene. In the case where the resin layer Y does not substantially contain an antistatic agent, even when heat is applied to the laminated polyester film, the antistatic agent is not easy to seep out to the outermost surface of the laminated polyester film, and the laminated polyester film maintains its original conductivity, thereby satisfying formula (2).
[0092] In addition, in order to satisfy the above formula (1) and formula (2), it is preferred that the resin layer Y does not substantially contain an antistatic agent, and the layer in contact with the resin layer Y is a layer having antistatic properties. Furthermore, in order to satisfy the above formula (1), the thickness of the resin layer Y is preferably set to 300 nm or less, more preferably 100 nm or less, and further preferably 50 nm or less. In order to play the role of a functional layer of the resin layer Y, the thickness of the resin layer Y is preferably 20 nm or more. By setting the thickness of the resin layer Y to the above range, the antistatic property of the layer in contact with the resin layer Y (resin layer X in the laminated polyester film of the present invention) is utilized, and the above formula (1) is easily satisfied.
[0093] In the film of the present invention, the resin layer X contains the compound A having a vinyl alcohol residue and the compound B having a thiophene residue. The interaction between the compound A and the compound B improves the fluidity of the layer X, and as a result, it is possible to suppress the generation of fine defects such as fine coating omissions and microcracks in the resin layer X. When the resin layer Y is provided in contact with the resin layer X to form a laminated polyester film, it is possible to suppress the generation of fine defects such as fine coating omissions and microcracks in the resin layer Y. As a result, when the laminated polyester film of the present invention is heated, the oligomers generated from the polyester film are less likely to ooze out into the resin layer Y, and the heat resistance is improved. As a result, the above formula (2) can be within a preferred range.
[0094] In addition, as the compound having antistatic property contained in the resin layer X, from the viewpoint of heat resistance, the compound B having a thiophene residue is preferred, and a polythiophene compound is particularly preferred. In particular, when the resin layer X contains the compound B as a high molecular weight body, compared with the case where the resin layer X contains the antistatic agent as a low molecular weight body, the antistatic agent contained in the resin layer X can be suppressed from seeping into the resin layer Y to reduce the heat resistance.
[0095] When an addition reaction type organopolysiloxane is used as the resin layer Y of the laminated polyester film of the present invention, the organopolysiloxane is obtained by reacting hydrogen organopolysiloxane with an alkenyl group-containing organopolysiloxane by addition reaction with a platinum catalyst, but it is known that hydrogen organopolysiloxane can also undergo a condensation reaction with a compound having a hydroxyl group by means of a platinum catalyst (International Publication Patent Document WO2014 / 099497). When the resin layer Y contains hydrogen organopolysiloxane and the resin layer X in contact with the resin layer Y contains polyvinyl alcohol, the hydrogen organopolysiloxane condenses with the polyvinyl alcohol, and the adhesion at the interface between the resin layer X and the resin layer Y is improved, which is preferred. As a result of the improved adhesion between the resin layer X and the resin layer Y, even when heat is applied to the laminated polyester film having the resin layer X and the resin layer Y, the oligomers contained in the polyester film will not precipitate on the surface, and the antistatic property, transparency, and demolding property of the laminated polyester film will not be impaired, and the above formula (1) and formula (2) can be satisfied.
[0096] The resin layer X preferably does not contain a resin having a crosslinking point with other components represented by polyurethane resins, polyester resins, acrylic resins, etc., or a so-called binder resin having an N (nitrogen) element or a carbonyl group. In the case where a binder resin having an N element or a carbonyl group having a crosslinking point with other components is not contained, for example, the compound A in the present invention does not form a crosslinking structure with the binder resin, and thus the effect of improving the adhesion at the interface between the resin layer Y and the resin layer X can be obtained.
[0097] The surface free energy of the resin layer Y of the laminated film of the present invention is preferably 30 mN / m or less. More preferably, it is 15 mN / m or less. The lower limit is not particularly set, but is a value exceeding 0 mN / m according to the calculation method of the surface free energy. If the surface free energy of the resin layer Y is within the above-mentioned preferred range, when the laminated polyester film is used as a process film, particularly as a process film for demolding from a demolding object, the demolding object has excellent demolding properties.
[0098] The haze change of the laminated film of the present invention after heat treatment at 150°C for 60 minutes is preferably 10% or less. More preferably, it is 5% or less. The lower limit is not particularly set, but according to the calculation method of the haze change, it is 0% or more. When the haze change after heat treatment at 150°C for 60 minutes is within the above preferred range, there are few oligomers precipitated on the surface of the laminated film, and it is easy to control the surface resistivity of the resin layer Y surface to a preferred value. In addition, the laminated film has excellent performance when used as a process film in the processing steps of various industrial products.
[0099] The laminated polyester film of the present invention preferably has a solvent durability of the surface of the resin layer Y measured in accordance with JIS L 0849 (2013) (friction tester type II) of 50% or more and 100% or less.
[0100] As described above, since the adhesion between the resin layer X and the resin layer Y is improved, the wear resistance of the resin layer Y is improved, and the solvent durability can be made into a preferred range. The upper limit of the solvent durability is 100%. If the solvent durability is in the preferred range, it is suitable for use as a process film.
[0101] In the laminated polyester film of the present invention, it is preferred that the water contact angle on the resin layer Y side satisfies the following formula (3) and formula (4).
[0102] (3) 0°≤HYa≤80°
[0103] (4) 10°≤HYp-HYa≤100°
[0104] Here, HYp represents the water contact angle on the resin layer Y side of the laminated polyester film, and HYa represents the water contact angle on the resin layer Y side of the laminated polyester film after the laminated polyester film is immersed in pure water at 25° C. for 5 minutes.
[0105] The laminated polyester film of the present invention satisfies the above formula (3) and formula (4), which means that the water contact angle of the resin layer Y changes after being immersed in pure water at 25°C for 5 minutes, and also means that the water contact angle after being immersed in pure water at 25°C is not too large, that is, it can be close to the water contact angle of the polyester film, and the resin layer Y is in a state that can be washed and peeled off with water. By satisfying this embodiment, the resin layer Y can be washed with water, and when the laminated polyester film of the present invention is washed, for example, by the method described later, the polyester film as the substrate can be easily taken out and reused, which is preferred.
[0106] As a method for making the laminated polyester film of the present invention satisfy the above formula (3), it is also a preferred embodiment to easily extract the resin layer X with water. From the perspective of easily extracting the resin layer X with water, the epoxy group content in the solid content of the resin layer X is preferably 5 mg / g or more and 100 mg / g or less.
[0107] In addition, from the viewpoint of mold releasability, HYp ≥ 90° is more preferred.
[0108] The ratio of compound A to compound B contained in the resin layer X in the laminated polyester film of the present invention is 10 parts by mass or more and 700 parts by mass or less of compound B relative to 100 parts by mass of compound A. More preferably, it is 10 parts by mass or more and 300 parts by mass or less. When the ratio of compound A to compound B contained in the resin layer X is within the above preferred range, the antistatic property is excellent, and on the other hand, the film forming property is excellent, and as a result, the heat resistance and antistatic property can be excellent.
[0109] Next, a method for producing the laminated polyester film of the present invention will be described below, but the present invention is not limited to the laminated polyester film obtained by this method.
[0110] The polyester film used in the present invention can be processed into a sheet by heating and melting the raw material dried as needed in an extruder and extruding it from a die onto a cooled casting drum (melt casting method). The sheet is cooled and solidified by electrostatic contact on a drum whose surface temperature is cooled to 20°C or more and 60°C or less to form an unstretched sheet. The temperature of the casting drum is more preferably 20°C or more and 40°C or less, and more preferably 20°C or more and 30°C or less.
[0111] Next, the unstretched sheet is biaxially stretched at a temperature T1n (°C) satisfying the following formula (i) to be stretched to 3.6 times or more in the length direction (MD) of the film and to be stretched to 3.9 times or more in the width direction (TD) of the film so that the area ratio is 14.0 times or more and 20.0 times or less.
[0112] The stretching ratio in the film width direction is preferably 3.0 times or more, more preferably 3.5 times or more and 5.0 times or less. By setting the stretching ratio in the film width direction to 3.0 times or more, when the resin layer X is coated on the uniaxially stretched film using the online coating method described later, the components constituting the resin layer X will follow the film to be stretched and extended, so that the resin layer X can be uniformly provided. When the width direction stretching ratio is within the above preferred range, the film forming property of the film is excellent.
[0113] (i)Tg(℃)≤T1n(℃)≤Tg+40(℃)
[0114] In the above formula (i), Tg represents the glass transition temperature (° C.) of the polyester film.
[0115] The method of stretching the polyester film in the longitudinal direction is preferably a method utilizing a speed difference between rollers. In this case, it is also a preferred embodiment to stretch the polyester film in a plurality of sections while fixing the polyester film with a nip roller so that the polyester film does not slip.
[0116] Next, the biaxially stretched polyester film is subjected to a heat setting treatment at a temperature (Th0 (° C.) satisfying the following formula (ii) for 1 second to 30 seconds, and then cooled uniformly and slowly to room temperature to obtain a polyester film used in the present invention.
[0117] (ii)Tmf-35(℃)≤Th0(℃)≤Tmf(℃)
[0118] In the above formula (ii), Tmf represents the melting point (° C.) of the film.
[0119] By obtaining a biaxially stretched film satisfying the condition (ii), it is possible to impart a suitable orientation to the film, and to improve the handling properties when used as a release film.
[0120] Next, a method for providing the resin layer X and the resin layer Y on the above-mentioned polyester film will be described below.
[0121] As the components constituting the resin layer X, when compound A and compound B are contained as described above, especially when compound B is obtained in the form of an aqueous dispersion, it is preferred to use a method in which compound A and compound B forming the resin layer X are dissolved or dispersed in water and applied on the polyester film of the present invention. As a coating method, conventional coating methods such as gravure coating, Meyer rod coating, air knife coating, and blade coating can be used. In particular, from the perspective of uniformly setting the resin layer X, it is preferred to use a resin for coating the surface layer of the polyester film after uniaxial stretching in the length direction, and an online coating method in which the resin layer X is formed while the polyester film is stretched in the width direction. The thickness of the resin layer X is preferably 50 nm or more and 1,000 nm or less. If the thickness of the resin layer X is in the preferred range described above, the resin layer X can be evenly coated on the surface of the polyester film, adhesion is not easy to occur, and the operability is excellent.
[0122] Next, the method for setting the resin layer Y is described. The resin layer Y can be set at the same time as the resin layer X, or can be set separately. In the case of setting at the same time, there can be cited a method of simultaneously coating the two layers using a mold, etc., or a method of coating using a coating agent formed by pre-mixing the components of the resin layer X and the components of the resin layer Y. In order to improve the lamination accuracy of the resin layer X and the resin layer Y, it is preferred that the resin layer X and the resin layer Y are set separately. A coating liquid in which the components of the resin layer Y are dissolved can be used, and a conventional coating method such as gravure coating, Meyer rod coating, air knife coating, and blade coating can be used to coat the laminated polyester film containing the resin layer X obtained by the above method. The thickness of the resin layer Y is preferably greater than 10 nm and less than 1,000 nm. When the thickness of the resin layer Y is in the above preferred range, the function of the resin layer Y is fully manifested, and on the other hand, the antistatic property can be fully manifested.
[0123] The laminated polyester film of the present invention, as described above, is obtained by providing a resin layer X containing at least two of a compound A having a vinyl alcohol residue and a compound B having a thiophene residue on at least one side of the polyester film, and then providing a resin layer Y having a release function. The laminated polyester film can be suitably used as a release film for process use or a laminated film with other functional layers.
[0124] Next, a method for washing the laminated polyester film of the present invention with water is described below, but is not limited thereto.
[0125] The laminated polyester film of the present invention is preferably provided to the process of unwinding the laminated polyester film, the process of providing warm water to the surface of the unwinding laminated film and peeling the surface laminated portion from the laminated film, and the process of winding the peeled polyester film. The temperature of the warm water is preferably above 50°C and below 120°C. If it is in the above-mentioned preferred temperature range, sufficient cleaning performance can be obtained. On the other hand, since the glass transition temperature of the polyester film is not exceeded, it will not cause obstacles to the film transportation. The time for water to contact the surface of the laminated polyester film is more than 5 seconds, preferably more than 10 seconds, and more preferably more than 30 seconds and less than 600 seconds. The process of providing warm water to the surface of the unwinding laminated film is preferably carried out in a water tank, covering the entire laminated film. By covering the entire laminated polyester film with warm water, water pressure is generated in the direction of film flow, and the cleaning performance is improved. The speed of conveying the film is more than 5m / minute, preferably more than 10m / minute, and more preferably more than 20m / minute and less than 100m / minute. It is also important to apply tension to the laminated film when conveying the laminated polyester film in this process. By applying tension, the surface of the laminated polyester film can be stretched, and the washability can be improved. The tension is 5 N / m or more and 1,000 N / m or less, more preferably 20 N / m or more and 800 N / m or less, and further preferably 30 N / m or more and 500 N / m or less. In the case of the preferred tension range, the surface of the laminated polyester film is stretched, and the washability is excellent. On the other hand, the film is not easy to wrinkle, the surface stretchability is excellent, and the washability becomes good.
[0126] [Evaluation method of characteristics]
[0127] (I) Residues of Compound A and Compound B
[0128] The resin layer X or the resin layer Y of the laminated polyester film was analyzed from the surface in the depth direction under the following conditions. As secondary ions, C 4 H 5 O - ions, the resin layer X has vinyl alcohol residues, and C 6 HS - When , the resin layer X has a thiophene residue.
[0129] <Measurement conditions>
[0130] Device: TOF.SIMS 5 (manufactured by ION-TOF)
[0131] Pulse width: 100ns
[0132] Secondary ion polarity: positive
[0133] Post-acceleration: 9.5kV
[0134] Mass range (m / z): 0 to 1,500
[0135] Grating size: 40μm square
[0136] Scan number: 64scan
[0137] Number of pixels (one side): 256 pixels
[0138] Primary ion species: Bi
[0139] Measurement vacuum degree (before sample introduction): 4×10 -7 Below Pa
[0140] Primary ion acceleration voltage: 30kV
[0141] Etching ions: Argon cluster ions.
[0142] (II) Thickness of each resin layer
[0143] The thickness of each resin layer of the laminated polyester film was determined by the following method: A cross section of the laminated polyester film was cut using a microtome in a direction parallel to the width direction of the laminated polyester film. The cross section was observed using a scanning electron microscope at a magnification of 5000 times to measure the thickness of each resin layer of the laminated polyester film.
[0144] (III) Surface resistivity (Ω / sq)
[0145] After the sample was left at 25°C and 65% relative humidity for 24 hours, it was measured in this atmosphere using a digital ultra-high resistance / micro-ammeter R8340A manufactured by Advantest with an applied voltage of 100 V. Five points were randomly selected from the laminated polyester film for measurement, and the average value was determined as the surface resistivity.
[0146] (III-1) Surface resistivity after heat treatment at 150°C for 60 minutes
[0147] The laminated polyester film was cut into 20 cm squares, attached to a metal frame, and left to stand for 1 hour in a 150°C hot air oven (PH-302 manufactured by TABI ESPEC Co., Ltd.). The laminated polyester film was then removed from the metal frame and the surface resistivity was measured according to item C., and the result was expressed as Ω. (150) .
[0148] (IV) Haze change after heat treatment at 150°C for 60 minutes (Δhaze) (%)
[0149] The laminated polyester film was cut into 20 cm squares, and the haze was measured and taken as H(0). The laminated polyester film was attached to a metal frame and left to stand for 1 hour in a hot air oven (PH-302 manufactured by Timespace Co., Ltd.) at 150°C. Then, the laminated polyester film was removed from the metal frame and the haze was measured and taken as H(0). (150)From H (150) Subtract H (0) , as the change in haze (Δ haze) after heat treatment at 150°C for 60 minutes.
[0150] The haze value was measured according to JIS K 7136 (2000) using NDH-5000 manufactured by Nippon Denshoku Industries Co., Ltd. Five locations were randomly selected from the laminated polyester film for measurement, and the average value was calculated.
[0151] (V) Solvent durability of resin layer Y
[0152] The measurement was performed by the following method using a Gakushin type testing machine (in accordance with JIS L 0849 (2013)) manufactured by Daiei Kagaku Seiki Mfg. Co., Ltd.
[0153] [Friction treatment with solvent-impregnated cloth]
[0154] The surface of the resin layer Y of the film was subjected to a rubbing treatment using the following testing machine and rubbing head.
[0155] Testing machine: Gakushin type testing machine (friction testing machine type II described in JIS L 0849 (2013))
[0156] Friction head: Cotton cloth soaked in toluene (No. 3 fine white cloth)
[0157] Load: 1.0kg
[0158] Number of times: 30 round trips.
[0159] [Peeling treatment]
[0160] A polyester adhesive tape (Nitto Denko Corporation No. 31B, width 19 mm) was pressed with a 2.0 kg roller and attached to the portion of the resin layer Y surface that had been rubbed with a solvent-impregnated cloth. After standing for 24 hours in an atmosphere of 23°C and 65% RH, the peeling force between the sample surface and the polyester adhesive tape was measured using a VPA-H200 peel tester manufactured by Kyowa Interface Science Co., Ltd. at a peeling angle of 180° and a peeling speed of 300 mm / min. The peeling force F(B) of the resin layer Y surface after the rubbing treatment with the solvent-impregnated cloth was calculated by converting it into a 50 mm width. The peeling force F(A) of the resin layer Y surface before the rubbing treatment with the solvent-impregnated cloth was also measured using the same method, and the solvent durability was determined based on the following formula.
[0161] Solvent durability (%) = F(A) / F(B)×100.
[0162] (VI) Copolymerization amount of compound A (mol%)
[0163] Using the following device,13 The copolymerization amount (mol %) was determined from the peak area of the carbon signal introduced by the modified group in the CNMR spectrum and the DEPT135 spectrum.
[0164] Equipment: ECZ-600R (manufactured by JEOL Resonance Co., Ltd.)
[0165] Measurement method: Single 13 C pulse with inversegated 1 H decoupling
[0166] Measurement frequency: 150.9MHz
[0167] Pulse width: 5.25μs
[0168] Lock solvent: D 2 O
[0169] Chemical shift standard: TSP (0ppm)
[0170] Cumulative times: 10,000 times
[0171] Measurement temperature: 20℃
[0172] Sample rotation speed: 15Hz.
[0173] (VII) Saponification degree of compound A
[0174] The amount of acetic acid groups contained in the sample was quantitatively determined and calculated by titration with an aqueous sodium hydroxide solution in accordance with JIS K 6726 (1994) polyvinyl alcohol testing method.
[0175] (VIII) Average degree of polymerization of compound A
[0176] According to the polyvinyl alcohol testing method of JIS K 6726 (1994), a sample was completely saponified with an aqueous sodium hydroxide solution, and then the viscosity at 25° C. was measured using an Ostwald viscometer, and the average degree of polymerization was calculated from the intrinsic viscosity.
[0177] (IX) Surface free energy (mN / m)
[0178] The contact angle meter DM501 manufactured by Kyowa Interface Science Co., Ltd. and the accompanying analysis software FAMAS were used to measure the surface of the resin layer Y by the following method. Glycerin, ethylene glycol, formamide, and diiodomethane were used as standard liquids to obtain the static contact angle of each liquid at 25° C. The static contact angle of each liquid and the dispersion component, polar component, and hydrogen bond component of the surface free energy of each liquid described in the non-patent document 1 were introduced into the "Extended Hawkes formula of Hata and Kitasaki" described in the non-patent document (J. Panzer: J. Colloid Interface Sci., 44, 142 (1973).), and the simultaneous equations were solved to obtain the dispersion component, polar component, and hydrogen bond component of the surface free energy of the layer Y, and the total of these values was taken as the surface free energy.
[0179] The static contact angle was measured by leaving the sample to stand for 12 hours in an environment of 25°C. The time when the droplet was in contact with the sample surface was regarded as 0 seconds. The static contact angle was calculated using the θ / 2 method using the image taken 30 seconds later. The position was changed and the measurement was repeated 5 times. The average value of the static contact angle was used to calculate the dispersion component, polar component, and hydrogen bond component of the surface free energy of the resin layer X and the resin layer Y.
[0180] (IX) Application as process membrane
[0181] (IX-1) For green sheet molding
[0182] [Preparation of dielectric paste]
[0183] Glass beads with a number average particle size of 2 mm are added to 100 parts by mass of barium titanate (manufactured by Fuji Titanium Industry Co., Ltd., trade name HPBT-1), 10 parts by mass of polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd., trade name BL-1), 5 parts by mass of dibutyl phthalate and 60 parts by mass of toluene-ethanol (mass ratio 30:30), and the mixture is mixed and dispersed using a jet mill for 20 hours, and then filtered to prepare a paste-like dielectric paste.
[0184] [Peel force (mN / 50mm)]
[0185] The dielectric paste was applied to the surface of layer Y of the laminated film by die coating in a manner that the thickness after drying was 0.1 μm, and the paste was dried and cured at 100°C for 60 seconds. A polyester adhesive tape (No. 31B manufactured by Nitto Denko Co., Ltd., width 19 mm) was attached to the surface of the dielectric paste of the laminated polyester laminated with the dielectric paste, and the 180° peel strength was measured at a peeling speed of 300 mm / min using VPA-H200 manufactured by Kyowa Interface Science Co., Ltd., converted to a width of 50 mm. According to the size of the peeling force, the following evaluation was performed. Evaluation A was the best.
[0186] Evaluation A: 35mN / 50mm or less
[0187] Evaluation B: greater than 35mN / 50mm and less than 45mN / 50mm
[0188] Evaluation C: greater than 45mN / 50mm and less than 55mN / 50mm
[0189] Evaluation D: greater than 55 mN / 50 mm.
[0190] [Frequency of rupture]
[0191] A rectangular cut with a long side in the length direction of the film was cut in a manner of 50 mm in width and 150 mm in length on the dielectric paste of the laminated polyester laminated with the dielectric paste. A polyester adhesive tape (Nitto Denko Co., Ltd., No. 31B, width 19 mm) was pasted to the center of any short side of the cut so that the adhesive portion became 10 mm in the length direction of the cut, and the dielectric paste was peeled off at an angle of 180° and a speed of 300 mm / min using VPA-H200 manufactured by Kyowa Interface Science Co., Ltd. The above measurement was performed 30 times, and the following evaluation was performed based on the number of times the dielectric paste was broken during the peeling. Evaluation A was the best.
[0192] Rating A: Less than 5 times
[0193] Evaluation B: 5 times or more and less than 10 times
[0194] Evaluation C: 10 times or more and less than 15 times
[0195] Rating D: More than 15 times.
[0196] [evaluate]
[0197] The peeling force and the cracking frequency were evaluated according to the above standards, and the one that was not excellent in the two evaluations was adopted as the evaluation result.
[0198] (IX-2) Adhesive transfer
[0199] [Manufacturing of adhesive]
[0200] After adding 97 parts by mass of butyl acrylate, 3 parts by mass of acrylic acid, 0.2 parts by mass of azobisisobutyronitrile as a polymerization initiator and 233 parts by mass of ethyl acetate, nitrogen was introduced and nitrogen replacement was performed for about 1 hour while stirring. Then, the flask was heated to 60°C and reacted for 7 hours to obtain an acrylic polymer with a weight average molecular weight (Mw) of 1.1 million. To the acrylic polymer solution (the solid content was designated as 100 parts by mass), trimethylolpropane toluene diisocyanate (trade name "コロネート" (registered trademark) L, made by Nippon Polyurethane Industry (Strain)) as an isocyanate crosslinking agent: 0.8 parts by mass and silane coupling agent (trade name "KBM-403", made by Shin-Etsu Chemical Industry (Strain)): 0.1 parts by mass were added to prepare an adhesive composition.
[0201] [Peel force (mN / 50mm)]
[0202] The adhesive was applied to the surface of layer Y of the laminated polyester film by die coating so that the thickness after drying was 10 μm, and dried at 140° C. for 60 seconds. A polyester film #50T60 manufactured by Toray Industries, Ltd. was attached to the surface of the adhesive of the laminated polyester laminated with the adhesive, and cut into a width of 19 mm and a length of 300 mm as a sample. The peeling force at an angle of 180° when peeling the laminated film from the sample was measured at a speed of 300 mm / min using VPA-H200 manufactured by Kyowa Interface Science Co., Ltd., and converted to a width of 50 mm.
[0203] [assessment]
[0204] The peeling force was evaluated as follows: Evaluation A was the best.
[0205] Evaluation A: 120mN / 50mm or less
[0206] Evaluation B: greater than 120mN / 50mm and less than 150mN / 50mm
[0207] Evaluation C: greater than 150 mN / 50 mm and less than 300 mN / 50 mm
[0208] Evaluation D: greater than 300 mN / 50 mm.
[0209] (X) Water contact angle of resin layer Y (HYp, HYa)
[0210] The laminated polyester film was cut into 10 cm squares, and the water contact angle of the surface laminated with layer Y was measured as HYp. Next, the cut laminated polyester film was immersed in pure water at 25°C and stirred for 5 minutes, then the laminated polyester film was taken out, the water on the surface was wiped off, and the water contact angle of the surface laminated with resin layer Y was measured as HYa. For the water contact angle, a contact angle meter DM501 manufactured by Kyowa Interface Science Co., Ltd. and the accompanying analysis software FAMAS were used to measure the angle of the droplet 1 second after the water droplet fell on the surface of the laminated polyester film. The values of HYa and |HYp-HYa| were measured to evaluate the removability of the resin layer Y.
[0211] (XI) Epoxy content of resin layer X (mg / g)
[0212] <Extraction conditions of resin layer X>
[0213] Cut off 0.5m of laminated polyester film 2 The resulting mixture was cut and placed in a flask with 80 ml of water, and layer X was extracted while applying ultrasound at a frequency of 40 kHz and an output of 360 W for 30 minutes. The obtained aqueous solution was filtered to remove impurities, and then the solvent was removed by freeze drying to obtain a solid component.
[0214] <Analysis conditions>
[0215] The solid content obtained by extraction with heavy water was measured under the following conditions: 1 HNMR: The epoxy group was quantitatively determined using the peak area derived from the obtained epoxy group.
[0216] Device: ECZ-600R (manufactured by JEOL Resonance Co., Ltd.)
[0217] Measurement method: Single pulse measurement
[0218] Frequency: 600.17MHz
[0219] Pulse width: 5.88μs
[0220] Chemical shift standard: TSP (sodium 3-trimethylsilylpropionate-2,2,3,3-d 4 )(0ppm)
[0221] Total times: 16 times
[0222] Measurement temperature: 20℃
[0223] Sample speed: 15Hz
[0224] When obtaining the spectrum, a known amount of sodium 3-(trimethylsilyl) propionate (TSP) was added as an internal standard. In the obtained spectrum, the peak area Ea observed at 2.7 ppm derived from the epoxy group and the peak area Ta observed at 0 ppm derived from the internal standard substance were calculated. The amount of epoxy groups equivalent to Ea was calculated from the ratio of Ea to Ta and the amount of the added standard sample, and was taken as the amount of epoxy groups in layer X.
[0225] (XII) Total organic content in the solid content of resin layer X (mass %)
[0226] <Extraction conditions of resin layer X>
[0227] Cut off 0.5m of laminated polyester film 2 After cutting, it was put into a flask with 80 ml of water, and layer X was extracted while ultrasonic washing was performed for 30 minutes at a frequency of 40 kHz and an output of 360 W. The obtained aqueous solution was filtered to remove impurities, and then the solvent was removed by freeze drying to obtain a solid component.
[0228] <Converted mass of resin layer X>
[0229] The thickness of the resin layer X is measured by the above-mentioned method B., and the volume of the resin layer X is calculated, and then the density 1.0 which is the density of the organic component is integrated to obtain the volume.
[0230] <Total amount of organic components in the solid content of the resin layer X>
[0231] The mass of the solid content obtained by the above-mentioned extraction method was measured and divided by the converted mass of the resin layer X to calculate the percentage.
[0232] (XIII) Adhesion M(X) of resin layer X
[0233] A 5 cm square film with a resin layer X was cut with a load of 10 g to form a 0.5 cm square grid. A 31B tape manufactured by Nitto Denko Co., Ltd. was attached to the cut portion and then peeled off. The number of grids where the resin layer X was not transferred to the tape side was counted and expressed as a percentage.
[0234] Example
[0235] Hereinafter, the present invention will be described with reference to Examples, but the present invention is not necessarily limited to these Examples.
[0236] [Manufacturing of PET-1]
[0237] Antimony trioxide and magnesium acetate tetrahydrate were used as catalysts to polymerize terephthalic acid and ethylene glycol using a conventional method to obtain a melt-polymerized polyester having a glass transition temperature of 81°C, a melting point of 255°C, an intrinsic viscosity of 0.65, and a terminal carboxyl group content of 20 eq. / t.
[0238] [Preparation of coating agent M]
[0239] 100 parts by mass of an addition reaction type silicone resin release agent (manufactured by Toray Daw Corning Silicone Co., Ltd., trade name LTC750A) and 2 parts by mass of a platinum catalyst (manufactured by Toray Daw Corning Silicone Co., Ltd., trade name SRX212) were prepared using toluene as a solvent so that the solid content became 5% by mass to obtain a coating agent M.
[0240] [Preparation of coating agent N]
[0241] Coating agent N was obtained by dissolving polyvinyl alcohol "GL-05" (saponification degree 88, average polymerization degree 500) manufactured by Mitsubishi Chemical Corporation as PVA-1 in water to a concentration of 4 mass %.
[0242] [Preparation of coating agent O]
[0243] With reference to Japanese Patent Application Laid-Open No. 9-227627, PVA-2 having a saponification degree of 88, an average polymerization degree of 400, and a copolymerization amount of sodium sulfonate of 1 mol% was prepared. This PVA was dissolved in water to a concentration of 4% by mass to obtain a coating agent O.
[0244] [Preparation of coating agent P]
[0245] With reference to Japanese Patent Application Laid-Open No. 2004-285143, PVA-3 having a saponification degree of 88, an average polymerization degree of 450, and a copolymerization amount of 1,2-ethylene glycol of 6 mol% was prepared. This PVA was dissolved in water to a concentration of 4 mass %, thereby obtaining a coating agent P.
[0246] [Coating Agent Q: Preparation of a Mixture Containing Compound B]
[0247] 49 parts by mass of a 1% iron (III) sulfate aqueous solution, 8.8 parts by mass of 3,4-ethylenedioxythiophene as a thiophene compound, and 117 parts by mass of a 10.9% peroxodisulfuric acid aqueous solution were added to 1887 parts by mass of an aqueous solution containing 20.8 parts by mass of polystyrene sulfonic acid as an acidic polymer compound. The mixture was stirred at 18° C. for 23 hours, and 154 parts by mass of a cation exchange resin (“Lebatt” (registered trademark) Monoplastic S100H) and 232 parts by mass of an anion exchange resin (“Lebatt” (registered trademark) Monoplastic M800) were added to the mixture. After stirring for 2 hours, the ion exchange resin was separated by filtration to obtain a mixture (solid content concentration of 1.3% by mass) composed of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid, which was used as a coating agent Q.
[0248] [Coating agent R: Compound C (epoxy compound)]
[0249] As the coating agent R, a polyglycerol polyglycidyl ether epoxy crosslinking agent (manufactured by Nagase ChemTech Co., Ltd., "Denacol" (registered trademark) EX-512, molecular weight of about 630, epoxy equivalent of 168, water solubility of 100%) was used.
[0250] [Preparation of coating agent S]
[0251] Referring to Japanese Patent Application Laid-Open No. 9-227627, PVA-4 having a saponification degree of 88, an average polymerization degree of 50, and a copolymerization amount of sodium sulfonate of 1 mol% was prepared. This PVA was dissolved in water to a concentration of 4% by mass to obtain a coating agent S.
[0252] [Preparation of coating agent T]
[0253] 10 parts by mass of a long-chain alkyl group-containing polyvinyl resin ("Pieroil" (registered trademark) 1050 manufactured by Lion Spicer Chemicals Co., Ltd.) as a long-chain alkyl group-containing compound, 2.5 parts by mass of a melamine-based crosslinking agent ("Sumimar" (registered trademark) M-55 manufactured by Sumitomo Chemical Co., Ltd.) as a crosslinking agent, and 1.3 parts by mass of p-toluenesulfonic acid ("TAYCACURE" AC-700 manufactured by TEICA Co., Ltd.) as an acid catalyst were weighed and mixed in 400 parts by mass of toluene and 130 parts by mass of methyl ethyl ketone as a solvent to prepare a coating agent T.
[0254] [Preparation of coating agent U]
[0255] As the coating agent U, an antistatic agent having a polystyrene sulfonic acid as a basic skeleton (manufactured by Fuji Chemical, antistatic agent "Fujistat" (registered trademark) YE908) was used.
[0256] (Example 1)
[0257] PET-1 was vacuum dried at 160°C for 2 hours and then put into an extruder, melted at 280°C, and extruded through a die onto a casting drum with a surface temperature of 25°C to prepare an unstretched sheet. Next, the sheet was preheated with a heated roll group, stretched 3.3 times in the longitudinal direction (MD direction) at a temperature of 90°C, and then cooled with a roll group at a temperature of 25°C to obtain a uniaxially stretched polyester film. On the obtained uniaxially stretched film, a coating agent prepared by mixing coating agent N and coating agent Q and diluting with pure water was applied by a bar coating method so that the mass ratio of compound A to compound B was as described in Table 1 and the thickness after drying was as described in Table 1. Then, while clamping both ends of the film with a clamp, it was stretched 4.0 times in the width direction (TD direction) perpendicular to the longitudinal direction in a heating zone at a temperature of 100°C in a tenter. Furthermore, heat fixing was performed at a temperature of 230°C for 10 seconds in a heat treatment zone in the tenter. Next, after being uniformly and slowly cooled in a cooling zone, the film was wound up to obtain a laminated polyester film laminated with the resin layer X. Table 1 shows the production conditions and properties of the obtained laminated polyester film.
[0258] The surface of the resin layer X of the obtained laminated polyester film opposite to the surface in contact with the polyester film was coated with a coating agent M by gravure coating to a thickness of 50 nm to obtain a resin layer Y. The properties of the obtained laminated polyester film are shown in Table 2.
[0259] The results of using a polyester film laminated with a resin layer Y as a process film are shown in Table 3. Since the mass ratio of compound A to compound B is equal, the Δ haze is slightly larger, and the Ω haze of layer Y is (150) / Ω (0) The peeling force F(B) of the resin layer Y after rubbing with a solvent-impregnated cloth is slightly large in the adhesive transfer application. The solvent used in the adhesive coating causes the properties of the layer Y to be poor. In addition, due to the Ω (150) The antistatic property is slightly poor, and although the peeling force of the adhesive is slightly large, it is not a problem in practical use.
[0260]
[0261]
[0262]
[0263] (Examples 2 to 10)
[0264] As the resin layer X, except that coating agent N, coating agent O, coating agent P, coating agent Q, and coating agent S were used so as to achieve the coating thickness, mass ratio of compound A and compound B, and the type described in Tables 1 and 4, the same operation as in Example 1 was performed to obtain a polyester film laminated with resin layer X and resin layer Y. The properties of the obtained laminated polyester film are shown in Tables 2 and 5, and the results using the laminated polyester film as a process film are shown in Tables 3 and 6.
[0265]
[0266]
[0267]
[0268] In Examples 2, 3, 7, 8 and 10, Δhaze is small, Ω (150) / Ω (0) The ratio F(A) / F(B) is in a preferred range, and the solvent durability ratio F(A) / F(B) is also in a preferred range. Therefore, it can be seen that the composite film exhibits excellent performance for green sheet molding and binder transfer.
[0269] In Examples 4 and 9, the ratio of compound A is less than that of compound B, so the Δhaze is slightly larger. As a result, the Ω haze of layer Y is (150) / Ω (0) In particular, in the case of green sheet molding, oligomers as foreign matter are generated when heat is applied in the process, and the cracking frequency is slightly increased when the molded green sheet is peeled off, which is poorly evaluated, but there is no problem in practical use. In the case of adhesive transfer, the solvent durability F(A) / F(B) is slightly large, and the properties of the resin layer Y are poor due to the solvent when the adhesive is applied. Therefore, although the peeling force of the adhesive is slightly large, there is no problem in practical use.
[0270] In Example 5, although the ratio of compound A is comparable to that of compound B, the thickness of resin layer X is thin and the Δhaze is slightly larger. As a result, the Ω haze of layer Y is (150) / Ω (0) In the case of green sheet molding, when heat is applied in the process, oligomers as foreign matter are generated, and the antistatic property is slightly reduced. As a result, when the molded green sheet is peeled off, it is easy to stick to layer Y. The evaluation of peeling force and cracking frequency are slightly poor, but there is no problem in practical use. In the case of adhesive transfer, the peeling force F(B) of the surface of the resin layer Y after friction treatment with a solvent-impregnated cloth is slightly large. The properties of the resin layer Y are deteriorated by the solvent when the adhesive is applied. Therefore, although the peeling force of the adhesive is slightly large, there is no problem in practical use.
[0271] In Example 6, the thickness of the release layer is large, and therefore, Ω (0) and Ω (150) It is slightly larger, and its properties for green sheet molding and adhesive transfer are slightly inferior, but it is not a problem in practical use.
[0272] (Example 11)
[0273] As the resin layer X, the same operation as in Example 1 was performed except that the coating agent N and the coating agent Q were used so as to have the coating thickness, the mass ratio of compound A and compound B, and the type described in Table 4, to obtain a polyester film laminated with the resin layer X. On the surface of the resin layer X of the obtained laminated polyester film opposite to the surface in contact with the polyester film, the coating agent T was coated by gravure coating so as to have a thickness of 50 nm to obtain a resin layer Y, thereby obtaining a laminated polyester film. The properties of the obtained laminated polyester film are described in Table 5.
[0274] The results of using a polyester film laminated with a resin layer Y as a process film are shown in Table 6. Since a resin different from the resin containing a compound having a siloxane bond as a main component was used as layer Y, the surface free energy was slightly larger and the Δhaze was slightly larger. As a result, the Ω haze of layer Y was (150) / Ω (0) In the case of green sheet molding, when heat is applied in the process, oligomers are generated as foreign matter, and the antistatic property is slightly reduced. As a result, when the molded green sheet is peeled off, it is easy to stick to layer Y. The evaluation of peeling force and cracking frequency are slightly poor, but there is no problem in practical use. In the case of adhesive transfer, the surface free energy is slightly large. In addition, the peeling force F(B) of the surface of the resin layer Y after friction treatment with a solvent-impregnated cloth is slightly large. The solvent used in the adhesive coating causes the properties of the layer Y to be poor. In addition, due to Ω (150) The antistatic property is slightly poor, and although the peeling force of the adhesive is slightly large, it is not a problem in practical use.
[0275]
[0276]
[0277]
[0278] (Examples 12, 13, 15)
[0279] As the resin layer X, except that coating agent N, coating agent Q, and coating agent R were used so as to have the coating thickness, mass ratio of compound A, compound B, and compound C, and the type described in Table 7, the same operation as in Example 1 was performed to obtain a polyester film laminated with resin layer X and resin layer Y. The properties of the obtained laminated polyester film are shown in Table 8, and the results using the laminated polyester film as a process film are shown in Table 9.
[0280] In Examples 12, 13, and 15, since the compound C was used in the resin layer X, the removability of the resin layer X and the resin layer Y was good.
[0281] In Example 12, Δ haze is small, Ω (150) / Ω (0) The solvent durability ratio F(A) / F(B) was also within the preferred range, and thus it was found that the composite film exhibited excellent performance for green sheet molding and binder transfer applications.
[0282] In Examples 13 and 15, although the mass ratio of Compound C was slightly large and the Δ haze was slightly increased, there was no problem in practical use for green sheet molding and binder transfer.
[0283] (Example 14)
[0284] As the resin layer X, coating agents N and Q were used to prepare coating agents so as to achieve the coating thickness, mass ratio and type of compound A and compound B described in the table. The coating agent was applied to T60 manufactured by Toray Industries, Ltd. having a thickness of 50 μm so as to achieve the thickness described in the table, and dried at 150° C. to obtain a laminated polyester film having layer X. Furthermore, layer Y was laminated thereon in the same manner as in Example 1 to obtain a laminated polyester film having layers X and Y.
[0285] It can be seen that since the resin layer X is produced by off-line coating, the coating film has slight defects, so the Δ haze is slightly high and the adhesion is also low. The evaluation result of the laminated polyester film having the resin layer X and the resin layer Y as the process film shows that although the Δ haze etc. increase, there is no problem in practical use.
[0286] (Comparative Example 1)
[0287] The same operation as in Example 1 was performed except that only compound B was used as the resin layer X and coating agent Q was used so as to have the coating thickness described in Table 4, thereby obtaining a polyester film having a laminate of resin layer X and resin layer Y. The properties of the obtained laminated polyester film are shown in Table 5, and the results using the laminated polyester film as a process film are shown in Table 6.
[0288] Since compound A is not contained, Δhaze, Ω (150) / Ω (0) , the solvent durability ratio F(A) / F(B) was poor and it was not suitable for use as a process film. It was believed that fine coating gaps and micro cracks occurred.
[0289] (Comparative Example 2)
[0290] As the resin layer X, except that the coating agent Q and the coating agent R were used so as to have the mass ratio of compound B and compound B and the coating thickness described in Table 4, the same operation as in Example 1 was performed to obtain a laminated polyester film having the resin layer X and the resin layer Y laminated thereon. The properties of the obtained laminated polyester film are shown in Table 5, and the results using the laminated polyester film as a process film are shown in Table 6.
[0291] Since compound A is not contained, Δhaze, Ω (150) / Ω (0) , the solvent durability ratio F(A) / F(B) was poor and it was not suitable for use as a process film. It was believed that fine coating gaps and micro cracks occurred.
[0292] (Comparative Example 3)
[0293] As the components constituting the resin layer X, coating agent N was used as compound A, and coating agent U was used as the compound having antistatic properties, and the coating agent was prepared in such a way that the solid contents of compound A and the compound having antistatic properties were equal. Except for using this coating agent, the same operation as in Example 1 was carried out to prepare a laminated polyester film having layer X and a laminated polyester film having layer X and layer Y. Since compound B was not contained, Δ haze, Ω (150) / Ω (0) Poor, not suitable for use as process membrane.
[0294] Industrial Applicability
[0295] The laminated polyester film of the present invention has excellent antistatic properties and heat resistance, and can be suitably used as a protective film for an adhesive layer in adhesive products and a process film in the processing steps of various industrial products.
Claims
1. A laminated polyester film comprising a resin layer X on at least one surface of a polyester film, wherein the resin layer X contains at least a compound A having a vinyl alcohol residue and a compound B having a thiophene residue. 2 . The laminated polyester film according to claim 1 , wherein the epoxy group content in the solid content of the resin layer X measured from the laminated polyester film under specific extraction and analysis conditions is 5 mg / g or more and 100 mg / g or less. 3 . The laminated polyester film according to claim 1 , wherein the total amount of organic components in the solid content of the resin layer X extracted under specific extraction conditions is 90% by mass or more, when the converted mass of the resin layer X of the laminated polyester film is 100% by mass. 4 . The laminated polyester film according to claim 1 , wherein in 100% by mass of the resin layer X, the total content of the compound A having a vinyl alcohol residue, the compound B having a thiophene residue and the epoxy compound C is 90% by mass or more. The laminated polyester film according to claim 1 or 2, wherein the degree of polymerization of the compound A is 50 or more and 1,000 or less.
6. The laminated polyester film according to claim 1 or 2, wherein the adhesion M(X) of the resin layer X satisfies the following conditions, M(X)≥90(%). 7 . The method for producing a laminated polyester film according to claim 1 , comprising the steps of coating a coating agent for forming the resin layer X on a polyester film and stretching the polyester film in this order. 8 . The laminated polyester film according to claim 1 , comprising a polyester film, the resin layer X, and a resin layer Y in this order.
9. The laminated polyester film according to claim 8, wherein The surface resistivity of the surface of the resin layer Y satisfies the following formula (1) and formula (2): (1)10 6 ≤Ω (0) ≤10 10 (2)Oh (150) / Oh (0) <50 Among them, Ω (0) represents the surface resistivity (Ω / sq) of the resin layer Y before heat treatment, Ω (150) It shows the surface resistivity (Ω / sq) of the surface of the resin layer Y after heat treatment at 150°C for 60 minutes. 10 . The laminated polyester film according to claim 8 , wherein the surface free energy of the resin layer Y is 30 mN / m or less. 11 . The laminated polyester film according to claim 8 , wherein the resin layer Y is a resin having a compound having a siloxane bond as a main component.
12. The laminated polyester film according to claim 8, wherein the water contact angle on the resin layer Y side satisfies the following formula (3) and formula (4), (3) 0°≤HYa≤80° (4) 10°≤|HYp-HYa|≤100° in, HYp represents the water contact angle on the resin layer Y side of the laminated polyester film, and HYa represents the water contact angle on the resin layer Y side of the laminated polyester film after the laminated polyester film is immersed in pure water at 25° C. for 5 minutes. 13 . The laminated polyester film according to claim 8 , wherein the change in haze after heat treatment at 150° C. for 60 minutes is 10% or less. 14 . The laminated polyester film according to claim 8 , wherein the solvent durability of the surface of the resin layer Y measured in accordance with JIS L 0849 (2013) (friction tester type II) is 50% or more and 100% or less.
15. The laminated polyester film according to claim 8, which is used as a process film in a product manufacturing process.
Citation Information
Patent Citations
Production of sulfonic-acid-modified polyvinyl alcohol
JP1997227627A
Laminate
JP2000006324A
Protective film for dry film resist and photosensitive resin laminate
JP2019066888A
Permanent antistatic primer layer
US5391472A
Off film
CN101357521A