Metal cylinder with bottom
Through the use of the split arch die head, the problem of wrinkles on the periphery of the dome-shaped bottom surface of the metal seamless can is solved, forming annular line, improving the appearance quality and product value of the product.
Patent Information
- Application Number
- CN202380028603.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-04
- Filing Date
- 2023-02-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-02-01
AI Technical Summary
The dome-shaped bottom surface of existing metal seamless cans is prone to wrinkles on the peripheral edges, affecting the appearance and commodity value, especially in beverage cans.
A divided arch die head, including an arch ring and a base die head, is used to delineate the peripheral edge and central part of the dome-shaped base surface, and forms an annular line to avoid the occurrence of wrinkles by independently moving up and down.
The dome-shaped bottom surface of the seamless can be thinned at the periphery, instead of wrinkles, forming annular line, improving appearance quality and commodity value, and avoiding the generation of wrinkles.
Smart Images

Figure CN118900807A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a metal bottomed cylinder having a dome-shaped bottom surface, such as a seamless metal can, and also relates to a molding die for molding the dome-shaped bottom surface and a doming method using the molding die. Background Art
[0002] Generally, for a metal bottomed cylinder obtained by metal forming (punching, drawing and ironing), such as a seamless can, the bottom is formed into a dome shape for the purpose of weight reduction, improvement of pressure resistance and installation stabilization. Such bottom forming is called doming, and is performed by holding the bottom peripheral edge of the cylinder with an annular die called a retaining ring while pushing up the doming die head from the annular die to make the bottom surface of the cylinder concave into a dome shape (see Patent Document 1).
[0003] Furthermore, in the dome-shaped bottom surface formed as described above, there is a problem that wrinkles are easily generated at the peripheral portion, and the wrinkles are particularly obvious in aluminum can bodies. In the past, such wrinkles were formed on the bottom surface, so it was not a big problem. However, nowadays, beverage cans such as aluminum seamless cans are often placed and sold in a manner that the bottom of the can can be seen, so recently, the current situation is that it is necessary to improve this.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2018-177289 Summary of the invention
[0007] Problems to be solved by the invention
[0008] Therefore, an object of the present invention is to provide a metal bottomed cylinder having a dome-shaped bottom without wrinkles.
[0009] Another object of the present invention is to provide a molding die used for dome molding (arching) of the bottom of the above-mentioned metal bottomed cylinder and a dome molding method using the molding die.
[0010] Solutions for solving problems
[0011] According to the present invention, there is provided a metal bottomed cylinder having a grounding portion at the bottom, a rising portion extending upward from the inner side of the grounding portion, and a dome-shaped bottom surface connected to the rising portion, wherein the metal bottomed cylinder is characterized in that:
[0012] A ring-shaped line is observed at the peripheral edge of the dome-shaped bottom surface.
[0013] In the metal bottomed cylinder of the present invention, it is preferred that:
[0014] (1) The metal bottomed cylinder is an aluminum seamless can.
[0015] According to the present invention, there is also provided a molding die for use in forming a dome at the bottom of a metal bottomed cylinder, wherein the molding die is characterized in that:
[0016] It consists of an annular holding mold for holding the bottom periphery of a metal bottomed cylinder and an arching die head for defining a dome-shaped bottom surface.
[0017] The arch die is divided into an arch ring for defining the peripheral edge of the dome-shaped bottom surface and a base die for defining the central portion of the dome-shaped bottom surface further inside the peripheral edge. The arch ring and the base die can move up and down independently.
[0018] According to the present invention, there is also provided a dome forming method, which is a dome forming method for the bottom of a metal bottomed cylinder, wherein the dome forming method is characterized in that it comprises the following steps:
[0019] preparing a molding die as described above;
[0020] The punch sleeve is lowered from the inside of the metal bottomed cylinder to press the lower end peripheral edge of the cylinder against the action surface of the annular holding die, thereby forming a flange portion and a grounding portion on the bottom peripheral edge of the cylinder;
[0021] While holding the flange and the grounding portion of the cylinder body by the action surfaces of the punch sleeve and the annular holding die, the arch ring is raised to form a rising portion and a peripheral edge of a dome-shaped bottom surface inside the grounding portion; and
[0022] The base die is arranged to form the central portion of the dome-shaped bottom surface.
[0023] Effects of the Invention
[0024] The metal bottomed cylinder of the present invention has a dome-shaped bottom surface that is recessed in a dome shape, but no wrinkles are found in the dome-shaped peripheral edge portion, and instead, ring-shaped lines are observed.
[0025] In the present invention, the die used in the molding of the bottom of the cylinder, i.e., the arch molding, is divided into an arch ring for defining the peripheral portion of the dome-shaped bottom surface and a base die for defining the central portion of the dome-shaped bottom surface that is closer to the inner side than the peripheral portion, and the surface of the peripheral portion of the dome-shaped bottom surface is formed by a special mold called the arch ring. As a result, the surface of the peripheral portion of the dome-shaped bottom surface is stretched and thinned, and the generation of wrinkles is prevented along with the thinning. In short, the arch is performed using a special arch ring that determines the peripheral portion of the dome-shaped bottom surface, so the portion thinned by the arch ring becomes an indentation, and the trace of the inner end of the arch ring is observed as a ring line.
[0026] As described above, in the metal cylinder of the present invention, annular lines are observed instead of wrinkles at the peripheral edge of the dome-shaped bottom surface, thereby ensuring high commercial value without impairing the appearance when used as a beverage can, for example. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic side sectional view showing the entire metal bottomed cylinder of the present invention.
[0028] Figure 2 yes Figure 1 An enlarged partial side sectional view of the bottom of a metal bottomed cylinder.
[0029] Figure 3 yes Figure 1 A photograph of the bottom surface of a metal bottomed cylinder.
[0030] Figure 4 This is a photograph of the bottom surface of a conventionally known metal bottomed cylinder.
[0031] Figure 5 is shown for manufacturing Figure 1 A schematic diagram of the process of making a metal bottomed cylinder.
[0032] Figure 6 It is shown in Figure 5 Figure 1 is a diagram of the forming die used in the arching process.
[0033] Figure 7 It is used to illustrate Figure 5 Diagram of the arching process. DETAILED DESCRIPTION
[0034] <Metal bottomed cylinder>
[0035] The metal bottomed cylinder of the present invention is obtained, for example, by punching, drawing, and re-drawing-thinning a metal thin-walled blank plate, and then performing a cambering process on the bottom. Finally, after the metal bottomed cylinder is obtained, it is subjected to post-processing such as washing and drying, external surface printing, top varnish coating and baking, internal surface coating and baking, necking and flange processing, and the final shape is generally as a whole as follows. Figure 1 shown.
[0036] Reference Figure 1 The metal bottomed cylinder of the present invention, which is generally indicated by 10, comprises: a main body 1 having a straight cylindrical shape on the outer surface; a grounding portion 5 formed via a flange portion 3 inclined inward from the lower end of the main body 1; and a dome-shaped bottom surface 7 located in a region surrounded by the grounding portion 5. In addition, the upper portion of the main body 1 is connected to a necking portion 8 formed by post-processing, and a flange portion 9 is formed at the upper end of the necking portion 8.
[0037] The dome-shaped bottom surface 7 is composed of a peripheral portion 7a connected to the upper end of the rising portion 6 rising inward from the grounding portion 5 and a central portion 7b surrounded by the peripheral portion 7a. The peripheral portion 7a corresponds to the portion that is contacted by the arch ring used in the arching described later, and its length is about 2mm to 30mm when observed in a side section. When observed in a side section, the dome-shaped bottom surface 7 composed of the peripheral portion 7a and the central portion 7b has a generally fixed large curvature radius as a whole. By forming the bottom surface 7 of this form at the bottom, the bottomed cylinder 10 can be stably set, and the load strength relative to the axial direction can be improved.
[0038] In the present invention, there is no particular restriction on the metal constituting the bottomed cylinder 10, and it may be various metals or alloys. However, in view of light weight and thin-wall processability, aluminum or aluminum alloy is preferred. Moreover, in order to maximize the advantages of the present invention, a seamless tank whose inner surface is coated with an organic resin is preferred.
[0039] and Figure 1 Refer to Figure 2 The bottom enlarged partial side section view and Figure 3 In the bottom photograph of the dome-shaped bottom surface 7, an important feature of the present invention is that a ring line 11 is observed at the boundary between the peripheral edge portion 7a and the central portion 7b of the dome-shaped bottom surface 7.
[0040] That is, the dome-shaped bottom surface 7 is obtained by arching, but in the conventionally known metal bottomed cylinder, such as Figure 4 As shown in the bottom photograph of FIG. 1 , wrinkles X exist in the region corresponding to the peripheral edge portion 7a of the dome-shaped bottom surface 7. However, in the present invention, as shown in FIG. Figure 3As can be understood from the bottom photograph of the , a ring line 11 is formed instead of the wrinkle X. As can be understood from the peripheral portion 7a that originates from the arching ring used when arching, the ring line 11 originates from the indentation of the arching ring, the area outside the ring line 11 is the peripheral portion 7a, and the area inside the ring line 11 is the center portion 7b. In addition, the thickness t0 of the ring line 11 originating from the local thin-walled portion is reduced by about 3% to 5% relative to the thickness t1 at a position about 0.5 mm inside the peripheral portion 7a, and the wrinkle X is eliminated by stretching. That is, in the present invention, the ring line 11 is formed instead of the wrinkle X.
[0041] In such a metal bottomed cylinder 10, the thickness at the center portion O of the dome-shaped top surface 7 is usually equivalent to the thickness of the thin-walled blank used in the molding, and the thickness of the main body 1 is determined by the degree of thinning processing (thinning rate).
[0042] For example, in the case of an aluminum seamless can used as a beverage can, the thickness of the base plate is about 0.180 mm to 0.350 mm, and the thickness of the thinnest portion of the main body 1 is 30% to 50% of the base plate thickness.
[0043] <Manufacturing of Metal Bottomed Cylinder 10>
[0044] The metal bottomed cylinder 10 of the present invention having the above-described configuration is manufactured by molding using the above-described metal blank (an organic resin coating may be provided on the side corresponding to the inner surface).
[0045] The bottomed cylindrical body 10 having the dome-shaped bottom surface 7 is obtained by the forming process using the metal blank plate as described above, such as punching, drawing, ironing and bulging in the usual manner.
[0046] The process from punching to arching is shown in Figure 5 .
[0047] That is, Figure 5 As shown in (a), the blank plate 21 is punched out by a punching punch 23 and a punching die 25 to obtain a circular plate 27 (punching process). Figure 5 As shown in (b), a drawn cup (bottomed cylindrical body) 35 (drawing process) is obtained by using a drawing die 31 and a drawing punch 33. Here, the obtained drawn cup 35 can also be provided for the cambering process described later, but usually, it is continuously performed from re-drawing to ironing as needed.
[0048] That is, Figure 5As shown in (c), the drawing cup 35 held by the pressing member 41 in the redraw die 43 is pushed downward using the ironing punch 45, and then, after being ironed through a plurality of ironing dies 47a to 47c, is arched at the lowest position. The arching is performed using the clamping ring 51 and the arching die 61 described later. By the arching, the dome-shaped bottom surface 7 is formed simultaneously with the flange portion 3 and the grounding portion 5.
[0049] After the arching, the formed seamless can (metal bottomed cylinder) 10 is pulled out from the punch 45 using a stripper finger 53, whereby this process is completed and subsequent post-processes such as cleaning, drying, and necking are performed.
[0050] It should be noted that in the above-mentioned thinning process, Figure 5 In (c), three thinning dies are arranged to perform thinning in three stages, but the number of the thinning dies is not limited to three, and can be set to an appropriate number according to the degree of thinning as the purpose. One die can be used to perform thinning in one stage, or more than two dies can be arranged to perform thinning in multiple stages. Of course, when multiple thinning dies are arranged along the processing direction and thinning is performed in multiple stages, the inner diameter (processing diameter) becomes smaller as it moves toward the downstream side of the processing direction.
[0051] In short, after such a thinning process, the bottom surface 7 is domed to form a dome shape.
[0052] like Figure 6 As shown, the forming die for arching is composed of a clamping ring (ring-shaped holding die) 51 and an arching die head 60, and arching is performed by the cooperation of these forming dies and a punch 45. In the present invention, an important feature is that the arching die head 60 is divided into a base die head 61 and an arching ring 63, and is arranged in a manner that each can move up and down independently.
[0053] That is, if Figure 6 As can be understood, the action surface 51a at the upper end of the clamping ring (annular retaining mold) 51 is inclined inward and downward, and the flange portion 3 connected to the lower end of the main body portion 1 is formed by the action surface 51a, and the contact surface 5 is formed at the lower end of the action surface 51a.
[0054] The base die 61 is a die that defines the central portion 7b of the dome-shaped bottom surface 7, and the action surface 61a at the upper end thereof corresponds to the central portion 7b of the dome-shaped bottom surface 7. The dome ring 63 is a die that defines the peripheral portion 7a of the dome-shaped bottom surface 7, and the action surface 63a at the upper end thereof corresponds to the peripheral portion 7a of the dome-shaped bottom surface 7. These action surfaces 61a and 63a are smoothly connected to form the dome-shaped bottom surface 7.
[0055] As described above, the peripheral portion 7a of the dome-shaped bottom surface 7 is a portion where wrinkles are easily generated. By setting the profile defining this portion separately from the profile defining the central portion 7b, the stress applied to the peripheral portion 7a of the dome-shaped bottom surface 7 is concentrated, thereby extending the generated wrinkles, avoiding the generation of wrinkles, and forming a ring line 11 at a position corresponding to the inner end of the action surface 63a of the arch ring 63. That is, when viewed in side section, the length of the action surface 63a is equivalent to the length of the peripheral portion 7a of the dome-shaped bottom surface 7.
[0056] The arching of the above-mentioned forming die is achieved by Figure 7 The process shown is carried out.
[0057] The clamping ring 51 is not shown in the figure but is forced upward by the air. Figure 7 As shown in (a), in the initial stage, the action surface 63a of the arch ring 63 is located below the action surface 51a of the clamp ring 51, and the action surface 61a of the base die 61 is located below the action surface 63a of the arch ring 63.
[0058] When the punch 45 is lowered in the above state and the main body 1 of the cylindrical body 10 is pressed down, as shown in FIG. Figure 7 As shown in (b) of FIG. 1 , the lower end of the main body 1 is pressed against the action surface 51 a of the clamp ring 51 , thereby forming the flange 3 at the lower end of the main body 1 .
[0059] Next, when the arch ring 63 is raised, Figure 7 As shown in (c), the grounding portion 5 is defined, and the inner side of the grounding portion 5 is pulled up to define the rising portion 6. Furthermore, the action surface 63a of the arch ring 63 pushes the surface closer to the inner side than the rising portion 6, thereby defining the peripheral portion 7a of the dome-shaped bottom surface 7.
[0060] When the peripheral edge portion 7a of the dome-shaped bottom surface 7 is formed as described above, Figure 7 As shown in (d), by delaying the configuration of the base die head 61, the action surface 61a thereof is pressed against the bottom of the cylinder 10 to form the central portion 7b of the dome-shaped bottom surface 7, thereby defining the dome-shaped bottom surface 7, and observing the portion corresponding to the end of the action surface of the arch ring 63 by Figure 2 , Figure 3 The annular wire 11 shown in the figure can effectively prevent the generation of wrinkles by the arched ring 63.
[0061] After the arching is completed in this way, as described above, the punch 45 is pulled out, and the obtained molded body is pulled away from the punch 45 by the stripper claw 53, and the subsequent processes, cleaning, drying, necking processing, flange processing, painting and other post-processes are carried out to obtain a bottomed cylinder (seamless can) with no wrinkles on the bottom surface and high commercial value.
[0062] Description of Reference Numerals
[0063] 1: Main body;
[0064] 3: convex edge;
[0065] 5: grounding part;
[0066] 6: rising part;
[0067] 7: dome-shaped bottom surface;
[0068] 7a: peripheral part;
[0069] 7b: central part;
[0070] 10: Cylinder with bottom;
[0071] 51: clamping ring (ring-shaped retaining mold);
[0072] 60: Arch die head;
[0073] 61: base die head;
[0074] 63: Arched ring.
Claims
1. A metal bottomed cylinder, the metal bottomed cylinder having a grounding portion at the bottom, a rising portion extending upward from the inner side of the grounding portion, and a dome-shaped bottom surface connected to the rising portion, wherein the metal bottomed cylinder is characterized in that: A ring-shaped line is observed at the peripheral edge of the dome-shaped bottom surface.
2. The metal bottomed cylinder according to claim 1, wherein: The metal bottomed cylinder is an aluminum seamless can.
3. A molding die used for forming a dome at the bottom of a metal bottomed cylinder, wherein: It consists of an annular holding mold for holding the bottom periphery of a metal bottomed cylinder and an arching die head for defining a dome-shaped bottom surface. The arch die is divided into an arch ring for defining the peripheral edge of the dome-shaped bottom surface and a base die for defining the central portion of the dome-shaped bottom surface further inside the peripheral edge. The arch ring and the base die can move up and down independently.
4. A dome forming method, the dome forming method is a dome forming method for the bottom of a metal bottomed cylinder, the dome forming method is characterized by comprising the following steps: Preparing the molding die as claimed in claim 3; The punch sleeve is lowered from the inside of the metal bottomed cylinder to press the lower end peripheral edge of the cylinder against the action surface of the annular holding die, thereby forming a flange portion and a grounding portion on the bottom peripheral edge of the cylinder; While holding the flange and the grounding portion of the cylinder body by the action surfaces of the punch sleeve and the annular holding die, the arch ring is raised to form a rising portion and a peripheral edge of a dome-shaped bottom surface inside the grounding portion; and The base die is arranged to form the central portion of the dome-shaped bottom surface.
Citation Information
Patent Citations
Aluminum seamless can
JP2018177289A
can bodies for beverage cans
DE102015215590A1
Method for forming barrel for two-piece can
GB2237763A
Manufacture of seamless can
JP1992371332A
Seamless can and its forming method
JP1997285832A