Use of adhesives, sealants or coatings on green concrete and other highly alkaline substrates

By applying the water-based polymer dispersion composition on fresh high alkaline substrates, the problem of damage to curing behavior caused by high alkalinity and high water content in the prior art is solved, and rapid curing and long-lasting stickiness are achieved Adhesion, shortens usage time and reduces cost.

CN118900829APending Publication Date: 2024-11-05SIKA TECH AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027192.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-14
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

When existing adhesives, sealants or coating compositions are used on fresh concrete, cement mortar, lime mortar or silicate coatings, the curing behavior is damaged due to high alkalinity and high water content, and the curing behavior is damaged and sticky. The adhesion decreases and the substrate needs to be dried before application is applied, resulting in increased time and cost.

Method used

Plasticizers containing more than 20% aqueous dispersion polymers, emulsifiers, dispersants and ester or ether groups for application within a few days after the substrate is dried and Curing to ensure adhesion and stability.

Benefits of technology

Rapid curing and adhesion on fresh high alkaline substrates is achieved, the degradation of the composition is avoided, the use time is significantly shortened and the adhesion performance and stability are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005039989300000181
    Figure BDA0005039989300000181
  • Figure BDA0005039989300000191
    Figure BDA0005039989300000191
  • Figure BDA0005039989300000201
    Figure BDA0005039989300000201
Patent Text Reader

Abstract

The invention relates to the use of a water-based polymer dispersion composition comprising more than 20% by weight, based on the total composition, of at least one water-dispersed polymer P as an adhesive, sealant or coating applied to at least one basic substrate having a pH of at least 10 when wetted with water, at least one water-dispersed polymer P dispersed in water at a concentration of 40-80% by weight based on the dispersion of the water-dispersed polymer P wherein the glass transition temperature Tg of the at least one water-dispersed polymer P is lt as determined by DSC according to ISO 11357 standard; 0 DEG C, at least one surfactant, preferably a nonionic surfactant, at least one dispersant, in particular a polymeric ammonium or sodium salt of a carboxylic acid copolymer, and optionally at least one plasticizer PL having at least one ester or ether group, wherein the alkaline base material is fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint. The use of the invention allows for sealing, bonding or coating such overbased substrates shortly after deposition or production of such overbased substrates, while the applied polymer dispersions do not degrade or lose adhesion to these highly demanding substrates.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the use of an adhesive, sealant or coating composition on a highly alkaline substrate selected from fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint, and to a method of applying such a composition on such a substrate. Background Art

[0002] Curable or dryable compositions, particularly compositions based on polyurethane or silane-modified polymers (SMP), are often used as adhesives, sealants or coatings in the construction field. Typical substrates for applying such products are derived from cement, lime or silicate-bonded building materials, such as concrete or cement mortar. When these building materials have just been applied or processed and thus the substrates in the form of foundations, walls, screeds, plasters, etc. are still fresh, they have a pH value of 10 or higher, and the surface is obviously alkaline, because the hydroxides present therein have not yet been carbonated. Fresh concrete is also referred to as "young" or "raw" or "wet". In this state, the still highly alkaline substrate is very problematic for the composition applied thereon, because the high alkalinity and high water content of the substrate that has not yet dried may seriously affect the curing behavior or mechanical properties of the composition applied on such substrates. In order to protect the adhesive, sealant or coating composition from contacting with the alkaline surface, the substrate must be fully aged and dried, which requires time, or pre-treated before applying the composition, for example, by neutralizing with fluate (e.g., fluorosilicate), or by sealing with a primer (e.g., epoxy resin coating). However, in practice, this is not usually done in order to save time and money. In the boundary layer, hydrolysis reactions of the components of the sealant, adhesive or coating composition can occur under alkaline conditions, which can not only lead to a significant impairment of the adhesion of the sealant, adhesive or coating composition on the substrate, but also to annoying odor emissions, impaired curing or final properties, or even chemical degradation of the composition. Among the sensitive compounds, in particular the plasticizers present in most of these compositions, or the curing catalyst, or the binder polymer matrix itself. Typical sensitive plasticizers used are fatty alcohol dicarboxylates, such as diisodecyl phthalate (DIDP), diisononyl cyclohexane-1,2-dicarboxylate (DINCH) or di(2-ethylhexyl) adipate (DOA). Their hydrolysis leads to the release of fatty alcohols, which have a very unpleasant odor and migrate into the pore structure of the substrate, then evaporate or wash out into the environment and cause a musty odor over a long period of time. This persistent odor is observed in particular in the case of parquets bonded to fresh cement screeds with elastic polyurethane or SMP adhesives. Curable compositions such as polyurethanes or SMPs also often contain curing catalysts, which can be damaged by the high alkalinity of green concrete and other such highly alkaline substrates. This can result in slow or incomplete curing of such compositions.

[0003] Thus, to date, in order to properly use an adhesive, sealant or coating composition on a fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint substrate, it has been necessary to wait a sufficient period of time for the substrate to dry and reduce its alkalinity so that the composition can be applied thereon and the adhesive, sealant or coating having the proper performance on these substrates can be obtained. For example, a typical polyurethane or silicone composition may require several weeks of substrate drying in order to properly and continuously adhere to these substrates without showing signs of degradation. Of course, it would therefore be desirable to have an adhesive, sealant or coating composition that can be applied directly to still highly alkaline and wet substrates, including fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint, or applied after a much shorter waiting period of a few days or less, while the composition cures or dries and adheres properly and does not degrade. SUMMARY OF THE INVENTION

[0005] It is an object of the present invention to provide the use of a composition as defined as an adhesive, sealant or coating applied to at least one alkaline substrate having a pH of at least 10 when wetted with water, wherein the alkaline substrate is fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint. It is therefore to provide such a composition suitable for this intended use, which is applied to such a substrate within a very short time after deposition or production of the substrate, for example within a few days or less, and cures or dries appropriately, continuously adheres to the substrate and shows no signs of degradation of the composition itself or its components.

[0006] Surprisingly, it has been found that water-based compositions according to claim 1 can be used in these applications and produce the desired stability and working efficiency over a long period of time. When used as claimed in claim 1, they can be applied to still alkaline and wet substrates only a few days or less after the substrates have been manufactured, but still cure or dry easily and without any signs of degradation, even if they contain plasticizers. In addition, they exhibit excellent and long-lasting adhesion on these substrates.

[0007] According to another aspect of the present invention, a method for sealing a joint, bonding two substrates, or coating a surface is provided.

[0008] Preferred embodiments are the subject matter of the dependent claims. DETAILED DESCRIPTION

[0009] Substance names beginning with "poly" indicate substances that formally contain two or more of the functional groups that appear in their names per molecule. For example, polyols refer to compounds that have at least two hydroxyl groups. Polyethers refer to compounds that have at least two ether groups.

[0010] The term "polymer" in this document includes, on the one hand, a collection of chemically homogeneous macromolecules that still differ in degree of polymerization, molar mass and chain length, which collection is prepared by polymerization reactions (chain-growth addition polymerization, free-radical polymerization, polyaddition, polycondensation). On the other hand, the term also includes derivatives of such a collection of macromolecules from polymerization reactions, in other words, compounds obtained by reaction (e.g. addition or substitution) of functional groups on existing macromolecules, and which may be chemically homogeneous or chemically inhomogeneous.

[0011] The "molecular weight" of an oligomer or polymer is understood herein to be the molecular weight average M n (number average), which is typically determined by GPC using polystyrene as the standard.

[0012] If not otherwise specified, the unit term "weight %" refers to the weight percentage based on the weight of the corresponding total composition. The terms "weight" and "mass" are used interchangeably herein.

[0013] All industrial specifications and standard methods mentioned in this document are referenced to the respective current editions at the time of submission.

[0014] The term "(meth)acrylic acid" means methacrylic acid or acrylic acid. Thus, the term "(meth)acrylate" means methacrylate or acrylate.

[0015] The term "polyacrylate polymer" means a polymer obtained by free radical polymerization of two or more (meth)acrylate monomers. Copolymers of (meth)acrylate monomers and copolymers of (meth)acrylate monomers with other vinyl-containing monomers are also included in the term "polyacrylate polymer". The terms "polyacrylate polymer", "polyacrylate" and "acrylate polymer" are used interchangeably.

[0016] The term "shelf life" refers to the period of time after which the dispersion adhesive composition has substantially coagulated, separated or settled such that it cannot be readily applied to a substrate surface as a homogenous, uniform film or bead.

[0017] The term "shelf-stable composition" refers to a composition having a shelf life of greater than 6 months when stored in a closed container at room temperature and 50% relative humidity (abbreviated as "rh").

[0018] The term "room temperature" (abbreviated "RT") denotes a temperature of 23°C.

[0019] The term "standard pressure" means an absolute pressure of 1 bar.

[0020] In a first aspect of the present invention, the present invention relates to the use of a water-based polymer dispersion composition comprising:

[0021] a) more than 20% by weight, based on the total composition, of at least one water-dispersible polymer P, dispersed in water in a concentration of 40 to 80% by weight, based on the dispersion of the water-dispersible polymer P, wherein the at least one water-dispersible polymer P has a glass transition temperature T<0° C. g , which is determined by DSC according to ISO 11357 standard,

[0022] b) at least one emulsifier, preferably a nonionic emulsifier,

[0023] c) at least one dispersant, in particular a polymeric ammonium salt of a carboxylic acid copolymer, and

[0024] d) optionally, at least one plasticizer PL having at least one ester or ether group,

[0025] It is used as an adhesive, sealant or coating to be applied to at least one alkaline substrate which has a pH of at least 10 when wetted with water, wherein the alkaline substrate is fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint.

[0026] The alkaline substrate is fresh, meaning an incompletely carbonated substrate based on cement, lime (calcium hydroxide) and / or silicate (water glass). More specifically, the alkaline substrate is fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint. In the same context, the term "fresh" in relation to those substrates is used synonymously with the term "young" or "raw" or "wet".

[0027] The pH of a water-wet alkaline substrate can be measured using pH paper or a pH meter or indicator or any other suitable method to measure the pH of an alkaline aqueous solution.

[0028] The above concrete or other alkaline substrate is called "fresh" as long as it can still undergo alkaline reaction under the condition of pH 10 or higher. The time during which the concrete or other alkaline substrate is still fresh in this context depends on its setting time and the ambient temperature. This time usually varies in the range of 1-10 days.

[0029] The term "dispersion" refers to a physical state of matter comprising at least two distinct phases, wherein a first phase is distributed in a second phase, which is a continuous medium. Preferably, the dispersion comprises a solid phase as solid particles dispersed in a continuous liquid phase.

[0030] The term "aqueous polymer dispersion" refers to a polymer dispersion having water as the primary carrier. Preferably, "aqueous" refers to a 100% water carrier. In this context, compounds denoted as PIB, ALK or PL or conventional additives known to those skilled in the art of aqueous polymer dispersions are not considered to be carriers in this context.

[0031] Preferably, the dispersion adhesive composition comprises less than 5 wt%, preferably less than 1 wt%, of volatile organic compounds having a boiling point of less than 150°C, based on the total weight of the dispersion adhesive composition.

[0032] The aqueous polymer dispersion comprises one or more water-dispersible polymers P, preferably free-radically polymerized polymers obtained from ethylenically unsaturated monomers. Preferably, such polymers contain a C1-C1 (meth)acrylic acid. 20 Alkyl esters, vinyl esters of carboxylic acids containing up to 20 carbon atoms, vinyl aromatic compounds containing up to 20 carbon atoms, ethylenically unsaturated nitriles, vinyl halides, non-aromatic hydrocarbons having at least two conjugated double bonds or mixtures of these monomers are the main monomers.

[0033] Preferably, the monomers of polymer P consist of more than 50% by weight of acrylic monomers. Acrylic monomers are defined herein to include (meth)acrylic acid, esters of (meth)acrylic acid, amides of (meth)acrylic acid and nitriles of (meth)acrylic acid. As ethylenically unsaturated monomers, acrylate monomers that can be used include methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, decyl acrylate, methyl methacrylate, butyl methacrylate, isodecyl methacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate, acrylamide or substituted acrylamides, styrene or substituted styrenes, butadiene, vinyl acetate or other vinyl esters, acrylonitrile or methacrylonitrile. Silicon-containing monomers such as vinyltrialkoxysilanes (including vinyltrimethoxysilane), allyltrialkoxysilanes (including allyltrimethoxysilane), (meth)acryloxyalkyltrialkoxysilanes (including methacryloxypropyltrimethoxysilane), (meth)acryloxyalkylalkyldialkoxysilanes (including methacryloxypropylmethyldiethoxysilane), (meth)acryloxyalkoxyalkyltrialkoxysilanes (including methacryloxyethoxyethyltrimethoxysilane) and mercaptoalkyltrialkoxysilanes (including mercaptopropyltrimethoxysilane) may also be added, preferably in an amount of 0.01% to 6% by weight, based on the weight of polymer P. Low levels of ethylenically unsaturated monocarboxylic acids may be used, such as 0 to 7% by weight of methacrylic acid or acrylic acid, based on the weight of polymer P.

[0034] Suitable and preferred polymers P include, for example, polyvinyl acetate, polyvinyl alcohol, polyacrylates, polyurethanes, polyurethane-acrylates, natural-based polymers, carboxylated polystyrene-copolymers, carboxylated butadiene styrene copolymers, carboxylated butadiene rubber styrene-butadiene copolymers, styrene-isoprene copolymers, ethylene-vinyl acetate copolymers (EVA), ethylene-methacrylate copolymers, ethylene-ethyl acrylate copolymers, ethylene-butyl acrylate copolymers (EBA), ethylene-(meth)acrylic acid copolymers, ethylene-2-ethylhexyl acrylate copolymers, ethylene-acrylate copolymers and polyolefin block copolymers.

[0035] The above copolymers, meaning polymers made from more than one type of monomer, may be block copolymers or random copolymers.

[0036] The polymers P may also be further functionalized, which means that they may contain further functional groups such as hydroxyl, carboxyl, anhydride, acrylate and / or glycidyl methacrylate groups.

[0037] Preferably, the water-dispersible polymer P contains the abovementioned monomers and mixtures thereof in an amount of 60-100%, more preferably 85-100%, most preferably 95-99.8%, based on the weight of the polymer.

[0038] Preferred (meth)acrylic acids C1-C 20 Alkyl esters include 12 Alkyl (meth)acrylates of alkyl groups, for example methyl (meth)acrylate, n-butyl acrylate, ethyl acrylate and 2-ethylhexyl acrylate. Particularly suitable polymers P may be mentioned as polymers P which are obtained by polymerization of mixtures of alkyl acrylates and alkyl (meth)acrylates.

[0039] Suitable vinyl esters of carboxylic acids containing up to 20 carbon atoms include, for example, vinyl laurate, vinyl stearate, vinyl propionate, vinyl esters of tertiary saturated monocarboxylic acids, vinyl acetate, and mixtures of two or more thereof.

[0040] Suitable vinyl aromatic compounds include, for example, vinyltoluene, α- and p-methylstyrene, α-butylstyrene, 4-n-butylstyrene, 4-n-decylstyrene and styrene.Acrylonitrile and methacrylonitrile are examples of suitable nitriles.

[0041] Suitable vinyl halides include, for example, ethylenically unsaturated compounds substituted with chlorine, fluorine or bromine, such as vinyl chloride or vinylidene chloride, and mixtures thereof.

[0042] For the preparation of suitable water-dispersible polymers P, suitable nonaromatic hydrocarbons having 2 to 8 carbon atoms and at least two olefinic double bonds are also present, for example butadiene, isoprene and chloroprene.

[0043] Other monomers which may be present in the water-dispersible polymer P in an amount of preferably 0 to 40% by weight, preferably 0 to 20% by weight, most preferably 0.2 to 10% by weight are especially (meth)acrylic acids C1-C 10 Hydroxyalkyl esters, (meth)acrylamide and its derivatives substituted on the nitrogen by C1-C4-alkyl, ethylenically unsaturated carboxylic acids, dicarboxylic acids, their half esters and anhydrides, for example (meth)acrylic acid, maleic acid, fumaric acid, maleic anhydride, maleic acid and fumaric acid half esters and itaconic acid.

[0044] In a particularly preferred embodiment of the use or process according to the invention, the at least one water-dispersible polymer P is selected from poly(meth)acrylate polymers, styrene-(meth)acrylate copolymers and vinyl acetate-(meth)acrylate copolymers.

[0045] In all embodiments of the use or process according to the invention, the at least one water-dispersible polymer P has a glass transition temperature T measured by DSC according to ISO 11357 of <0°C, in particular <-5°C, preferably <-10°C, more preferably <-20°C, most preferably <-30°C. g .

[0046] Preferably, the at least one water-dispersible polymer P has a glass transition temperature (T ) determined by DSC according to ISO 11357 of -60°C to -5°C, more preferably -50°C to -10°C, most preferably -40°C to -10°C. g ).

[0047] The term "glass transition temperature" means the temperature above which a polymer component becomes soft and flexible and below which it becomes hard and glassy, ​​measured by differential scanning calorimetry (DSC) according to ISO 11357 standard. The measurement can be carried out with a Met tler Toledo 822e apparatus at a heating rate of 2°C / min. T can be determined from the measured DSC curve with the aid of DSC software. g value.

[0048] The number average molecular weight (M) of suitable water-dispersible polymers P is n ) is preferably 5,000-200,000 g / mol, preferably 25,000-200,000 g / mol, most preferably 50,000-200,000 g / mol. The weight average molecular weight (M) of a suitable water-dispersible polymer P is w) is 50,000-800,000 g / mol, preferably 100,000-800,000 g / mol, most preferably 150,000-800,000 g / mol.

[0049] Preferably, the number average molecular weight (M n ) is not more than 200,000 g / mol and the weight average molecular weight (M w ) is at least 100,000 g / mol.

[0050] The number-average and weight-average molecular weights can be determined by gel permeation chromatography using polystyrene as standard on polymer solutions in tetrahydrofuran.

[0051] The water-dispersible polymer P can be prepared by free-radical polymerization using mass polymerization, solution polymerization, suspension polymerization or emulsion polymerization techniques, which are known to those skilled in the art. Preferably, the polymer is obtained by solution polymerization with subsequent dispersion in water, or in particular by emulsion polymerization, to obtain an aqueous polymer dispersion.

[0052] According to one or more embodiments of the present invention, the aqueous polymer dispersion comprises one or more polyacrylate polymers as polymer P. Preferably, the aqueous polymer dispersion is an aqueous polyacrylate dispersion, wherein the amount of other polymers than polyacrylate is less than 5.0 wt. %, preferably less than 2.5 wt. %, most preferably less than 1.0 wt. %, based on the total weight of the aqueous polymer dispersion.

[0053] Suitable polyacrylate dispersions and processes for their preparation are described, for example, in EP 0 490 191 A2, DE 198 01 892 A1 and EP 0 620 243.

[0054] Suitable commercially available aqueous polyacrylate dispersions of the preferred polymer P include S 410, V 278, DS 5017 290D, A 323, A378, 380, S 559, S 790, 5036, 5047 (from BASF), EAF 60 and EAF 67 (from APP), DM 1340 (from Celanese), CA 162, E-3362, 2620, 928ER, CA 172, 4400 and A920 (from DowChemical), D 310 (from Synthomer), EP 17, 240HD and EAF68 (from Wacker).

[0055] The aqueous polymer dispersion comprising a preferred embodiment of the polymer P may comprise two or more different polyacrylate polymers having different glass transition temperatures and different monomer compositions as polymer P. The aqueous polymer dispersion comprising two or more different polyacrylate polymers can be prepared by mixing commercially available polyacrylate dispersions, such as those described above.

[0056] In a particularly preferred embodiment of the use or the process according to the invention, the at least one polymer P is comprised in the aqueous polymer dispersion composition in an amount of at least 22% by weight, preferably at least 25% by weight, more preferably at least 28% by weight, most preferably at least 30% by weight, based on the total weight of the aqueous polymer dispersion composition.

[0057] The water-based polymer dispersion composition used for the use and process of the present invention preferably additionally comprises at least one polyolefin oligomer PIB. The at least one polyolefin oligomer PIB is liquid at 23° C. and standard pressure.

[0058] The term "liquid" means in this context that the substance in question is a nearly incompressible fluid which conforms to the shape of its container but maintains a (nearly) constant volume regardless of pressure.

[0059] In a particularly preferred embodiment of the use or process according to the invention, at least one polyolefin oligomer PIB is present in the water-based polymer dispersion composition to be used for the use and process according to the invention in a total amount of 0.5 to 10.0 wt.-%, preferably 1.0 to 5.0 wt.-%, more preferably 1.5 to 4.0 wt.-%, based on the total weight of the water-based polymer dispersion composition.

[0060] All polyolefin oligomers that are liquid under the above conditions are suitable for the purpose of the present invention. The term "polyolefin" includes all polymers obtained by polymerization of olefin monomers such as 1-ethylene, propylene, 1-butene, 2-butene, isobutylene and higher olefins and mixtures thereof. Preferred monomers include C4 unsaturated monomers such as 1-butene and isobutylene, which can be used as a mixture.

[0061] In a preferred embodiment, the at least one polyolefin oligomer PIB comprises or consists of a polybutene oligomer and / or a polyisobutylene oligomer. Most preferred is a polyisobutylene oligomer.

[0062] Suitable and preferred polyisobutylene oligomers for use as the polyolefin oligomer PIB include V190, V 230, V 500, V 640, V700 and V 1500 (BASF) and L-8, H-100 and H-2100 (INEOS) and 150(KEMAT).

[0063] The water-based polymer dispersion composition for the use and process according to the invention preferably comprises at least one hydrogenated mixture ALK of alkanes, isoalkanes and / or cycloalkanes having a boiling point of at least 150° C., in particular >200° C., preferably >250° C., more preferably >300° C., most preferably >350° C., which is liquid at 23° C. and standard pressure.

[0064] The term "liquid" means in this context that the substance in question is a nearly incompressible fluid which conforms to the shape of its container but maintains a (nearly) constant volume regardless of pressure.

[0065] Preferably, the hydrogenated mixture of at least one alkane, isoalkane and / or cycloalkane ALK has a boiling point > 200°C, preferably > 250°C, more preferably > 300°C, most preferably > 350°C.

[0066] The hydrogenated mixture ALK of at least one alkane, isoalkane and / or cycloalkanes preferably comprises alkanes, isoalkanes and / or cycloalkanes based on the C10-C30 fraction, preferably the C12-C25 fraction, more preferably the C13-C23 fraction.

[0067] The hydrogenation mixture ALK of at least one alkane, isoalkane and / or cycloalkane preferably comprises aromatic compounds (hydrocarbons having an aromatic moiety), such as substituted or unsubstituted benzene and substituted or unsubstituted naphthalene, in an amount of <1 wt.-%, preferably <0.5 wt.-%, more preferably <0.1 wt.-%.

[0068] Suitable hydrogenation mixtures ALK for at least one alkane, isoalkane and / or cycloalkane are, for example G 400H, G 280H, G 3H(TOTAL).

[0069] Preferably, at least one hydrogenated mixture of alkanes, isoalkanes and / or cycloalkanes ALK is present in the water-based polymer dispersion composition in a total amount of 0.5-10.0 wt%, preferably 1.0-5.0 wt%, most preferably 1.5-4.0 wt%, based on the total weight of the water-based polymer dispersion composition.

[0070] The water-based polymer dispersion compositions used for the uses and processes according to the invention preferably comprise at least one filler.

[0071] Fillers influence the rheological properties of the uncured composition and the mechanical properties and surface properties of the fully cured composition. Suitable fillers are inorganic and organic fillers, such as natural, ground or precipitated chalk (which is entirely or mainly composed of calcium carbonate), and which are optionally coated with fatty acids, more particularly stearic acid; barium sulfate (BaSO4, also known as barite or precipitated crystal stone), calcined kaolin, aluminum oxide, aluminum hydroxide, silicon dioxide, especially finely divided silicon dioxide from a pyrolysis process, carbon black, especially industrially manufactured carbon black, titanium dioxide, PVC powder or hollow beads. Preferred fillers are calcium carbonate, calcined kaolin, carbon black, finely divided silicon dioxide and flame retardant fillers, such as hydroxides or hydrates, especially aluminum hydroxides or hydrates, preferably aluminum hydroxide.

[0072] It is entirely possible and may even be advantageous to use mixtures of different fillers.

[0073] Chalk (calcium carbonate) is very preferred as filler for the composition of the invention. Uncoated chalk is particularly preferred, and uncoated ground chalk is most preferred, such as is available under the trade name 40GU (Omya AG, Switzerland) obtained.

[0074] The type and amount of filler are not particularly limited in the present invention. Examples of suitable fillers include calcium carbonate, calcium sulfate and calcium-containing minerals such as limestone, calcite, chalk, dolomite, wollastonite, gypsum, apatite, phosphate rock and mixtures thereof.

[0075] The term "filler" in the present disclosure refers to a solid particulate material which is typically used as a filler in a water-based polymer dispersion composition and has a low water solubility. Preferably, the filler has a water solubility of less than 0.1 g / 100 g water at a temperature of 20°C, more preferably less than 0.05 g / 100 g water, and most preferably less than 0.01 g / 100 g water.

[0076] Preferably, the filler has a median particle size d in the range of 1.0-100.0 μm, more preferably 1.0-60.0 μm, most preferably 2.0-50.0 μm.50 .

[0077] In this disclosure, the term "median particle size d 50 ” refers to the particle size at which 50% by volume of all particles are smaller than the d50 value. The term “particle size” refers to the area-equivalent spherical diameter of the particle. The particle size distribution can be measured by laser diffraction according to the method described in standard ISO 13320:2009. A Mastersizer 2000 device (trademark of Malvern Instruments Ltd, GB) can be used to measure the particle size distribution.

[0078] Preferably, the one or more fillers are present in the water-based polymer dispersion composition in a total amount of 10.0-60.0 wt%, preferably 20.0-60.0 wt%, most preferably 40.0-60.0 wt%, based on the total weight of the water-based polymer dispersion composition.

[0079] In the same or different preferred embodiments, the filler preferably comprises chalk and / or dolomite.

[0080] According to one or more embodiments, in particular when the intended use of the polymer dispersion composition is as a coating, the water content of the polymer dispersion composition is 10-70 wt %, preferably 15-60 wt %, and most preferably 20-50 wt %, based on the total weight of the polymer dispersion composition.

[0081] According to one or more embodiments, in particular when the intended use of the polymer dispersion composition is as a joint sealant or adhesive, the water content of the polymer dispersion composition is 5-45 wt. %, preferably 10-35 wt. %, most preferably 12-30 wt. %, based on the total weight of the polymer dispersion composition.

[0082] According to one or more embodiments, the solids content of the polymer dispersion composition is 40-95 wt%, preferably 50-90 wt%, and most preferably 65-85 wt%.

[0083] As used herein, solid content refers to the portion of the aqueous polymer dispersion composition that is not volatile when heated to a temperature of 105° C. at one atmosphere of pressure for one hour. Thus, solid content refers to polymeric materials, nonvolatile plasticizers, inorganic solids, and nonvolatile organic materials, while the non-solid portion is typically composed of water and any organic material that is readily volatile at 105° C.

[0084] According to one or more embodiments, the weight ratio of water to polymer P in the polymer dispersion composition is from 3:2 to 1:4, preferably from 1:1 to 1:3, most preferably from 9:11 to 3:7.

[0085] According to one or more embodiments, the water-dispersible polymer P is present in the polymer dispersion composition in a total amount of 21.0-65.0 wt%, preferably 25.0-55.0 wt%, most preferably 30.0-45.0 wt%, based on the total weight of the polymer dispersion composition.

[0086] The water-based polymer dispersion composition used for the use and method of the present invention optionally and preferably contains one or more plasticizers PL having at least one ester or ether group. The amount of plasticizer PL depends on the intended application and the polymer P used. g Very soft polymers P (e.g. -60°C) do not necessarily require the addition of plasticizers PL or use very small amounts of plasticizers PL for processing. g When the polymer P has a temperature of, for example, -10°C, it is recommended to use preferably higher amounts of plasticizer PL.

[0087] One or more plasticizers PL having at least one ester or ether group are preferably used in the aqueous polymer dispersion composition in a total amount of 0.5-30.0 wt. %, preferably 1.0-20 wt. %, in particular 2.5-15.0 wt. %, based on the total weight of the aqueous polymer dispersion composition.

[0088] Suitable plasticizers PL are liquid or solid inert organic substances with a low vapor pressure, which preferably have a boiling point measured at standard pressure above 200° C. The plasticizers may be chosen from adipic and sebacic acid plasticizers, phosphoric acid plasticizers, citric acid plasticizers, fatty acid esters and epoxidized fatty acid esters, polypropylene glycol, polyethylene glycol, benzoic acid esters and phthalic acid esters or esters of 1,2-dicarboxycyclohexane.

[0089] Suitable fatty acid esters include alkyl esters of fatty acids containing more than 14 or more than 16 carbon atoms, for example alkyl esters of lauric acid, myristic acid, stearic acid, arachidic acid and behenic acid, and mixtures thereof. Suitable fatty alcohols are alcohols of the above-mentioned fatty acids, for example obtainable from fatty acids or their esters using methods known to those skilled in the art.

[0090] In a preferred embodiment of the process according to the invention, the plasticizer PL having at least one ester or ether group is selected from phthalates, cyclohexane esters or benzoates.

[0091] In a particularly preferred embodiment of the use or the process according to the invention, the plasticizer PL is a phthalate or a hydrogenated phthalate, preferably diisononyl-1,2-cyclohexanedicarboxylate.

[0092] In a particularly preferred embodiment of the use or method according to the present invention, the water-based polymer dispersion composition comprises at least one plasticizer PL as described above and / or comprises at least one polyolefin oligomer PIB as described above and / or comprises at least one hydrogenated mixture ALK of alkanes, isoalkanes and / or cycloalkanes as described above, wherein the total amount of the combined amount of polyolefin oligomer PIB, hydrogenated mixture ALK and plasticizer PL in the composition before drying is 0-20% by weight, preferably 3-15% by weight, more preferably 5-10% by weight, based on the total water-based polymer dispersion composition.

[0093] The water-based polymer dispersion composition used in the use and method of the invention further comprises at least one surfactant, preferably a nonionic surfactant. In the use or method of the invention, a surfactant is required to ensure homogeneity of the composition before application and sufficient wetting of the substrate.

[0094] Suitable surfactants include anionic surfactants, nonionic surfactants, cationic surfactants or amphoteric surfactants, but preferably nonionic surfactants or anionic surfactants are used, and nonionic surfactants are most preferred. Typically, the amount of surfactant used is 0.1-5% by weight, based on the total weight of the polymer dispersion composition.

[0095] Suitable and preferred nonionic surfactants include polyethylene oxide condensates of alkylphenols, polyoxyalkylene derivatives of propylene glycol, condensates of ethylene oxide with the reaction products of propylene oxide and ethylenediamine, ethylene oxide condensates of aliphatic alcohols, long-chain tertiary amine oxides, long-chain tertiary phosphine oxides, fatty acid ethoxylates and long-chain dialkyl sulfoxides. Useful anionic surfactants include those obtained by alkylating aromatic cores, alkylated aromatic hydrocarbons obtained by sulfonation, and neutralizing sulfonated products. Alkylbenzene sulfonates, such as dodecylbenzene sulfonate, are typical representatives of this class. Fatty alcohol sulfates can also be used as surfactants. Fatty acid ethoxylates are preferred.

[0096] The water-based polymer dispersion composition for the use and process of the invention also comprises at least one dispersant, in particular a polymeric ammonium or sodium salt of a carboxylic acid copolymer. Dispersants are required to ensure the stability of the dispersion, especially when large amounts of polymer P and / or fillers are used.

[0097] Suitable dispersants include all dispersants commonly used in the field of water-based polymer dispersion compositions, but preference is given to using nonionic or anionic surfactants, most preferably polymeric ammonium salts of carboxylic acid copolymers. These types of dispersants have a particularly high compatibility with the preferred polymers P and exhibit particularly good dispersion stability. Typically, the amount of dispersant used is 0.1 to 5% by weight, based on the total weight of the polymer dispersion composition.

[0098] The water-based polymer dispersion composition used for the uses and methods of the present invention may also contain one or more tackifiers. Examples of suitable tackifiers may include hydrocarbon resins or hydrogenated products thereof, rosins or hydrogenated products thereof, rosin esters or hydrogenated products thereof, terpene resins or hydrogenated products thereof, terpene phenolic resins or hydrogenated products thereof, and polymerized rosins or polymerized rosin esters or acrylic liquid resins.

[0099] The water-based polymer dispersion composition used for the purposes and methods of the present invention may also contain one or more other additives, such as wetting agents, emulsifiers, thickeners, defoamers, flame retardants, stabilizers, colorants, antioxidants, UV absorbers and / or biocides. These other additives commonly used in water-based dispersion additives are known to those skilled in the art.

[0100] Suitable defoamers are preferably compounds based on mineral oils or silicones. Suitable thickeners include compounds based on (meth)acrylic acid copolymers, cellulose derivatives, mineral thickeners such as clays, silica or mixtures thereof.

[0101] Biocides (preservatives) may be added to the polymer dispersion composition according to the invention in an amount of up to 2 wt. %, preferably 0.2 to 1.8 wt. %, more preferably 0.4 to 1.5 wt. % biocide relative to the total polymer dispersion composition.

[0102] Generally, any known type of biocide (also known as a preservative) can be used in the compositions of the present invention.

[0103] Suitable preservatives are the customary preservatives, for example benzisothiazolinone (BIT), methylisothiazolinone (MIT), octylisothiazolinone (OIT) and chloromethylisothiazolinone (CMIT).

[0104] According to one or more embodiments, the total amount of other additives is preferably 0-15.0 wt%, more preferably 0-10.0 wt%, based on the total weight of the polymer dispersion composition.

[0105] The polymer dispersion composition can be prepared by mixing the ingredients together at room temperature. Any suitable mixing apparatus can be used to prepare the polymer dispersion composition.

[0106] When used as adhesives, the polymer dispersion compositions are particularly suitable for bonding and sealing applications on alkaline substrates in the construction industry, in particular for the bonding of modular floors on fresh cement screeds or for the bonding of components on fresh concrete.

[0107] When used as a sealant, the polymer dispersion composition is particularly suitable for sealing joints, seams or cavities in alkaline substrates in construction, especially for sealing expansion joints or connection joints between components.

[0108] When used as a coating, the polymer dispersion composition is particularly suitable for protecting alkaline substrates, especially floors or walls, in particular as a coating for balconies, terraces, open spaces, bridges, car parks, or for sealing roofs, especially flat roofs or slightly sloping roof areas or roof gardens, or for water sealing inside buildings, for example under tiles or ceramic slabs in plumbing units or in kitchens, or as a floor covering in kitchens, industrial buildings or manufacturing spaces, or as a seal in collecting tanks, channels, shafts, silos, tanks or wastewater treatment plants.

[0109] The polymer dispersion compositions are particularly suitable for sealing joints in alkaline substrates or coating alkaline substrates having a pH of at least 10 when wetted with water, including fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paints. However, the polymer dispersion compositions are also suitable for other substrates commonly found in construction, such as wood, metals and alloys, dry mineral or concrete substrates, natural stone and other substrates commonly found in construction.

[0110] The polymer dispersion composition according to the invention preferably has a tack of 0 (zero) g after drying for 28 days at 23° C. in air at 50% relative humidity, the tack being defined by the amount of quartz sand (0.7 mm - 1.2 mm particle size) poured onto the surface of a specimen in the form of a disk having a diameter of 4.2 mm and a height of 5 mm and dried in air at 23° C. and 50% rh, when the specimen is turned 180° after the addition of the sand with the side covered with the sand facing downwards, and the amount of sand still adhering to the surface is used to determine the tack.

[0111] The water-based polymer dispersion composition to be used for the use and method of the present invention preferably exhibits a Shore A hardness of less than 50, in particular 5-40, preferably 10-35, more preferably 15-30, most preferably 15-25 after drying in air at 23° C. and 50% relative humidity for 28 days. The Shore A hardness is most preferably about 20.

[0112] According to another aspect of the present invention, there is provided a method for sealing a joint between two substrates and / or coating a surface of a substrate and / or bonding two substrates, the method comprising the following steps:

[0113] i) applying a water-based polymer dispersion composition as described above into a joint between two substrates and / or on the surfaces of the substrates to form a wet film of the composition thereon,

[0114] ii) optionally joining a second substrate to the first substrate so that the wet film on the first substrate is in contact with the second substrate, or so that the two wet films on the two substrates are in contact with each other to achieve bonding therebetween,

[0115] iii) exposing the wet sealant in the filled joints and / or the wet film of sealant on the surface to air until the joint sealant and / or the surface film are dry,

[0116] At least one substrate surface to which the wet composition is applied consists of an alkaline substrate having a pH of at least 10 when wetted with water, wherein the alkaline substrate is fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint.

[0117] All embodiments of the water-based polymer dispersion composition described for the inventive use also apply to the inventive method described herein, in particular the preferred embodiments of the water-based polymer dispersion composition or its ingredients or properties.

[0118] Concrete and other hydraulic binder compositions are usually applied in liquid form to a mold and initially hardened there, after which the mold is removed. At this point the concrete has begun to harden, but is still "green" and highly alkaline on the surface. Only after demoulding can the excess water evaporate and final drying can take place. As discussed in the introduction to this document, common curable compositions of the prior art are usually applied several weeks after the concrete has been demoulded to ensure sufficient drying and low alkalinity of the surface.

[0119] In a preferred embodiment of the method of the invention as further described above, the water-based polymer dispersion composition is applied to the alkaline substrate within 10 days, preferably within 8 days, more preferably within 5 days, most preferably within 3 days after the alkaline substrate itself has been applied in wet, uncured form or has been demoulded in the case of an initially molded substrate such as concrete. Most preferably, the water-based dispersion composition is applied to the substrate between 1 and 3 days after the substrate has been applied or demoulded while still alkaline.

[0120] In a preferred such embodiment, the water-based polymer dispersion composition is applied to the demoulded concrete substrate, preferably to the surface thereof that was covered by the mold prior to demoulding.

[0121] The polymer dispersion composition can be applied to the surface of the substrate using, for example, a toothed trowel or a roller.

[0122] Example

[0123] The present invention is further explained in the following experimental part, however, these experimental parts should not be construed as limiting the scope of the present invention. Unless otherwise stated, the ratios and percentages shown are all by weight. Therefore, "weight %" refers to the weight percentage based on the weight of the total composition given in the corresponding case. "RT" refers to room temperature or ambient temperature and describes a temperature of 23°C. The abbreviation "rh" or "%rh" refers to the relative humidity (in %) of the ambient air in a given embodiment or test method.

[0124] Test Method

[0125] Adhesion properties (failure mode) were determined by adhesive strip adhesion test at 23°C on differently aged green (fresh) concrete samples according to DIN EN ISO 21194. One test series was carried out on green concrete 24 hours after demolding, a second series was carried out 3 days after demolding of the green concrete, and a third series was carried out 6 days after demolding of the green concrete. Adhesion samples of the tested polymer dispersion compositions were dried at room temperature for 28 days. The second series of samples were likewise dried, but additionally subjected to water immersion for 7 days (28d RT plus 7 days H2O). The third series of samples were again additionally subjected to a temperature of 40°C for 7 days and then evaluated for adhesion (28d RT+7 days H2O+7 days 40°C). The adhesion properties in Tables 6-9 are classified as 1-5, where 1 is the best adhesion (100% cohesive failure) and 5 is the worst adhesion (100% adhesive failure). The increasing numbers 2-4 in between indicate adhesion property curves with increasing adhesion failure modes, so that the adhesion properties become worse.

[0126] Production of concrete substrates:

[0127] Adhesion was tested on new cement mortar prisms prepared as follows:

[0128] A series of different green concrete samples C-1 to C-5 were prepared for use as substrates in adhesion testing. The exact composition of each concrete sample is listed in Table 1.

[0129] In all preparations, a dry mix was first prepared by mixing all solid ingredients (eg cement, sand, fillers, etc.) until visually homogeneous.

[0130] Then, a liquid mixture is prepared by mixing all liquid ingredients (including water) into a homogeneous liquid mixture.

[0131] The liquid mixture was then added to the dry blend with manual stirring until a homogeneous viscous mixture was obtained.

[0132] The homogeneous concrete mixture thus obtained was then poured into a silicone mould lined with PTFE foil. The final dimensions of each fresh concrete sample were 14.5 cm x 14.5 cm x 1 cm and the weight was approximately 100 g.

[0133] The samples were then stored under standard climatic conditions.

[0134] After 24 hours, the cured but still fresh concrete substrate samples were removed from the mold, brushed on the outer parts with a steel brush and dusted. After the waiting times specified above (24 hours, 3 days or 6 days under standard climatic conditions, i.e. 23° C. and 50% RH), the test polymer dispersion compositions described below were applied to the fresh (green) mortar prisms thus prepared and demoulded.

[0135]

[0136] Table 1: Example compositions. *Adjusted to pH 8 by NaOH (25 wt% in water)

[0137] Raw materials, such as water-based polymer dispersion compositions

[0138] The raw materials used for the example polymer dispersion compositions are shown in Table 2 along with their description with respect to important properties.

[0139]

[0140] Table 2: Raw materials used in example compositions. * "Solids" defines the weight concentration of polymer P in the respective aqueous dispersion.

[0141] Example Composition

[0142] Several inventive and non-inventive (reference) polymer dispersion compositions were prepared from the starting materials in Table 2 using the following procedure.

[0143] Mixing Steps

[0144] All example compositions were prepared in a laboratory mixer using the following procedure:

[0145] a) Acronal V278 acrylic dispersion or VAc-EHA dispersion was adjusted to pH 8 by using caustic soda (25 wt% NaOH in water).

[0146] b) Adding liquid raw materials except acrylic thickener.

[0147] c) Add the powdered material in several steps, interrupted by stirring at each step. After all the powder has been added, disperse the powder for 10 minutes.

[0148] d) Adding an acrylate thickener.

[0149] e) Mix under vacuum and fill the formulation into cartridges.

[0150] f) The cartridges were stored at 23°C and 50% rh for at least 24 hours before starting the test procedure.

[0151] Details of Example Compositions

[0152] Several comparative (denoted "R") and inventive (denoted "I") example compositions were prepared from the raw materials in Table 1 according to the mixing procedures detailed above. The composition and relative amounts (in weight %) of the raw materials are shown in Tables 3 and 4.

[0153] Composition (wt.-%) I1 I2 I3 I4 R5 R6 I7 R8 Acronal V278(pH 8*) 37 37 37 37 29 21 37 - VAc-EHA(pH 8*) - - - - - - - 32.3 Nonionic surfactants 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.5 Dispersants 0.5 0.5 0.5 0.5 0.5 0.5 0.5 0.4 DINP 4 6 6 8 5.5 7 - 6 DINCH - - - - - - 4 - Hydroseal G400H 2 - 2 - 2 2 2 - Glissopal V1500 2 2 - - 2 2 2 - <![CDATA[CaCO3]]> 52 52 52 52 58.5 65 - - dolomite - - - - - - 50.1 58.3 <![CDATA[TiO2]]> - - - - - - 2 1.5 Acrylic thickener 1 1 1 1 1 1 1 1 Clay Thickener 1 1 1 1 1 1 0.9 1

[0154] Table 3: Example compositions. * Adjust to pH 8 with NaOH (25 wt% in water)

[0155]

[0156]

[0157] Table 4: Example compositions. * Adjust to pH 8 with NaOH (25 wt% in water)

[0158] Other comparative compositions

[0159] Additional comparative sealants or adhesives were used in some test scenarios. These comparative compositions are commercial products based on different chemically cured matrix polymers. They are listed in Table 5 below:

[0160]

[0161] Table 5: Comparative sealants used for comparison with the compositions of the present invention.

[0162] Test results of adhesion tests on different raw concrete samples

[0163] The results of the test methods used for each example composition are described in detail in Tables 6 to 9. The term "RT" means that the applied specimens of the test composition on green concrete were stored under standard climatic conditions (23° C., 50% relative air humidity) for a specified time in days ("d"). "40° C." means storage in an oven at 40° C. "H2O" means storage immersed in water.

[0164] Concrete condition I1 I2 I3 I4 R5 R6 I7 R8 C-1(24h) 28d RT 1 2 2 2 5 coa 1 5 C-1(24h) 28d RT+7d 40℃ 4 4 4 4 5 coa 1 5 C-1(24h) <![CDATA[28d RT+7d 40℃+7d H2O]]> 3 1 1 2 5 coa 1 5 C-1(3d) 28d RT 2 2 3 2 5 coa n / m 5 C-1(3d) 28d RT+7d 40℃ 4 4 4 4 5 coa n / m 5 C-1(3d) <![CDATA[28d RT+7d 40℃+7d H2O]]> 3 3 1 3 5 coa n / m 5

[0165] Table 6: Test results (adhesion on green concrete aged 24 hours and 3 days, respectively). "coa" means that the sample set and was not usable. "n / m" means that the test was not performed and the corresponding value was not measured.

[0166] The results of Table 6 show that the compositions I1-I4 and I7 according to the invention exhibit significantly better adhesion on green concrete than the comparative compositions R5 and R8. The comparative composition R6, which has too low a content of polymer P (13% by weight, based on the total composition), coagulated and could not be used in the test protocol.

[0167]

[0168] Table 7: Test results (adhesion on green concrete samples C-2 and C-3 aged 6 days).

[0169] The results in Table 7 show that softer compositions (with higher amounts of plasticizer) lead to advantageous improvements in adhesion and adhesion stability, especially after water storage and subsequent heat storage.

[0170]

[0171] Table 8: Test results (adhesion on green concrete samples C-2 and C-3 aged 6 days). "des" means that the sealant sample disintegrated (failed) during the measured storage period.

[0172]

[0173] Table 9: Test results (adhesion on green concrete samples C-3 to C-5 aged 6 days). "f" refers to a flat untreated concrete sample, while "s" refers to a concrete sample that was sanded to roughen the surface before applying the composition.

[0174] The results in Tables 8 and 9 show that only the water-based polymer dispersion compositions of the present invention produce adequate and durable adhesion on green concrete. Sealants based on other curing chemistries, including polyurethanes, organosilane-modified polymers, and silicones, do not function as adhesively stable sealants on green concrete. This is true for both untreated and mechanically surface treated concrete surfaces.

[0175] Other comparative compositions

[0176] Several additional comparative (designated "R") example compositions not in accordance with the invention were prepared from the raw materials in Table 1 according to the mixing procedure detailed above.

[0177] These comparative compositions use T g (>0° C.) are not suitable for polymer dispersions for the use according to the invention.

[0178] The composition and relative amounts (in wt %) of the raw materials are shown in Table 10.

[0179] Composition (wt.-%) R19 R20 R21 R22 R23 <![CDATA[Axilat DS 910(pH 8 * )]]> 32 32 - - - <![CDATA[ECO 6716(pH 8 * )]]> - - 32 - - <![CDATA[AC 31(pH 8 * )]]> - - - 32 - <![CDATA[PST 50A(pH 8 * )]]> - - - - 32 Nonionic surfactants 0.5 0.5 0.5 0.5 0.5 Dispersants 0.5 0.5 0.5 0.5 0.5 DINP - 10 10 10 10 dolomite 65 55 55 55 55 Acrylic thickener 1 1 1 1 1

[0180] Table 10: Comparative compositions. * Adjust to pH 8 with NaOH (25 wt% in water)

[0181] Compositions R19-R23 were subsequently tested on green concrete using the protocol described above and are shown in Table 6. The results of these adhesion tests are shown in Table 11.

[0182] Concrete condition R19 R20 R21 R22 R23 C-1(24h) 28d RT 5 5 5 5 5 C-1(24h) 28d RT+7d 40℃ 5 5 5 5 5 C-1(3d) 28d RT 5 5 5 5 5 C-1(3d) 28d RT+7d 40℃ 5 5 5 5 5

[0183] Table 11: Test results (adhesion on green concrete with 24h and 3d aging, respectively).

[0184] The data in Table 11 show that based on T g Compositions of polymers having a temperature above 0°C are not suitable for use in the present invention.

Claims

1. Use of a water-based polymer dispersion composition, the water-based polymer dispersion composition comprising: a) more than 20% by weight, based on the total composition, of at least one water-dispersible polymer P, dispersed in water in a concentration of 40 to 80% by weight, based on the dispersion of the water-dispersible polymer P, wherein the at least one water-dispersible polymer P has a glass transition temperature T<0° C. g , which is determined by DSC according to ISO 11357 standard, b) at least one surfactant, preferably a nonionic surfactant, c) at least one dispersant, in particular a polymeric ammonium or sodium salt of a carboxylic acid copolymer, and d) optionally, at least one plasticizer PL having at least one ester or ether group, It is used as an adhesive, sealant or coating to be applied to at least one alkaline substrate which has a pH of at least 10 when wetted with water, wherein the alkaline substrate is fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint.

2. The method according to claim 1, wherein the at least one water-dispersible polymer P is selected from the group consisting of poly(meth)acrylate polymers, styrene-(meth)acrylate copolymers and vinyl acetate-(meth)acrylate copolymers.

3. The method according to claim 1 or 2, wherein the at least one water-dispersible polymer P has a glass transition temperature T<-5°C, preferably <-10°C, more preferably <-20°C, most preferably <-30°C, determined by DSC according to ISO 11357. g .

4. The use according to any one of claims 1 to 3, wherein the water-based polymer dispersion composition further comprises at least one polyolefin oligomer PIB which is liquid at 23°C and standard pressure and is preferably selected from polybutene and / or polyisobutylene.

5. The use according to any one of claims 1 to 4, wherein the water-based polymer dispersion composition further comprises at least one hydrogenated mixture ALK of alkanes, isoalkanes and / or cycloalkanes having a boiling point of at least 150°C, which is liquid at 23°C and standard pressure.

6. The use according to any one of claims 1 to 5, wherein the at least one polymer P is contained in the water-based polymer dispersion composition in an amount of at least 22% by weight, preferably at least 25% by weight, more preferably at least 28% by weight, most preferably at least 30% by weight, based on the total weight of the water-based polymer dispersion composition.

7. The use according to any one of claims 1 to 6, wherein the water-based polymer dispersion composition exhibits a Shore A hardness of less than 50 after drying in air at 23°C and 50% relative humidity for 28 days.

8. The use according to any one of claims 1 to 7, wherein the composition further comprises at least one filler in an amount of 40% to 60% by weight, based on the total composition, wherein the filler preferably comprises chalk and / or dolomite.

9. The use according to claim 4, wherein the at least one polyolefin oligomer PIB is present in the water-based polymer dispersion composition in a total amount of 0.5-10.0 wt%, preferably 1.0-5.0 wt%, more preferably 1.5-4.0 wt%, based on the total weight of the water-based polymer dispersion composition.

10. The use according to claim 5, wherein the at least one hydrogenated mixture of alkanes, isoalkanes and / or cycloalkanes ALK is present in the water-based polymer dispersion composition in a total amount of 0.5-10.0 wt. %, preferably 1.0-5.0 wt. %, most preferably 1.5-4.0 wt. %, based on the total weight of the water-based polymer dispersion composition.

11. The use according to any one of the preceding claims, wherein the water-based polymer dispersion composition comprises at least one plasticizer PL and / or comprises at least one polyolefin oligomer PIB and / or comprises at least one hydrogenated mixture ALK comprising alkane, isoalkane and / or cycloalkane, wherein the total amount of the combined amount of polyolefin oligomer PIB and hydrogenated mixture ALK and plasticizer PL in the composition before drying is from 0 to 20% by weight, preferably from 3 to 15% by weight, more preferably from 5 to 10% by weight, based on the total water-based polymer dispersion composition.

12. Use according to any one of the preceding claims, wherein the plasticizer PL is a phthalate or a hydrogenated phthalate, preferably diisononyl-1,2-cyclohexanedicarboxylate.

13. A method for sealing a joint between two substrates and / or coating a surface of a substrate and / or bonding two substrates, the method comprising the steps of: i) applying the water-based polymer dispersion composition according to any one of claims 1 to 12 into a joint between two substrates and / or on the surfaces of the substrates to form a wet film of the composition thereon, ii) optionally joining a second substrate to the first substrate so that the wet film on the first substrate is in contact with the second substrate, or so that the two wet films on the two substrates are in contact with each other to achieve bonding therebetween, iii) exposing the wet sealant in the filled joints and / or the wet film of sealant on the surface to air until the joint sealant and / or the surface film are dry, Wherein at least one substrate surface to which the wet composition is applied consists of an alkaline substrate having a pH of at least 10 when wetted with water, wherein the alkaline substrate is fresh concrete, fresh cement mortar, fresh lime mortar or fresh lime or silicate paint.

14. The method according to claim 13, wherein the water-based polymer dispersion composition is applied to the alkaline substrate within 10 days, preferably within 8 days, more preferably within 5 days, most preferably within 3 days after the alkaline substrate itself has been applied or produced in a wet, uncured form or has been demoulded.

15. The method according to claim 14, wherein the water-based polymer dispersion composition is applied to the demoulded concrete substrate, preferably to the surface thereof which was covered by the mold before demoulding.