Method for preparing PVC and PVC product
By controlling the introduction of comonomers and adding comonomers in batches during emulsion polymerization, the problem that vinyl chloride copolymers in the prior art is difficult to achieve low gelling temperature and improved properties at the same time, and a low gelling temperature is prepared and low viscosity copolymers improve the properties and stability of the polymer.
Patent Information
- Application Number
- CN202380029172.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-21
- Filing Date
- 2023-03-21
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, when preparing copolymers containing vinyl chloride, it is difficult to achieve a combination of low gelling temperature and improved properties simultaneously, especially in terms of viscosity.
By specifically controlling the introduction of comonomers during emulsion polymerization, vinyl chloride and comonomers are added in batches to ensure that the comonomer content is less than 10% by weight and the copolymerization is added individually continuously or multiple times within at least 50% of the reaction time The monomer is then raised and the temperature of the reaction mixture is stripped and the unreacted vinyl chloride is stripped to prepare a copolymer containing vinyl chloride.
The preparation of copolymers with low gelling temperature and low viscosity is achieved, which improves the properties of the polymer, ensures the uniform distribution of comonomers in the copolymer, and enhances the mechanical stability and thermal stability of the product.
Smart Images

Figure BDA0005052415370000181 
Figure BDA0005052415370000191
Abstract
Description
[0001] The present invention relates to a process for preparing copolymers containing vinyl chloride by emulsion polymerization.
[0002] Polyvinyl chloride (PVC) is one of the most important thermoplastic materials on the market today. Due to its very good mechanical and physical properties, it is used in a large number of applications.
[0003] Several methods for preparing PVC are known. For example, PVC can be prepared by suspension polymerization of vinyl chloride in a suspending liquid and in the presence of a suspending agent. This produces a slurry (or suspension) of PVC particles, typically having a particle size of about 30 to 200 microns. The resulting PVC slurry is then dried, typically by centrifugation, followed by fluidized bed drying, to obtain porous (i.e., adsorbent) PVC. PVC prepared by the suspension method is called "S-PVC". S-PVC can absorb plasticizers to obtain a dry blend.
[0004] PVC can also be prepared by a process generally referred to as a paste or emulsion polymerization process. The emulsion polymerization process can be characterized in that the polymerization produces a latex of polymer particles of relatively small size compared to the S-PVC process, typically 0.01 to 5 microns. The latex can be dried, for example by spray drying to produce PVC particles in the form of agglomerates. The dried PVC polymer particles are generally much smaller than the dried particles prepared by the suspension PVC process.
[0005] It is known to add additives to PVC to adapt it for different applications. It is also known to polymerize vinyl chloride monomer in the presence of comonomers that provide improved properties. The most common comonomer used in PVC is vinyl acetate. Another specific class of comonomers that have found application in PVC are alkyl acrylates or alkyl methacrylates.
[0006] For example, WO 2014 / 188971 describes a copolymer containing vinyl chloride prepared by copolymerizing 30 to 98 wt % (inclusive) of an acrylic copolymer prepared by copolymerizing 100 parts by weight of an alkyl (meth)acrylate monomer with 0.1 to 10 parts by weight (inclusive) of a multifunctional monomer with 2 to 70 wt % (inclusive) of a vinyl chloride monomer.
[0007] For example, WO 2015 / 090657 describes a method for preparing a copolymer of a vinyl halide monomer and at least one other monomer B, wherein the monomer B is a monomer whose polymer has a Tg lower than the Tg of the polymer obtained by polymerizing at least one vinyl halide monomer. The method comprises a series of process steps by which different amounts of the corresponding monomers are introduced during the polymerization.
[0008] The addition of alkyl acrylates can provide polymers with improved properties in terms of low gelling temperature, ie polymers with lower gelling temperatures, which is advantageous in many applications. However, this may be at the expense of other advantageous or desirable properties, especially viscosity.
[0009] The present invention relates to copolymers of vinyl chloride and a comonomer, but wherein the comonomer is present in the final product at relatively low levels.
[0010] It is an object of the present invention to provide PVC copolymers which have an improved combination of properties and, in particular, have a relatively low gelling temperature.
[0011] In particular, the present inventors have discovered that improved copolymers containing vinyl chloride can be obtained by polymerizing vinyl chloride with a comonomer in an emulsion polymerization process by specifically controlling the incorporation of the comonomer during the emulsion polymerization process.
[0012] Thus, in a first aspect, the present invention provides a method for preparing a copolymer containing vinyl chloride, the method comprising:
[0013] a. batch copolymerization in an emulsion polymerization process comprising a mixture of vinyl chloride monomer (A) and a comonomer (B), wherein:
[0014] i. The weight ratio of A:B added to the polymerization process is greater than 10:1, and the corresponding copolymer contains less than 10% by weight of the comonomer
[0015] ii. Addition of comonomer (B)
[0016] 1. Continuously for at least 50% of the reaction time, or
[0017] 2. carried out in multiple separate additions with at least 50% of the reaction time separating the initial and final additions, or
[0018] 3. Perform the above combination,
[0019] b. After the reaction time,
[0020] i. raising the temperature of the reaction mixture and
[0021] ii. stripping unreacted vinyl chloride over a period of at least 10 minutes, and
[0022] c. Recovering copolymers containing vinyl chloride.
[0023] The present invention relates to an emulsion polymerization process. The term "emulsion polymerization" as used herein adopts the IUPAC definition "polymerization of an initially heterogeneous system whereby monomers, initiators, dispersion medium and possible colloidal stabilizers form, producing particles of colloidal size containing the polymer formed".
[0024] According to the above definition, and as used herein, emulsion polymerization includes "miniemulsion" and "microsuspension" polymerization methods, also both as defined by IUPAC.
[0025] In some embodiments, the polymerization may be a "seed polymerization," which is a polymerization in which previously prepared polymer particles ("seeds") are added to the process and polymerization is carried out thereon to form larger particles. This enables, for example, the preparation of larger particles than can be obtained from a single step polymerization process and / or the production of bimodal particles with improved properties (such as mechanical stability).
[0026] The copolymer comprises vinyl chloride monomer (A) and comonomer (B). Comonomer (B) is preferably a comonomer that reduces the glass transition temperature of the copolymer compared to PVC homopolymer. In particular, preferably, the copolymer containing vinyl chloride has a glass transition temperature T of less than 82°C. g Such comonomers are known in the art and are in fact often referred to as "soft monomers" because they lower the glass transition temperature. Therefore particularly preferred examples and comonomers for comonomer (B) in the process of the present invention include vinyl carboxylates, vinyl ethers, olefins and alkyl (meth)acrylates. Particularly preferred comonomers (B) are vinyl carboxylates, in particular vinyl acetate, and alkyl (meth)acrylates.
[0027] Additional comonomers may be present in the polymerization, either additional "soft monomers" of the type described above, or other comonomers. However, in all embodiments of the first aspect of the invention, it is required that the corresponding copolymers contain less than 10% by weight of comonomer. Thus, when more than one comonomer is present, the total amount of comonomer in the resulting copolymer must still be less than 10% by weight.
[0028] In a preferred embodiment, the comonomer (B) is an alkyl (meth)acrylate. The term "alkyl (meth)acrylate" is used herein as a shorthand for alkyl acrylate and alkyl methacrylate. For example, butyl (meth)acrylate refers to butyl methacrylate and butyl acrylate.
[0029] In a preferred embodiment, comonomer (B) is an alkyl acrylate. However, when described hereinafter, it should be understood that embodiments of the present invention, even when only acrylates are mentioned, are equally applicable to equivalent methacrylates as well as any other comonomers, unless the context clearly indicates otherwise.
[0030] Preferred alkyl (meth)acrylates contain C1 to C10 alkyl groups. Preferred alkyl groups contain C2 to C8 alkyl groups. Particularly preferred alkyl (meth)acrylates according to the present invention are alkyl acrylates rather than alkyl methacrylates. Particularly preferred alkyl acrylates for use as comonomers according to the present invention are ethyl acrylate, ethylhexyl acrylate, tert-butyl acrylate and n-butyl acrylate, with n-butyl acrylate being most preferred.
[0031] A particular feature of the first aspect of the invention is that the vinyl chloride-containing copolymer obtained contains less than 10% by weight of comonomer.
[0032] The term "copolymer" as used herein encompasses products with a single comonomer (e.g., vinyl chloride with n-butyl acrylate), but also encompasses products with two or more comonomers (e.g., vinyl chloride with n-butyl acrylate and an additional comonomer). For example, a product comprising vinyl chloride and two comonomers may also be referred to as a terpolymer, but such copolymers are included within the definition of copolymer as used herein.
[0033] When a sole comonomer is present, such as n-butyl acrylate, this means that the copolymer contains less than 10% by weight of this comonomer (relative to the total monomers). In the case of the presence of additional comonomers, this means less than 10% by weight of all comonomers in total.
[0034] In general, the comonomer content of the product can be determined by any suitable technique. One suitable technique preferred for the purposes of the present invention is to use 1 H nuclear magnetic resonance (NMR).
[0035] Preferably, the copolymer comprises at least 1 wt% comonomer, such as at least 2 wt% comonomer, and most preferably at least 3 wt% comonomer. Preferably, the copolymer comprises less than 9 wt% comonomer, such as less than 8 wt% comonomer, and more preferably less than 7 wt% comonomer.
[0036] In the preferred embodiment where comonomer (B) is an alkyl (meth)acrylate, preferably the copolymer comprises at least 1 wt% of alkyl (meth)acrylate, such as at least 2 wt% of alkyl (meth)acrylate, and most preferably at least 3 wt% of alkyl (meth)acrylate. Preferably, the copolymer comprises less than 9 wt% of alkyl (meth)acrylate, such as less than 8 wt% of alkyl (meth)acrylate, and more preferably less than 7 wt% of alkyl (meth)acrylate.
[0037] In embodiments, the copolymer may preferably contain 3 to 7 weight percent of the alkyl (meth)acrylate.
[0038] In other embodiments, particularly when the copolymer is prepared by microsuspension polymerization, it may be preferred that the copolymer comprises 4 to 8 weight percent alkyl (meth)acrylate. This range has been found to produce polymers having low gelling temperatures and low viscosities.
[0039] The above ranges for the alkyl (meth)acrylate content apply to the case where the alkyl (meth)acrylate is the sole comonomer or other comonomers are present. (And when two or more alkyl (meth)acrylates are present, these above ranges apply to all alkyl (meth)acrylates present.)
[0040] When comonomer (B) is an alkyl (meth)acrylate, typical additional comonomers (when present) may include a second alkyl (meth)acrylate or another suitable comonomer. Examples of other comonomers that may be used include (meth)acrylic acid, maleic anhydride, vinyl acetate, other monomers containing carboxylate groups (such as diallyl phthalate, allyl methacrylate, and diallyl maleate as discussed further below), acrylamide and derivatives, vinylidene chloride, and allyl and vinyl ethers.
[0041] In some preferred embodiments, two (meth) alkyl acrylates, in particular two alkyl acrylates, may be present in the polymerization. For example, the polymerization may include a mixture of vinyl chloride monomer (A) and at least two (meth) alkyl acrylate comonomers, and preferably two alkyl acrylate comonomers.
[0042] A particularly preferred combination comprises the use of n-butyl acrylate and ethylhexyl acrylate as comonomers.
[0043] In all embodiments where one or more additional comonomers are present in addition to comonomer (B), a particularly preferred class of additional comonomers that may be present comprises crosslinker or chain extender monomers. Such monomers are well known in the art for use as comonomers with vinyl chloride. Preferred examples include diallyl phthalate, allyl methacrylate, diallyl maleate, trimethylolpropane diallyl ether, and tri- or di-ethylene glycol divinyl ether, and the like.
[0044] The weight ratio of A:B added to the polymerization process is greater than 10:1 and is such that the corresponding copolymer contains less than 10 wt% of comonomer. For the avoidance of doubt, the "weight ratio" refers to the total amount of A added to the total amount of B during the polymerization process, per addition.
[0045] A key feature of the present invention is the addition of comonomer (B) at different times throughout the polymerization.
[0046] 1. Continuously for at least 50% of the reaction time, or
[0047] 2. carried out in multiple separate additions with at least 50% of the reaction time separating the initial and final additions, or
[0048] 3. Perform in combination with the above.
[0049] With regard to the use of alkyl (meth)acrylates as comonomers, for example, alkyl (meth)acrylates tend to react faster than vinyl chloride. This is also true for many other comonomers suitable for use as comonomer (B). At least for this reason, and since in all embodiments comonomer (B) is only present at relatively low levels in the final copolymer, the addition of comonomer (B) in multiple stages ensures that the composition of the copolymer is produced more uniformly throughout the polymerization process, giving the product a more uniform structure. Without wishing to be bound by theory, this is also believed to be related to the improved properties obtained.
[0050] (Because of the requirements on when the comonomer is added, the products obtained by the present invention are believed to have a more uniform distribution of comonomer throughout the bulk of the polymer particle, which can be contrasted with products obtained when the comonomer is initially present but not added "later" in the polymerization - where most of the comonomer is then present in the core of the particle, or where the comonomer is added only at a late stage of the polymerization, rather than initially - where the comonomer is then present in the outer layers of the product.)
[0051] As used herein, "reaction time" is the total time measured from initiation of polymerization until (i) steps are taken to stop the reaction and / or (ii) until the reaction pressure decreases due to depletion of the vinyl chloride.
[0052] In particular, in a typical batch emulsion polymerization process, a stirred, temperature-controlled, pressure-resistant reaction vessel (also called an autoclave) is filled with monomer, a dispersion medium (usually water) and stabilizers. It is important to remove oxygen from the autoclave and the reaction medium (as this is a free radical scavenger). Vinyl chloride monomer is immiscible in water and takes the form of vinyl chloride droplets dispersed in the reaction medium and also present as a gas phase above the emulsion. The polymerization reaction temperature is generally in the range of 40-80°C, particularly 45-55°C. (The reaction is exothermic and the temperature is controlled by removing the heat of reaction at the rate at which it is generated). The pressure is generated due to the vapor pressure of the vinyl chloride.
[0053] Typically, such a process can react for several hours, such as 4 to 8 hours, during which time the conversion of the vinyl chloride monomer and other comonomers increases. For most reactions, the reaction pressure is usually fairly uniform, although if monomer or other components are added during the process, small changes, typically "spikes" in pressure, may occur when the monomer or other components are added. At some stage, the vinyl chloride monomer begins to be exhausted in the liquid phase, and the amount of vinyl chloride in the gas phase becomes insufficient to maintain the saturated vapor pressure. This is observed in the reaction curve by the appearance of a steady drop in reactor pressure.
[0054] According to the present invention, and as is commonly used in the art, this pressure drop marks the end of the "reaction time" (unless the reaction is stopped before then, for example by the addition of a terminator or "killer").
[0055] Typical reaction times will depend on the process conditions but will be known to those skilled in the art from prior experience with their particular system / conditions. Typically, the reaction time is between 4 and 8 hours.
[0056] It should be noted that after this time, further copolymerization (of vinyl chloride and comonomer) may still occur, particularly during step (b) of the invention, as will be discussed further. However, for the purposes of the present invention, any such subsequent time is not part of the "reaction time".
[0057] In a preferred first option of the invention, the comonomer is added continuously for at least 50% of the reaction time.
[0058] For the avoidance of doubt, the addition according to this requirement may be stopped or temporarily interrupted, as long as it is added continuously for at least 50% of the total reaction time. For example, in the case of a reaction time of 4 hours, comonomer (B) may be added continuously for the first 60 minutes of the reaction time, stopped for 15 minutes, then added continuously for the next 60 minutes, stopped for another 15 minutes, and then added continuously for a further 60 minutes before stopping for the last 30 minutes (before a pressure drop is observed). The total time of continuous addition in this example is then 3 hours, which is 75% of the 4 hour reaction time. Most preferably, comonomer (B) is added continuously to the process for at least 75% of the reaction time.
[0059] In a second option of the invention, the comonomer (B) is added in multiple additions, and wherein the initial addition and the final addition are separated by at least 50% of the reaction time. Preferably, the initial and final additions are separated by at least 75% of the reaction time. In this option, there may be at least 2 separate additions of the comonomer, preferably at least 3 and more preferably at least 4 separate additions. Each addition may comprise a single (i.e. "one-shot" or "instantaneous") injection, or may comprise additions over a longer period of time, such as 5 to 10 minutes or longer. (In the case of an initial addition and / or a final addition, then reference to an initial addition and a final addition separated by a certain percentage of the reaction time refers to the beginning of the initial addition and / or the end of the final addition.
[0060] In a preferred embodiment, the addition of comonomer (B) starts not later than 1 hour after the start of the reaction time and / or not later than 25% of the reaction time has elapsed.
[0061] (Regarding the option of comonomer (B) addition starting no later than when 25% of the reaction time has elapsed, it can be noted that this requirement is inherently met in the following options, wherein:
[0062] (i) adding comonomer (B) continuously to the process for at least 75% of the reaction time, and
[0063] (ii) the comonomer (B) is added in multiple additions, and the initial addition and the final addition are separated by at least 75% of the reaction time.)
[0064] In absolute terms, it is preferred that the addition of the comonomer (B) starts not later than 30 minutes after the start of the reaction time (ie the start of the reaction), more preferably not later than 10 minutes after the start of the reaction time.
[0065] Additionally or alternatively, it is preferred that the addition of comonomer (B) is started not later than 10% of the reaction time has elapsed, and more preferably not later than 5% of the reaction time has elapsed.
[0066] Most preferably, comonomer B is present at the start of the reaction (whether added continuously or via an initial addition).
[0067] When the comonomer (B) is added in multiple additions, it is preferably added in a single addition which can be relatively evenly distributed throughout the reaction time. For example, in a reaction time of 4 hours and 4 additions, one addition can be made at the beginning of the reaction, and then at about 1 hour, 2 hours, and 3 hours.
[0068] In the third option, a combination of options 1 and 2 can be used. For example, one option belonging to the second option is that the comonomer can be added in multiple additions, where one or more additions are continuous. If the total time of the one or more continuous additions is greater than 50% of the total reaction time, then options 1 and 2 can be satisfied.
[0069] In all options, preferably no comonomer (B) is added during the last 15 minutes of reaction time, and preferably no further monomers are added. In particular, during this period, the reaction is allowed to consume any comonomer (B) remaining in the reaction medium.
[0070] With regard to the vinyl chloride, this may also be added continuously during the polymerization process or in separate additions. However, generally and preferably, the majority of the vinyl chloride to be added, and preferably at least 70% of the vinyl chloride, is present at the start of the reaction. As an example, 80% of the total vinyl chloride may be present at the start of the reaction, and two additions of approximately 10% of the total amount may be made during the reaction time.
[0071] The above additions relate to comonomer (B) and vinyl chloride additions. When additional comonomers are added, they may be added in any suitable manner / in any suitable time frame. Any additional comonomers may be added individually or predominantly, for example, at the beginning of the reaction in a manner similar to vinyl chloride (including before initiation). Alternatively, they may be added continuously or multiple times individually at intervals throughout the reaction time in a manner similar to comonomer (B).
[0072] After the reaction time, the process of the present invention comprises step (b), which comprises:
[0073] i. increasing the temperature of the reaction mixture, and
[0074] ii. Stripping unreacted vinyl chloride over a period of at least 10 minutes.
[0075] Step (b) takes place after the "reaction time". In particular, step (b) in the present invention is considered to start immediately at the end of the reaction time (i.e. the end of the reaction time constitutes the start of step (b)), although it is not essential that step (i) or (ii) itself starts immediately at the start of step (b). Usually and very preferably, no monomer is added to the reaction mixture during step (b).
[0076] In step (i), the temperature of the reaction mixture is raised. Typically, this can be achieved by reducing the cooling applied and allowing the heat from the remaining polymerization taking place to heat the process. However, if necessary, additional heating can be applied. The temperature can be raised by at least 10°C, such as at least 20°C, compared to the temperature at the end of the reaction time. Typically, the temperature can be raised to a temperature of 70-85°C, and preferably 75-80°C, in this step. This can be compared to typical polymerization temperatures of 40-70°C, particularly 45-55°C.
[0077] The temperature is typically increased over a period of at least 10 minutes, such as 15 minutes to 1 hour.
[0078] The increase in temperature serves to increase the conversion of unreacted monomers, particularly vinyl chloride. For vinyl chloride monomer, the conversion after this step is typically over 90%.
[0079] In step (ii), any unreacted vinyl chloride is stripped from the mixture over a period of at least 10 minutes. This step is usually carried out after step (i), and in a preferred embodiment of the invention may be achieved by releasing any residual pressure in the reactor to discharge the contents while maintaining an elevated temperature, particularly at the temperature of step (ii), resulting in evaporation and removal of unreacted vinyl chloride from the emulsion. A vacuum may be applied to assist the removal in this step, and in particular such that the boiling point of the continuous medium (water) is reached.
[0080] The discharged components can be collected for reuse.
[0081] However, in other embodiments, the reactor contents may be discharged from the reactor and transferred to a separate vessel for the stripping step.The external stripping process may then be batch or continuous.
[0082] Stripping is preferably carried out for at least 20 minutes, such as from 20 minutes to 1 hour.
[0083] In a preferred embodiment, step (b) further comprises the step of adding an alkali metal hydroxide to the polymerization medium. Sodium hydroxide is most preferred.
[0084] The alkali metal hydroxide may be added at the beginning of step (b), for example as soon as the reaction time is over. Alternatively, the temperature increase in step (i) may be started first and the alkali metal hydroxide or other compound added during or even at the end of the temperature increase.
[0085] (In other embodiments, the alkali metal hydroxide may be added after step (b), such as before venting or at any time before discharge from the reactor.)
[0086] Step (b) typically takes from 30 minutes to 2 hours in total. Generally, it is desirable to minimize the time of step (b) so that other batch reactions can proceed as quickly as possible, but this must be balanced with the desire to remove residual monomer.
[0087] The stripped vinyl chloride copolymer is then recovered from the process. Typically, the product is recovered from the reactor as a latex of the copolymer and dried, for example, by spray drying as is conventional in the art. The latex may also be dried using any available technique known in the art for drying latexes, including coagulation. After drying, the final product typically contains less than 1 ppm of vinyl chloride monomer and less than 100 ppm of comonomer.
[0088] More generally, the present invention provides a method for preparing a copolymer containing vinyl chloride, which is a batch copolymerization in an emulsion polymerization process. Such processes are well known, and some typical details have been described. Generally, in addition to the requirements of the present invention and as described above, particularly including for adding comonomers during the reaction, the polymerization process can be operated according to any such known batch emulsion polymerization process conditions, including, for example, in any reactor type suitable for such polymerization. Also as has been pointed out, such conditions can include "conventional" emulsion polymerization process conditions, as well as those more commonly referred to as "mini-emulsion" and "micro-suspension" polymerization processes, both of which are well known in the art. Polymerization can, for example, use initiators, stabilizers, buffers and other components that are typically added in such reactions. Examples of suitable conditions and components can be found, for example, in WO 2013092730 Al, WO 2015090657 Al and EP 2960271Al.
[0089] As already indicated, a particularly preferred comonomer (B) for use in the process of the first aspect of the invention is n-butyl acrylate.
[0090] In a second aspect, a vinyl chloride-n-butyl acrylate copolymer is provided, which is preferably prepared according to the method of the first aspect of the present invention.
[0091] In this second aspect, preferred copolymers are preferred to the copolymers in the first aspect, for example with respect to the comonomer content, other comonomers that may be present.
[0092] For example, the copolymer preferably comprises less than 10 wt% n-butyl acrylate, preferably less than 9 wt% n-butyl acrylate, such as less than 8 wt% n-butyl acrylate, and more preferably less than 7 wt% n-butyl acrylate. Preferably, the copolymer comprises at least 1 wt% n-butyl acrylate, such as at least 2 wt% n-butyl acrylate, and most preferably at least 3 wt% n-butyl acrylate, such as at least 4 wt% n-butyl acrylate.
[0093] In embodiments, the copolymer may preferably comprise 3 to 7 weight percent n-butyl acrylate.
[0094] In other embodiments, particularly when the copolymer is prepared by microsuspension polymerization, the copolymer may preferably contain 4 to 8 weight percent n-butyl acrylate. This range has been found to produce polymers having low gelling temperatures and low viscosities.
[0095] In a first embodiment of this second aspect of the invention, the vinyl chloride-n-butyl acrylate copolymer:
[0096] A) has a resistance of 24 Pa.s or less according to ISO 3219 and ISO / TC61 / N4710 at 23°C 1.4s -1 The rheological properties of the plastisols were measured under
[0097] B) has a gel temperature of 76° C. or less, measured as the temperature at which a viscosity of 10,000 Pa.s is reached,
[0098] The plastisol rheology and gel temperature were measured on a plastisol formed by mixing the copolymer with 55 parts per hundred of diisononyl phthalate.
[0099] In particular, the copolymers of this embodiment exhibit an advantageous combination of low plastisol rheology and low gelation temperature. They may also exhibit low Tg (glass transition temperature) and good thermal stability. This embodiment is particularly directed to copolymers prepared by a microsuspension polymerization process, wherein both low gelation temperature and plastisol rheology are desirable. (It should be noted that microsuspension and emulsion grades of vinyl chloride copolymers generally have different properties and are generally used for different applications. This embodiment relates to microsuspension grades due to the requirements for viscosity (plastisol rheology), while emulsion grades will have a viscosity higher than 24 Pa.s (55 phr diisononyl phthalate) under the measurement method described in this embodiment.)
[0100] It is known that the addition of n-butyl acrylate can reduce the gelling temperature compared to the corresponding vinyl chloride homopolymer. However, the addition of n-butyl acrylate can also increase the plastisol rheology, which is undesirable. It has been found that the addition of n-butyl acrylate by the process of the invention leads to an even further reduction in the gelling temperature compared to the addition of n-butyl acrylate at the beginning of the polymerization, but the increase in the plastisol rheology compared to the homopolymer is smaller and in some cases even reduced.
[0101] In this first embodiment, the copolymer may contain at least 3 wt% but less than 15 wt% n-butyl acrylate, for example at least 3 wt% but less than 10 wt% n-butyl acrylate. Preferably, in this first embodiment, the copolymer may contain 4 to 8 wt% n-butyl acrylate.
[0102] Preferably, in this first embodiment, according to ISO 3219 and ISO / TC61 / N4710 at 23°C 1.4s -1 The plastisol rheology measured at 23°C is 23 Pa.s or less, such as 22 Pa.s or less, or 21 Pa.s or less. In some embodiments, according to ISO 3219 and ISO / TC61 / N4710 at 23°C 1.4s -1 The plastisol rheology measured at 20 Pa.s or less, such as 15 Pa.s or less, or even 10 Pa.s or less. Typically, the plastisol rheology is at least 2 Pa.s, such as at least 3 Pa.s.
[0103] Preferably, the gelling temperature, measured as the temperature at which a viscosity of 10,000 Pa.s is reached, is 75°C or lower, such as 74°C or lower or 73°C or lower. In some embodiments, the gelling temperature is 72°C or lower, such as 70°C or lower, such as 65°C or lower or 60°C or lower. Typically, the gelling temperature is at least 50°C.
[0104] (For the avoidance of doubt, both values are still measured on the already defined plastisol formed by mixing the copolymer with 55 parts per hundred of diisononyl phthalate.)
[0105] As will be known to those skilled in the art, plastisol rheology should be measured shortly after mixing with the plasticizer to minimize the effects of aging on the results. In the present invention, the rheology is measured within 1 hour after the copolymer is mixed with diisononyl phthalate. Preferably, the gel temperature is also measured within 1 hour after the copolymer is mixed with diisononyl phthalate.
[0106] In a second embodiment of this second aspect of the invention, the vinyl chloride-n-butyl acrylate copolymer:
[0107] A) 20Pa.s or higher according to ISO 3219 and ISO / TC61 / N4710 at 23°C 1.4s -1 The rheological properties of the plastisols were measured under
[0108] B) has a gel temperature of 76° C. or less, measured as the temperature at which a viscosity of 10,000 Pa.s is reached,
[0109] The plastisol rheology and gel temperature were measured on a plastisol formed by mixing the copolymer with 100 parts per hundred of diisononyl phthalate.
[0110] In particular, the copolymers of this embodiment exhibit an advantageous combination of high plastisol rheology and low gelation temperature. This embodiment is particularly directed to copolymers made by an emulsion polymerization process, where both low gelation temperature and high plastisol rheology are desirable. (It should be noted that the higher viscosity PVC resins are made by emulsion copolymerization rather than microsuspension, so the above measurements are made using higher levels of plasticizer than the equivalent measurements on microsuspension grades in the first embodiment, as is common in the art. Despite the higher plasticizer levels, the plastisol rheology values are higher than those in the first embodiment.)
[0111] As with microsuspension grades, it is known that for emulsion grades, the addition of n-butyl acrylate can reduce the gelling temperature compared to the corresponding vinyl chloride homopolymer. However, when producing emulsion grades, the addition of n-butyl acrylate at the beginning of polymerization can cause a significant reduction in the rheology of the plastisol, which is undesirable in such grades. It has been found that the addition of n-butyl acrylate by the process of the present invention still results in a desirable reduction in the gelling temperature, but the reduction in the plastisol rheology is smaller for a particular reduction in the gelling temperature. This can result in copolymers with similar gelling temperatures and higher plastisol rheologies. (Alternatively, the addition of n-butyl acrylate can be adjusted to provide an optimal balance of gelling temperature and plastisol rheology.)
[0112] In the second embodiment, the copolymer may contain at least 3 wt % but less than 15 wt % n-butyl acrylate, such as at least 3 wt % but less than 10 wt % n-butyl acrylate. Preferably, in the second embodiment, the copolymer contains at least 4 wt % n-butyl acrylate, such as 4 to 8 wt % n-butyl acrylate.
[0113] Preferably, in this second embodiment, according to ISO 3219 and ISO / TC61 / N4710 at 23°C 1.4s -1 The plastisol rheology measured at 23°C is 25 Pa.s or more, such as 30 Pa.s or more, 40 Pa.s or more or even 50 Pa.s or more. According to ISO 3219 and ISO / TC61 / N4710 at 23°C 1.4s -1 The rheology of the plastisol measured under RT is typically 140 Pa.s or less, such as 100 Pa.s or less.
[0114] Preferably, in this second embodiment, the gelling temperature, measured as the temperature at which a viscosity of 10,000 Pa.s is reached, is 75°C or lower, such as 74°C or lower or 73°C or lower. In some embodiments, the gelling temperature is 72°C or lower. Typically, the gelling temperature is at least 50°C. More preferably, the gelling temperature is at least 64°C, such as at least 68°C.
[0115] (For the avoidance of doubt, both are still measured on the already defined plastisol formed by mixing the copolymer with 100 parts per hundred of diisononyl phthalate, and as already described for the first embodiment, the rheology, and preferably the gel temperature, are measured within 1 hour after mixing the copolymer with diisononyl phthalate.)
[0116] The copolymer of the second embodiment, which is typical for emulsion grades, can be formed from primary particles having a particle size distribution having a peak at a diameter of less than or equal to 1.5 microns, and wherein the peak width at half maximum is less than 50% of the particle size at the peak. Typically, the peak of the particle size distribution can be at a diameter of less than or equal to 1 micron, such as less than or equal to 0.5 micron, less than or equal to 0.4 micron, and even less than or equal to 0.2 micron. Typically, the peak of the particle size distribution can be at a diameter of 0.01 micron or greater, such as 0.05 micron or greater.
[0117] (In contrast, the copolymers / microsuspension copolymers according to the first embodiment may have peaks in the particle size distribution at diameters up to 5 microns. They generally have a broadly peaked particle size distribution, i.e. having a peak width at half maximum greater than 50% of the particle size of the peak.)
[0118] It is also found that the copolymer of the second embodiment has improved gloss. In particular, the copolymer of the second embodiment can have a gloss of at least 75 GU (gloss units) measured according to ISO 2813. Preferably, the gloss is at least 80 GU. In some embodiments, the gloss can be at least 85 GU. Typically, the gloss can be as high as 97 GU.
[0119] In preferred embodiments applicable to the first and second embodiments described above, the copolymer may have a glass transition temperature (Tg) as measured by differential scanning calorimetry (DSC) of 80°C or less, such as 79°C or less, or 78°C or less. In some embodiments, the Tg is 75°C or less. Typically, the Tg is at least 64°C, such as at least 68°C, and most preferably at least 70°C.
[0120] Due to their combination of properties, the copolymers prepared by the first aspect of the invention or the copolymers according to the second aspect of the invention are particularly useful in many common PVC applications. This includes use as floor coverings, such as floor coverings and tiles, automotive underbody coatings, adhesive and sealant materials, and artificial leather materials.
[0121] Thus, in a third aspect, there is provided the use of the vinyl chloride-n-butyl acrylate copolymer prepared according to the method of the first aspect and / or the vinyl chloride-n-butyl acrylate copolymer of the second aspect as floor covering material, automobile bottom coating, adhesive and sealant material or artificial leather material.
[0122] In a fourth aspect, a PVC product is provided, comprising a vinyl chloride-n-butyl acrylate copolymer prepared according to the method of the first aspect, and / or a vinyl chloride-n-butyl acrylate copolymer of the second aspect, wherein the PVC product is a flooring material, an automobile bottom coating, an adhesive and sealant material, or an artificial leather material.
[0123] In preferred embodiments of these third and fourth aspects, the copolymer according to the first embodiment of the second aspect of the invention may be used in a portion of a floor covering.
[0124] In another preferred embodiment of these third and fourth aspects, the copolymer according to the second embodiment of the second aspect of the present invention can be used as a part of an automobile undercoat material.
[0125] The invention can be illustrated by the following examples. Example
[0126] Measurement method
[0127] The following methods were used in this example. Unless otherwise stated, when corresponding parameters are found in the claims or general description of the invention, the values of such parameters are then those that would be determined using these methods.
[0128] ■ The primary particle size distribution of the polymer latex was measured by the photoprecipitation method using an apparatus from CPS Instruments Inc. The results are expressed as the size of the top of each peak (μm) and the proportion of each peak (%).
[0129] ■ Using deuterated chloroform (CDCl3) or deuterated tetrahydrofuran (THF-d8) as solvent, the 1 The monomer percentage and acrylate percentage in the polymer were calculated from the H nuclear magnetic resonance (NMR) spectrum.
[0130] ■ The thermal stability was evaluated using the procedure described in ISO 182-3: based on the detection of hydrogen chloride evolved at 180°C and any acidic products. The equipment used was a 763 PVC Thermomat from Metrohm. The measurement was carried out on 0.5 g of PVC resin. The nitrogen flow rate was 7 L / h. The thermal stability time (expressed in minutes) was defined as the time required for the dehydrochlorination reaction at a temperature of 180°C to produce a conductivity of 50 μS / cm in a measuring cell containing ultrapure water.
[0131] ■ Determination of the glass transition temperature by differential scanning calorimetry (DSC). The apparatus used was a Pyris 1 from PerkinElmer, with a nitrogen flow rate of 30 mL / min throughout. The sample (20 mg) was stabilized at -5°C for 5 minutes, then heated to 170°C at 20°C / min, cooled to -5°C at 20°C / min, kept at -5°C for 15 minutes, and then heated to 170°C at 20°C / min. During the second heating, the glass transition was measured according to standard methods.
[0132] ■ Within 1 hour after mixing with 55 or 100 phr of DINP (diisononyl phthalate) to form a plastisol and subsequently at 23°C at 1.4 and 1000 s using a Haake Rheostress 1 rotational rheometer according to ISO 3219 and ISO / TC61 / N4710 -1 The plastisol rheology was measured between 5 and 10 phr. (55 phr was used in Comparative Examples AC and Examples 1-6, and 100 phr was used in Comparative Examples D and E and Examples 7-8.)
[0133] ■ The gelation curves of the plastisols were obtained using an ARES rotational rheometer from TA instrument. The experiment consisted of an oscillating temperature ramp from 25°C to 150°C at 3°C / min at a constant angular frequency of 1 rad / s. The curve obtained shows the complex viscosity vs. temperature. The value reported as an indication of gelation is the temperature at which a viscosity of 10,000 Pa.s is reached.
[0134] • The gloss of the PVC film was measured according to ISO 2813. The gloss was measured on the side of the film not in contact with the release paper substrate. The equipment used was a Dr Lange REFO3 using calibration standard LZM 151 (60° measured gloss of 94.5 GU) and a matte blackboard under the transparent film.
[0135] Comparative Examples AC and Examples 1-6
[0136] These examples illustrate polymerization under microsuspension conditions.
[0137] Comparative Example A
[0138] In this example, vinyl chloride was polymerized under microsuspension conditions in the absence of comonomer.
[0139] Specifically, in a premixer autoclave having a capacity of 15 L and equipped with a stirrer and a double jacket, 2.7 kg of water, 79.9 g of a 298 g / kg aqueous solution of sodium dodecylbenzenesulfonate, 4.15 g of dilauroyl peroxide (99.4%), 5.2 g of dimyristyl peroxydicarbonate (95.4%), 8.9 g of dioctyl adipate (100%) and 0.03 g of butylated hydroxyanisole (100%) were added and mixed together at 50 rpm.
[0140] In a polymerization reactor also having a capacity of 15 L and equipped with a stirrer and a double jacket, 2.7 kg of water, 1.8 g of sodium carbonate (100%), 119.9 g of a 298 g / kg aqueous solution of sodium dodecylbenzene sulfonate and 645.8 g of a 384.1 g / kg aqueous solution of small PVC seeds having a size of 130 nm were added and mixed together at 50 rpm.
[0141] The two reactors were connected together and closed to the atmosphere, a cycle of vacuum and subsequent nitrogen purge was applied, and finally vacuum was applied and the stirring speed of the premixer autoclave and polymerization reactor was increased to 250 rpm and 110 rpm, respectively. Subsequently, 1985 g and 2977 g of vinyl chloride were loaded into the premixer autoclave and polymerization reactor, respectively.
[0142] A stirring step of 30 minutes was maintained to ensure mixing of all raw materials. Subsequently, the premixer autoclave stirring speed was reduced to 50 rpm and the premixer was connected to a 2-stage high pressure homogenizer previously placed under vacuum and the mixture was recirculated for 5 minutes with two-stage pressures at 120 bar and 40 bar before transferring the mixture to the polymerization autoclave.
[0143] Subsequently, to rinse the pre-mixer autoclave and ensure that all reagents were transferred, 1 L of water was added to the pre-mixer autoclave, stirred for 3 minutes and transferred to the polymerization autoclave.
[0144] After the transfer from the premixer autoclave was complete, the reactor temperature was increased to reach a polymerization temperature (T pol Once T is reached pol , which defines the start of polymerization (t0).
[0145] During the polymerization, 2 additional injections of 496 g of vinyl chloride were introduced in the autoclave at t0+2h00 and t0+3h00.
[0146] The reaction was carried out until a pressure drop (-1 bar) was detected. In this specific comparative example, a pressure drop was observed at a reaction time of 7 hours and 48 minutes.
[0147] (It will be noted that under these conditions, pressure drops were generally observed at reaction times exceeding 7 hours, and generally between 7 and about 8 hours. Although reaction times slightly above 8 hours were observed in some examples where n-butyl acrylate was added continuously, this was generally the case in the examples conducted under microsuspension conditions herein. Without wishing to be bound by theory, it is believed that this is due to the presence of small amounts of polymerization inhibitors, which are added to the n-butyl acrylate to maintain storage stability, but which may slow the reaction rate in use. However, in all of Examples 1-6 reported below, the reaction times were in excess of 7 hours, and n-butyl acrylate was added over more than 75% of the reaction time.)
[0148] After the pressure drop has been detected, the temperature of the polymerization medium is raised to 80° C. It can then be evacuated (injection of 3.0 g of a commercial defoamer) and the residual vinyl chloride stripped from the autoclave. After stripping (25 minutes), the autoclave is cooled to room temperature and evacuated.
[0149] The solid content (or latex density) and pH of the latex are measured. The latex is filtered through a sieve with a mesh size of 1 mm. The latex is dried on a spray dryer and the resin obtained is sieved and ground according to standard procedures. For the spray dryer, the inlet temperature is 160°C and the outlet temperature is 60°C. The resin obtained is then ground at maximum intensity (14000 rpm) in a Kolloplex 160Z (pin mill).
[0150] The latex obtained had a pH of 9.1, a solids content of 48% and consisted of particles of 0.75 μm (87.3%) and 0.17 μm (12.7%).
[0151] The resin has a thermal stability of 28.2 minutes. The plastisol rheology shows a η 1.4 of 7.62 Pa.s. From the gel curve, a viscosity of 10 kPa.s is reached at 84.3°C, while DSC shows a Tg of 85.9°C.
[0152] Comparative Example B
[0153] The procedure of Comparative Example A was repeated, except that 300.7 g of n-butyl acrylate was additionally added to the premixer at the beginning of the process (during the first step, before connection to the polymerization reactor). (The vinyl chloride was still added in a staged manner as described in Comparative Example A.)
[0154] The latex obtained had a pH of 8.9, a solids content of 46.6% and consisted of particles of 0.71 μm (88.5%) and 0.16 μm (11.5%).
[0155] The n-butyl acrylate content of the resin was 3.8% by weight.
[0156] The resin has a thermal stability of 16.8 minutes. The plastisol rheology shows a η 1.4 of 24.5 Pa.s. From the gel curve, a viscosity of 10 kPa.s is reached at 76°C, while DSC shows a Tg of 79.6°C.
[0157] Example 1
[0158] The procedure of Comparative Example B was repeated, except that 300.7 g of n-butyl acrylate were continuously introduced into the polymerization reactor instead of the premixer between t0 and t0+7h00.
[0159] The latex obtained had a pH of 8.4, a solids content of 46.4% and consisted of particles of 0.70 μm (88.1%) and 0.16 μm (11.9%).
[0160] The resin has a thermal stability of 22.2 minutes. The plastisol rheology shows a η 1.4 of 14.6 Pa.s. From the gel curve, a viscosity of 10 kPa.s is reached at 71°C, while DSC shows a Tg of 77.9°C.
[0161] These examples show that the addition of n-butyl acrylate in the premixer (Comparative Example B) or continuously (Example 1) leads to a product with a lower gelling temperature (shown by a reduction in the temperature required to reach a viscosity of 10 kPa.s and by a reduction in Tg) compared to PVC homopolymer. However, this is at the expense of an increase in viscosity.
[0162] However, a comparison of Example 1 shows that the continuous addition of n-butyl acrylate according to the invention leads to a further improved (further reduced) gelling temperature and a lower viscosity than the addition at the start of the initial polymerization or before.
[0163] Comparative Example C
[0164] The procedure of Comparative Example B was repeated except that:
[0165] i) 330.8 g of n-butyl acrylate were added to the premixer at the beginning of the process (during the first step, before connection to the polymerization reactor),
[0166] ii) no PVC seeds are added to the polymerization reactor, and
[0167] iii) Use a different homogenizer. In particular, use a colloid mill homogenizer and recirculate the mixture 5 times, operating it at maximum speed.
[0168] The reaction time was slightly shorter than that expected in Comparative Example C, at about 6 1 / 2 hours. (However, as already noted, more than 7 hours is expected as in Examples 2 to 6 below.) Without wishing to be bound by theory, it is believed that in this comparative example, consumption of the inhibitor and reaction of the n-butyl acrylate may have occurred during the heating period so that the polymerization temperature was reached before t0.
[0169] The latex obtained had a pH of 9, a solid content of 49.8% and consisted of particles of 1.50 μm.
[0170] The n-butyl acrylate content of the resin was 4.3% by weight.
[0171] The plastisol rheology showed an η 1.4 of 16.2 Pa.s. From the gel curve, a viscosity of 10 kPa.s was reached at 77.4°C.
[0172] Example 2
[0173] The procedure of Comparative Example C was repeated, except that 330.8 g of n-butyl acrylate were continuously introduced into the polymerization reactor instead of the premixer between t0 and t0+7h00.
[0174] The latex obtained had a pH of 8.6, a solids content of 46.2%, and consisted of particles of 1.57 μm.
[0175] The plastisol rheology showed a η 1.4 of 4.7 Pa.s. From the gel curve, a viscosity of 10 kPa.s was reached at 71°C, while DSC showed a Tg of 75.1°C.
[0176] Comparison of Example 2 with Comparative Example C shows that the continuous addition of n-butyl acrylate according to the invention leads to an improved (lowered) gelling temperature and a lower viscosity (η 1.4) compared to addition at or before the start of the initial polymerization again.
[0177] Examples 3 to 6
[0178] The procedure of Example 2 was repeated, except that increasing amounts of n-butyl acrylate were used (in each case added continuously between t0 and t0+7h00).
[0179] The effect on viscosity is shown below:
[0180]
[0181]
[0182] These examples show that as the n-butyl acrylate content increases, the gelling temperature and Tg decrease further.
[0183] By working according to the invention, these results also continue to show low viscosities (η 1.4), although the viscosity increases again with increasing n-butyl acrylate content.
[0184] Comparative Examples D and E, and Examples 7 and 8
[0185] These examples demonstrate polymerization under emulsion conditions.
[0186] Comparative Example D
[0187] In this example, vinyl chloride was polymerized under emulsion conditions in the absence of comonomer.
[0188] The polymerization was carried out in a polymerization reactor having a capacity of 25 L and equipped with a stirrer and a double jacket.
[0189] 11.99 kg of water, 28.4 mL of a 2 g / L aqueous solution of copper sulfate pentahydrate, 79.3 g of a 110 g / L myristate solution (NaOH / NH4OH ratio) were added to the reactor, which was then closed and the stirrer set to a stirring speed of 50 rpm. Before the final application of vacuum, the reactor was purged of air by a cycle of vacuum and nitrogen purge. The stirring speed was increased to 160 rpm and 7.9 kg of vinyl chloride was charged.
[0190] The temperature was raised using a double jacket to reach a polymerization temperature (T pol Once T is reached pol , 45.1 mL of ammonia at 223 g / L and then 42.6 mL of ammonium persulfate at 100 g / L were introduced 5 minutes later to start polymerization. This constitutes t0 in this example.
[0191] At t0+0h20, a continuous feed of 110 g / L of myristate solution (the same as used at the start) was started. This was added continuously until t0+2h45 minutes after the start, corresponding to a total amount of 1257.9 g of myristate solution. The process was then stopped, and then a continuous introduction of 48 g / kg of an aqueous solution of sodium lauryl sulfate was started and added until t0+4h00. The total amount of the aqueous sodium lauryl sulfate solution added was 1056.3 g.
[0192] In addition, 789 g of vinyl chloride was injected twice at t0+1h30 and t0+2h30.
[0193] Once a pressure drop was detected (approximately 1 bar), 75.8 mL of 40 g / L sodium hydroxide solution was added and the temperature of the reactor was raised to 80°C.
[0194] A pressure drop / reaction time of just over 4 hours was observed, which is typical for reactions under these conditions.
[0195] The reactor was evacuated (4.7 g of commercial defoamer was injected) and unreacted vinyl chloride was stripped over a period of 25 minutes (after adding 2.5 mL of 223 g / L ammonia solution). After stripping, the reactor was cooled to room temperature and 417 mL of 50 g / kg sodium carbonate solution was added.
[0196] The latex was drained and the reactor was cleaned.
[0197] The solid content and pH of the latex were 40.8% and 10.5, respectively. The latex was filtered through a sieve with a mesh size of 1 mm. The latex was dried on a spray dryer, and the resin obtained was sieved and ground according to standard procedures. For the spray dryer, the inlet temperature was 160° C. and the outlet temperature was 70° C.
[0198] DSC showed a Tg of 79.9°C and the resin had a gloss of 69 GU.
[0199] The plastisol rheology showed an η 1.4 of 92 Pa.s and a gelling temperature of 79°C.
[0200] Comparative Example E
[0201] The method of Comparative Example D was repeated except that 489.2 g of n-butyl acrylate and the first amount of vinyl chloride were additionally added at the beginning of the process. (The vinyl chloride was still added in stages as described in Comparative Example D.) The reaction time was 4 hours.
[0202] The solid content and pH of the latex were 36.2% and 12.3, respectively. The latex was filtered, dried and ground as in Comparative Example D.
[0203] The n-butyl acrylate content of the resin was 4.6% by weight.
[0204] DSC showed a Tg of 75.9°C and the resin had a gloss of 85 GU.
[0205] The gelling temperature is 64°C, but the plastisol rheology shows an η 1.4 of only 6.7 Pa.s.
[0206] Example 7
[0207] The procedure of Comparative Example D was repeated, except that 295.5 g of n-butyl acrylate were continuously introduced into the polymerization reactor between t0+0h30 and t0+4h00 (ie initially the myristate solution was introduced first and then the aqueous lauryl sulfate solution was introduced simultaneously). The reaction time was 4 hours and 35 minutes.
[0208] The solid content and pH of the latex were 40.9% and 10.4, respectively.
[0209] The n-butyl acrylate content of the resin was 3.8% by weight.
[0210] DSC showed a Tg of 72.1°C and the resin had a gloss of 89 GU.
[0211] The gelling temperature was 67° C. and the plastisol rheology showed η 1.4 at 20 Pa.s.
[0212] Thus, a similar gelling temperature is obtained, but at a much higher plastisol rheology, compared to Comparative Example D. A lower Tg is also obtained.
[0213] Example 8
[0214] The procedure of Example 7 was repeated, except that 492.9 g of n-butyl acrylate were continuously introduced into the polymerization reactor between t0+0h30 and t0+4h00. The reaction time was 5 hours and 19 minutes.
[0215] The solid content and pH of the latex were 39.0% and 10.3, respectively.
[0216] The n-butyl acrylate content of the resin was 4.9% by weight.
[0217] DSC showed a Tg of 70.5°C and the resin had a gloss of 92 GU.
[0218] The gelling temperature was 63° C. and the plastisol rheology showed an η 1.4 of 52 Pa.s.
[0219] Thus, the process of the invention again yields similar gelling temperatures, but at a much higher plastisol rheology, compared to Comparative Example D. A lower Tg is also again achieved.
[0220] Comparative Example F
[0221] This comparative example is another comparative example provided to show the effect of adding only n-butyl acrylate in the late stages of the polymerization. The polymerization was carried out under microsuspension conditions.
[0222] Specifically, in a premixer autoclave having a capacity of 15 L and equipped with a stirrer and a double jacket, 1.5 kg of water, 112.3 g of a 199.7 g / kg aqueous solution of sodium dodecylbenzenesulfonate, 3.9 g of dilauroyl peroxide, 5.88 g of dimyristyl peroxydicarbonate, 8.4 g of dioctyl adipate and 0.03 g of butylated hydroxyanisole were added and mixed together at 50 rpm.
[0223] In a polymerization reactor with a capacity of 15 L and equipped with a stirrer and a double jacket, 3.5 kg of water, 1.7 g of sodium carbonate and 168.4 g of a 199.7 g / kg aqueous solution of sodium dodecylbenzene sulfonate and 572.7 g of a 407.8 g / kg aqueous dispersion of fine PVC seeds were added and mixed together at 50 rpm.
[0224] The two reactors were connected together and closed to the atmosphere, a cycle of vacuum and subsequent nitrogen purge was applied, and finally vacuum was applied and the stirring speed of the premixer autoclave and polymerization reactor was increased to 250 rpm and 110 rpm, respectively. Subsequently, 2043.5 g and 3065.2 g of vinyl chloride were loaded into the premixer autoclave and polymerization reactor, respectively.
[0225] A stirring step of 30 minutes was maintained to ensure mixing of all raw materials. Subsequently, the premixer autoclave stirring speed was reduced to 50 rpm, and the premixer was connected to a 2-stage high pressure homogenizer previously placed under vacuum, and the mixture was recirculated for 5 minutes with a two-stage pressure at 120 bar and 40 bar, and then the mixture was transferred to the polymerization autoclave.
[0226] Subsequently, to rinse the pre-mixer autoclave and ensure that all reagents were transferred, 1 L of water was added to the pre-mixer autoclave, stirred for 3 minutes and transferred to the polymerization autoclave.
[0227] After the transfer from the premixer autoclave was completed, the polymerization autoclave temperature was increased by double jacketing to reach a polymerization temperature (T pol Once T is reached pol , which defines the start of polymerization (t0).
[0228] From previous experiments under these conditions, it was estimated that 50% conversion of vinyl chloride occurs in about 5 hours. Thus, in this experiment, the addition of n-butyl acrylate was started 5 hours after initiation. More specifically, 312.5 g of n-butyl acrylate (purity 997.5 g / kg) were introduced continuously between t0+5h00 and t0+7h00. Two injections of 465 g of vinyl chloride were introduced in the autoclave at t0+2h00 and t0+3h00.
[0229] After 8 hours, the temperature of the polymerization medium was raised to 80° C. It was then possible to evacuate (inject 2.8 g of a commercial defoamer) and strip the autoclave of residual vinyl chloride. After stripping (25 minutes), the autoclave was cooled to room temperature and evacuated.
[0230] The solid content (or latex density) and pH of the latex are measured. The latex is filtered through a sieve with a mesh size of 1 mm. The latex is dried on a spray dryer and the resin obtained is sieved and ground according to standard procedures. For the spray dryer, the inlet temperature is 160°C and the outlet temperature is 60°C. The resin obtained is then ground at 14000 rpm in a Kolloplex 160Z (pin mill).
[0231] The latex had a pH of 11.1, a mechanical stability of more than 10 minutes and a solids content of 43.2%, consisting of particles of 0.54 μm (75.2%) and 0.18 μm (24.8%).
[0232] The resin has a thermal stability of 26.4 minutes, and the rheology of 55 phr DINP plastisol shows an η 1.4 of 367 Pa.s. From the gel curve, a viscosity of 10 kPa.s is reached at 76.0°C, and DSC shows a Tg of 82.6°C.
[0233] The n-butyl acrylate content of the resin was 3.9% by weight.
[0234] As can be seen above, the "post-addition" of n-butyl acrylate results in a product with a very high viscosity (η 1.4) and generally a higher gelling temperature and Tg (° C.).
Claims
1. A method for preparing a copolymer containing vinyl chloride, the method comprising: a. batch copolymerization in an emulsion polymerization process comprising a mixture of vinyl chloride monomer (A) and a comonomer (B), wherein: i. the weight ratio of A:B added to the polymerization process is greater than 10:1, and the corresponding copolymer contains less than 10% by weight of comonomer, ii. Addition of comonomer (B) 1. Continuously for at least 50% of the reaction time, or 2. carried out in multiple additions with at least 50% of the reaction time separating the initial and final additions, or 3. Perform the above combination, b. After the reaction time, i. raising the temperature of the reaction mixture and ii. stripping unreacted vinyl chloride over a period of at least 10 minutes, and c. Recovering copolymers containing vinyl chloride.
2. The process according to claim 1, wherein the addition of comonomer (B) is started not later than 1 hour after the start of the reaction time and / or not later than when 25% of the reaction time has elapsed.
3. The method according to claim 1 or claim 2, wherein the comonomer (B) is an alkyl (meth)acrylate.
4. The method according to claim 3, wherein the comonomer (B) is n-butyl acrylate.
5. The process according to any one of the preceding claims, wherein the copolymer comprises 3 to 10 wt% of comonomer (B).
6. A process according to any one of the preceding claims, wherein comonomer (B) is added continuously to the process over at least 50% of the reaction time.
7. A vinyl chloride-n-butyl acrylate copolymer, That: A) has a resistance of 24 Pa.s or less according to ISO 3219 and ISO / TC61 / N4710 at 23°C 1.4s -1 The rheological properties of the plastisols were measured under B) has a gel temperature of 76° C. or less, measured as the temperature at which a viscosity of 10,000 Pa.s is reached, The plastisol rheology and gel temperature were measured on a plastisol formed by mixing the copolymer with 55 parts per hundred of diisononyl phthalate.
8. The copolymer according to claim 7, wherein the -1 The plastisol rheology measured under 370°C is 23 Pa.s or less, such as 22 Pa.s or less, or 21 Pa.s or less.
9. A copolymer according to claim 7 or claim 8, wherein the gelling temperature measured as the temperature at which a viscosity of 10,000 Pa.s is reached is 74°C or less, such as 72°C or less.
10. Vinyl chloride-n-butyl acrylate copolymer, That: A) With 20Pa.s or higher according to ISO 3219 and ISO / TC61 / N4710 at 23℃1.4s -1 The rheological properties of the plastisols were measured under B) has a gel temperature of 76° C. or less, measured as the temperature at which a viscosity of 10,000 Pa.s is reached, The plastisol rheology and gel temperature were measured on a plastisol formed by mixing the copolymer with 100 parts per hundred of diisononyl phthalate.
11. The copolymer according to claim 10, wherein the -1 The plastisol has a rheology of 25 Pa.s or more, such as 30 Pa.s or more, 40 Pa.s or more or even 50 Pa.s or more, measured under 0.1% rheology.
12. A copolymer according to claim 10 or claim 11, wherein the gelling temperature, measured as the temperature at which a viscosity of 10,000 Pa.s is reached, is 74°C or less, such as 72°C or less.
13. The copolymer according to any one of claims 10 to 12, wherein the copolymer has a gloss measured according to ISO 2813 of at least 75 GU (Gloss Units), preferably at least 80 GU.
14. The copolymer according to any one of claims 7 to 13, wherein the copolymer has a Tg (glass transition temperature) glass transition temperature measured by differential scanning calorimetry (DSC) of 80°C or less, such as 78°C or less, or 75°C or less.
15. The copolymer according to any one of claims 7 to 14, wherein the copolymer comprises at least 3 wt% but less than 15 wt% n-butyl acrylate.
16. The copolymer of claim 15, wherein the copolymer comprises at least 3 wt% but less than 15 wt% n-butyl acrylate.
17. Use of a vinyl chloride-n-butyl acrylate copolymer obtained by the process according to any one of claims 1 to 6, and preferably a vinyl chloride-n-butyl acrylate copolymer according to any one of claims 7 to 16 as a floor covering material, an automobile undercoat material, an adhesive and sealant material or an artificial leather material.
18. A PVC product comprising a vinyl chloride-n-butyl acrylate copolymer prepared according to the process of any one of claims 1 to 6, and preferably a vinyl chloride-n-butyl acrylate copolymer according to any one of claims 7 to 16, the PVC product being a floor covering material, an automobile undercoat, an adhesive and sealant material or an artificial leather material.