Epoxy resin composition for sealing and electronic device
By using amidine silicate as a curing accelerator in the sealing epoxy resin composition, the problem of both storage stability and curing speed is solved, and the effect of high storage stability and rapid curing is achieved. It is suitable for sealing of electronic devices. part.
Patent Information
- Application Number
- CN202380028791.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-05
AI Technical Summary
The existing sealing epoxy resin compositions are difficult to take into account both the storage stability and the curing speed, and improving the storage stability usually leads to a reduction in the curing speed.
An epoxy resin composition containing amidine silicate as a curing accelerator is used. Amidine silicate consists of amidine cation and silicate anion, which has high alkalinity and high melting point, can maintain low activity at room temperature but is significant during heating. Improve and promote effective curing of epoxy resin.
It realizes the sealing components of electronic devices while maintaining high storage stability while increasing the curing speed.
Smart Images

Figure CN118900868A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure generally relates to an epoxy resin composition for sealing and an electronic device. More specifically, the present disclosure relates to an epoxy resin composition for sealing and an electronic device including a sealing portion made of the epoxy resin composition for sealing. Background Art
[0002] Patent document 1 discloses a sealing epoxy resin composition, which includes an epoxy resin (A), a phenolic resin curing agent (B), an inorganic filler (C) and a curing accelerator (D). According to Patent document 1, the curing accelerator (D) has an average particle size of 10 μm or less and may contain at least one compound selected from the group consisting of a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, and an adduct of a phosphonium compound and a silane compound (see paragraph 0032 of Patent document 1).
[0003] Citation List
[0004] Patent Literature
[0005] Patent Document 1: WO 2012 / 102336 A1 Summary of the invention
[0006] An object of the present disclosure is to provide an epoxy resin composition for sealing and an electronic device which has high storage stability and can increase the curing speed during curing.
[0007] The epoxy resin composition for sealing according to one aspect of the present disclosure contains an epoxy resin (A), a curing agent (B), a curing accelerator (C) and an inorganic filler (D). The curing accelerator (C) contains an amidine silicate (C1) represented by the following formula (1):
[0008]
[0009] In formula (1), R1 and R2 are each independently a hydrogen atom or an aliphatic hydrocarbon group having 1 or more and 5 or less carbon atoms, R3 and R4 are each independently a phenylene group or a naphthylene group, and R5 is at least one group selected from the group consisting of a phenyl group, a functional group represented by the following formula (2) and a functional group represented by the following formula (3):
[0010] -C n H 2n -X…(2)
[0011] In formula (2), n is 3 or more and 8 or less, X is at least one functional group selected from the group consisting of -SH, -NH, -NH-Ph, -Ph-CH=CH2, -NH-C2H4-NH2, -N=C=O, a glycidyl ether group, and a group represented by the following formula (3),
[0012]
[0013] According to another aspect of the present disclosure, an electronic device includes a semiconductor element and a sealing portion that seals the semiconductor element. The sealing portion is a cured product of the above-mentioned epoxy resin composition for sealing. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is a schematic cross-sectional view illustrating an electronic device according to an exemplary embodiment of the present disclosure. DETAILED DESCRIPTION
[0015] 1. Summary
[0016] First, it will be described how the inventors conceived the concept of the present disclosure.
[0017] As described above, Patent Document 1 (WO 2012 / 102336 A1) discloses a sealing epoxy resin composition comprising an epoxy resin (A), a phenolic resin-based curing agent (B), an inorganic filler (C), and a curing accelerator (D).
[0018] The present inventors have found through their unique research that preparing a sealing resin composition by mixing an epoxy resin, a curing agent and a curing accelerator as in Patent Document 1 sometimes results in a decrease in the storage stability of the resin composition. In addition, the present inventors have also found that attempts to improve the storage stability of the resin composition sometimes result in a decrease in the curing speed during curing. Therefore, in order to overcome such problems, the present inventors have conducted extensive research and ultimately conceived the concept of a sealing epoxy resin composition according to the present disclosure.
[0019] The epoxy resin composition for sealing according to the exemplary embodiment contains an epoxy resin (A), a curing agent (B), a curing accelerator (C) and an inorganic filler (D). The curing accelerator (C) contains amidine silicate (C1) represented by the following formula (1):
[0020]
[0021] The epoxy resin composition for sealing is curable by the reaction between the epoxy resin (A) and the curing agent (B). Adding a curing accelerator (C) to the epoxy resin composition for sealing allows the reaction to proceed even more efficiently. The inorganic filler (D) can adjust the physical properties of the sealing portion made from the epoxy resin composition for sealing, such as heat resistance, thermal conductivity and linear expansion coefficient.
[0022] Meanwhile, if the prepared epoxy resin composition for sealing is placed, the reaction will be carried out even at room temperature, for example, due to the improved reactivity of the epoxy resin composition for sealing as described above, it is difficult to store the prepared epoxy resin composition for sealing. That is, in this case, it will be difficult to maintain the high storage stability of the epoxy resin composition for sealing. In contrast, in the epoxy resin composition for sealing according to the present embodiment, the curing accelerator (C) contains amidine silicate (C1) represented by formula (1), so it is possible to improve the storage stability of the epoxy resin composition for sealing without causing the curability of the epoxy resin composition for sealing to be reduced while heating and curing the epoxy resin composition for sealing.
[0023] The reason why the high storage stability and high curing speed when curing are achieved according to the above-mentioned configuration of the present embodiment is not completely clear, but may be as follows. The amidine silicate (C1) contained in the curing accelerator (C) is a curing accelerator consisting essentially of amidine cations and silicate anions. The amidine cations have relatively high alkalinity and can have high activity, while the silicate anions have a skeleton derived from dihydroxynaphthalene or catechol, and therefore tend to have a high melting point. This is why amidine silicate (C1) tends to keep its activity sufficiently low under temperature conditions such as room temperature, but tends to improve its activity more and more significantly as the temperature rises. When heated to a temperature near its melting point, the activity of amidine silicate (C1) can be particularly significantly improved. Therefore, amidine silicate (C1) will more easily improve the storage stability of the epoxy resin composition for sealing, and will have enough activity to fully improve the curing speed of the epoxy resin composition for sealing while heating and curing the epoxy resin composition for sealing.
[0024] It can be seen that the present embodiment can provide a sealing epoxy resin composition having high storage stability and the ability to increase the curing speed during curing. Therefore, the sealing epoxy resin composition according to the present embodiment can be used to seal electronic components such as semiconductor elements in electronic devices.
[0025] 2. Details
[0026] Next, the epoxy resin composition for sealing and the electronic device 1 according to the present embodiment will be described in further detail. Note that the exemplary embodiment described below is only an exemplary one of the various embodiments of the present disclosure and should not be interpreted as limiting. In addition, the exemplary embodiment can be easily modified in various ways according to design selection or any other factors without departing from the scope of the present disclosure.
[0027] <Epoxy resin composition for sealing>
[0028] First, each component contained in the sealing epoxy resin composition will be described in detail. The sealing epoxy resin composition according to the present embodiment contains the epoxy resin (A), the curing agent (B), the curing accelerator (C), and the inorganic filler (D) as described above.
[0029] [Epoxy resin]
[0030] Epoxy resin (A) is a thermosetting component. In this embodiment, epoxy resin (A) and curing agent (B) in the epoxy resin composition for sealing can be reacted and cured. Epoxy resin (A) can impart heat resistance to the cured product of the epoxy resin composition for sealing.
[0031] The epoxy resin (A) contains at least one component selected from the group consisting of, for example, glycidyl ether epoxy resins, glycidyl amine epoxy resins, glycidyl ester epoxy resins, and oxidized olefin (alicyclic) epoxy resins. More specifically, the epoxy resin includes one or more components selected from the group consisting of, for example, alkyl-phenol-novolac epoxy resins, such as phenol-novolac epoxy resins and cresol-novolac epoxy resins; naphthol-novolac epoxy resins; phenol-aralkyl epoxy resins having, for example, a phenylene skeleton or a biphenylene skeleton; biphenyl-aralkyl epoxy resins; naphthol-aralkyl epoxy resins having, for example, a phenylene skeleton or a biphenylene skeleton; multifunctional epoxy resins, such as trisphenol-methane epoxy resins and alkyl-modified trisphenol-methane epoxy resins; triphenyl-methane epoxy resins; tetrakisphenol ethane type epoxy resin; dicyclopentadiene type epoxy resin; stilbene type epoxy resin; bisphenol type epoxy resin, such as bisphenol A type epoxy resin and bisphenol F type epoxy resin; biphenyl type epoxy resin; naphthalene type epoxy resin; alicyclic epoxy resin; bromine-containing epoxy resin, such as bisphenol A type brominated epoxy resin; glycidylamine type epoxy resin obtained by the reaction between epichlorohydrin and polyamines such as diaminodiphenylmethane and isocyanuric acid; and glycidylester type epoxy resin obtained by the reaction between polybasic acids such as phthalic acid and dimer acid and epichlorohydrin.
[0032] Note that these are only exemplary components that may be included in the epoxy resin (A) of the epoxy resin composition for sealing, and should not be construed as limiting. Alternatively, the epoxy resin (A) of the epoxy resin composition for sealing may also contain any other resin having an epoxy group. The resin having an epoxy group may be a monomer or a prepolymer, whichever is suitable.
[0033] [Curing agent]
[0034] As described above, the curing agent (B) is a compound that can react with the epoxy resin (A) in the sealing epoxy resin composition.
[0035] The curing agent (B) may contain, for example, a phenol compound. Adding the phenol compound to the curing agent (B) allows the epoxy resin (A) and the curing agent (B) to undergo a thermal curing reaction.
[0036] The phenol compound preferably includes at least one component selected from the group consisting of: for example, novolac type resins, such as phenol-novolac resins, cresol-novolac resins and naphthol-novolac resins; phenol-aralkyl resins having a phenylene skeleton or a biphenylene skeleton; aralkyl type resins, such as naphthol aralkyl resins having a phenylene skeleton or a biphenylene skeleton; polyfunctional phenolic resins, such as trisphenol methane type resins; dicyclopentadiene type phenolic resins, such as dicyclopentadiene type phenol-novolac resins and dicyclopentadiene type naphthol-novolac resins; terpene-modified phenolic resins; bisphenol type resins, such as bisphenol A and bisphenol F resins; and triazine-modified novolac resins.
[0037] Note that as long as the curing agent (B) can undergo a heat curing reaction with the epoxy resin (A), the curing agent (B) does not have to be a phenol compound. For example, the curing agent (B) may contain at least one component selected from the group consisting of a phenol compound, an acid anhydride, an imidazole compound, and an amine compound.
[0038] The equivalent of epoxy resin (A) is preferably 0.6 eq. or more and 10 eq. or less per equivalent of curing agent (B). Setting the equivalent of epoxy resin (A) to a value of 10 eq. or less allows the epoxy resin composition for sealing to have good curability, and also allows its cured product to have sufficient heat resistance and mechanical strength. Setting the equivalent of epoxy resin (A) to a value of 0.6 eq. or more allows the cured product to have high moisture resistance. The equivalent of epoxy resin (A) is more preferably 0.8 eq. or more and 5 eq. or less per equivalent of curing agent (B).
[0039] [Curing accelerator]
[0040] The curing accelerator (C) is a compound that can promote the curing reaction between the epoxy resin (A) and the curing agent (B) in the epoxy resin composition for sealing. In this embodiment, the curing accelerator (C) contains an amidine silicate (C1) represented by the following formula (1):
[0041]
[0042] (Amidine silicate)
[0043] The amidine silicate (C1) comprises a cationic part with an amidine skeleton and an anionic part with a silicate skeleton. In the present embodiment, as represented by formula (1), the cationic part has an imidazolium skeleton, and the anionic part has a silicate anion. The amidine silicate (C1) can contribute to improving the storage stability of the epoxy resin composition for sealing and improving the curing speed during curing. In addition, the amidine silicate (C1) has excellent compatibility with epoxy resin (A) and curing agent (B). Therefore, even when preparing the epoxy resin composition for sealing, the amidine silicate (C1) is not easy to agglomerate, which can improve the dispersibility of the epoxy resin composition for sealing in the molten state.
[0044] The amidine silicate (C1) has a relatively high melting point. This makes it easier to prepare the epoxy resin composition for sealing in solid form at room temperature (such as room temperature of about 25°C), thereby improving the storage stability of the epoxy resin composition for sealing. If the cationic part has high alkalinity, the activity tends to be high. In contrast, the amidine silicate (C1) according to the present embodiment has a high melting point and is in solid form at room temperature, so that the possibility of increasing the activity of the epoxy resin composition for sealing during storage is reduced, and the storage stability is not reduced. In addition, when the epoxy resin composition for sealing is heated and cured, the amidine silicate (C1) is activated to be sufficient to cure the epoxy resin composition for sealing in a relatively short time. The melting point of the amidine silicate (C1) is preferably above 160°C, more preferably above 180°C, and even more preferably above 200°C. The upper limit of the melting point of the amidine silicate (C1) can be, for example, below 300°C, but is not limited thereto.
[0045] In the formula (1) representing amidine silicate (C1), R1 and R2 are each independently a hydrogen atom or an aliphatic hydrocarbon group having more than 1 and less than 5 carbon atoms. R1 and R2 are preferably each independently an aliphatic hydrocarbon group having more than 1 and less than 20 carbon atoms, more preferably each independently an aliphatic hydrocarbon group having more than 1 and less than 10 carbon atoms. This allows the cationic part to maintain appropriate alkalinity without increasing its alkalinity too much, thereby reducing the possibility of causing the fluidity of the epoxy resin composition for sealing in a molten state to decrease. Optionally, amidine silicate (C1) may contain a variety of compounds represented by formula (1). For example, amidine silicate (C1) may contain a plurality of compounds in which only R1 is different from each other in formula (1), or a plurality of compounds in which only R2 is different from each other in formula (1), or a plurality of compounds in which both R1 and R2 are different from each other.
[0046] In the formula (1) representing the amidine silicate (C1), R3 and R4 are each independently a phenylene group or a naphthylene group, and R5 is at least one group selected from the group consisting of a phenyl group and a group represented by the following formula (2). Optionally, the amidine silicate (C1) may contain a plurality of compounds represented by the formula (1). For example, the amidine silicate (C1) may contain a plurality of compounds in which only R3 in the formula (1) is different from each other, or a plurality of compounds in which only R4 in the formula (1) is different from each other, or a plurality of compounds in which both R3 and R4 are different from each other.
[0047] -C n H 2n -X…(2)
[0048] In the formula (2) representing the amidine silicate (C1), X is at least one functional group selected from the group consisting of -SH, -NH, -NH-Ph, -Ph-CH=CH2, -NH-C2H4-NH2, -N=C=O, a glycidyl ether group, and a group represented by the following formula (3):
[0049]
[0050] In formula (1), R5 is a side chain group having an ethylene chain bonded to a silicon atom. If X in formula (2) is selected from at least one group consisting of -SH, -NH, -NH-Ph, -Ph-CH=CH2, -NH-C2H4-NH2, -N=C=O, a glycidyl ether group, and a group represented by formula (3), then an amidine silicate (C1) with a high melting point can be easily obtained. This is because at least one of these groups is selected as X, and due to the presence of a phenylene or naphthylene group bonded to a silicon atom via an oxygen atom, the possibility of increasing and decreasing the melting point of the amidine silicate (C1) is reduced, and the possibility of affecting crystallinity is reduced. As used herein, "-Ph" in "-NH-Ph" refers to a phenyl group, and "-Ph-" in "-Ph-CH=CH2" refers to a phenylene group.
[0051] In the formula (1) representing the amidine silicate (C1), R1 and R2 are preferably each independently a hydrocarbon group having 1 or 2 carbon atoms, and R5 is preferably a phenyl group or C3H6SH. This can further improve the storage stability of the sealing epoxy resin composition and achieve even higher curability when the sealing epoxy resin composition is cured.
[0052] The amidine silicate (C1) preferably includes at least one compound selected from the group consisting of compounds represented by the following formulae (11), (12) and (13). This can further improve the storage stability of the sealing epoxy resin composition and achieve even higher curability when the sealing epoxy resin composition is cured.
[0053]
[0054]
[0055] Note that the compounds represented by these formulae (11) to (13) can be synthesized by the method disclosed in JP 6917707 B2.
[0056] In the epoxy resin composition for sealing, relative to the total of 100 parts by mass of epoxy resin (A) and curing agent (B), the ratio of curing accelerator (C) is preferably more than 1 part by mass and less than 35 parts by mass. The ratio of curing accelerator (C) is set to a value of more than 1 part by mass, so that it is even easier to improve the curing speed of the epoxy resin composition for sealing when curing. The ratio of curing accelerator (C) is set to a value of less than 35 parts by mass, so that the epoxy resin composition for sealing is easier to maintain even higher storage stability. Relative to the total of 100 parts by mass of epoxy resin (A) and curing agent (B), the ratio of curing accelerator (C) is more preferably more than 3 parts by mass and less than 25 parts by mass, and even more preferably more than 3 parts by mass and less than 20 parts by mass.
[0057] Relative to the total of 100 parts by mass of epoxy resin (A) and curing agent (B), the proportion of amidine silicate (C1) is preferably more than 1 part by mass and less than 35 parts by mass. The proportion of amidine silicate (C1) is set to a value of more than 1 part by mass, so that it is even easier to increase the curing speed of the epoxy resin composition for sealing when curing. The proportion of amidine silicate (C1) is set to a value of less than 35 parts by mass, so that the epoxy resin composition for sealing is easier to maintain even higher storage stability. Relative to the total of 100 parts by mass of epoxy resin (A) and curing agent (B), the proportion of amidine silicate (C1) is more preferably more than 3 parts by mass and less than 25 parts by mass, and even more preferably more than 3 parts by mass and less than 20 parts by mass.
[0058] [Inorganic filler (D)]
[0059] The sealing epoxy resin composition contains an inorganic filler (D). The inorganic filler (D) can improve the heat resistance and thermal conductivity of the sealing portion 4. In addition, the inorganic filler (B) can also reduce the linear expansion coefficient of the sealing portion 4.
[0060] The average particle size of the inorganic filler (D) is preferably 0.5 μm or more and 15 μm or less. This makes it easier for the epoxy resin composition for sealing to maintain sufficient fluidity without causing reduced fluidity. Note that the average particle size of the inorganic filler (D) according to the present disclosure refers to the median diameter (D50) on a volume basis. The median diameter (D50) can be calculated based on the particle size distribution measured by a laser diffraction scattering method. For example, a laser diffraction particle size analyzer can be used to measure the particle size distribution. As a laser diffraction particle size analyzer, for example, "MT3300EX2" manufactured by MicrotracBEL Corporation can be used.
[0061] The inorganic filler (D) preferably includes inorganic particles each having a particle size of 0.1 μm or less. Relative to 100 parts by weight of the inorganic filler (D), the proportion of the inorganic particles is preferably 0.1 parts by weight or more and 30 parts by weight or less. This makes it easier for the epoxy resin composition for sealing to maintain even higher fluidity in a molten state. The lower limit of the particle size of the inorganic particles is not limited to any specific value. According to the present disclosure, the proportion of such inorganic particles each having a particle size of 0.1 μm or less can be detected by measuring the frequency distribution of the particle size of 0.1 μm or less using a laser diffraction particle size analyzer that can be the same as the above-mentioned particle size analyzer.
[0062] As the inorganic filler (D), any suitable material can be used without limitation as long as the purpose of the present disclosure can be achieved. For example, the inorganic filler (D) can contain at least one component selected from the group consisting of fused silica such as fused spherical silica, crystalline silica, alumina, aluminum nitride, and silicon nitride.
[0063] In the epoxy resin composition for sealing, relative to the total amount of epoxy resin (A), curing agent (B), curing accelerator (C) and inorganic filler (D), the ratio of inorganic filler (D) is preferably 60 mass % or more and 93 mass % or less. The ratio of inorganic filler (D) is set to a value of more than 60 mass %, so that the epoxy resin composition for sealing is even easier to maintain the fluidity in a sufficient molten state. The ratio of inorganic filler (D) is set to a value of less than 93 mass %, so that it is easier to ensure the sufficient filling property of the epoxy resin composition for sealing. Relative to the total amount of epoxy resin (A), curing agent (B), curing accelerator (C) and inorganic filler (D), the ratio of inorganic filler (D) is more preferably 60 mass % or more and 90 mass % or less, and even more preferably 65 mass % or more and 90 mass % or less.
[0064] [Other components]
[0065] The epoxy resin composition for sealing may further contain any appropriate compounds, resins, additives and other components in addition to the above-mentioned essential components. Examples of such additives include appropriate defoamers, surface conditioners, coupling agents, fluxing agents, viscosity modifiers, leveling agents, low stress agents and pigments.
[0066] The epoxy resin composition for sealing preferably contains no organic solvent or has an organic solvent content of 0.5 mass % or less.
[0067] <Method for producing epoxy resin composition for sealing>
[0068] Sealed epoxy resin composition can be manufactured, for example, in the following manner. By simultaneously or sequentially mixing the components that can be included in the above-mentioned epoxy resin composition for sealing with the appropriate additive compounding added thereto as needed to prepare the mixture. In this case, for example, a mixer or agitator can be used to mix the constituent components to sufficient homogenization, then kneading and heating with a kneading machine such as a hot roller or a kneading machine, and then cooling to room temperature. Specifically, by kneading epoxy resin (A) and curing accelerator (C) with each other, then mixing with curing agent (B) and inorganic filler (D) to prepare a kneaded product. In order to stir the mixture, as needed, for example, a disperser, a planetary mixer, a ball mill, a three-roll mill, a bead mill and any other agitator can be appropriately used in combination. Alternatively, if the inorganic filler (D) contains a variety of materials with different average particle diameters, it is also possible to prepare a mixture of inorganic fillers in which a variety of materials with different average particle diameters are mixed together before the inorganic filler (D) is added to the kneaded product, measure its average particle diameter, and then add the mixture of inorganic fillers to the kneaded product to prepare the sealed epoxy resin composition.
[0069] When heat treatment is performed, the heating temperature and heating time can be appropriately adjusted. In this case, the heating temperature is preferably a temperature at which, for example, the epoxy resin composition for sealing begins to flow and is lower than the temperature at which the epoxy resin (A) and the curing agent (B) begin to react with each other. Specifically, the heating temperature is preferably a temperature of 90°C or more and 140°C or less. In addition, the cooling method is not limited to any particular method and can be appropriately set. The present embodiment allows obtaining a sealing epoxy resin composition in solid form at 25°C.
[0070] Optionally, the epoxy resin composition for sealing can be manufactured by pulverizing the epoxy resin composition for sealing prepared by the above method. Optionally, the epoxy resin composition for sealing can be manufactured by pressing the epoxy resin composition for sealing in a sheet form. Still optionally, the epoxy resin composition for sealing can also have any other suitable shape.
[0071] The epoxy resin composition for sealing can be cured by heating the epoxy resin composition for sealing to a temperature at which the epoxy resin composition for sealing begins to solidify. This allows the cured product of the epoxy resin composition for sealing to be obtained. In the present embodiment, in particular, the epoxy resin composition for sealing has a high curing speed and excellent curability. The heat treatment conditions for the purpose of curing such as heating temperature, heating time and maximum heating temperature can be appropriately adjusted according to the characteristics of the type of epoxy resin (A), the type of curing agent (B), the type of curing accelerator (C) and various components.
[0072] <Physical Properties of Sealing Epoxy Resin Composition>
[0073] Next, preferred physical properties of the epoxy resin composition for sealing according to the present embodiment will be described.
[0074] The sealing epoxy resin composition preferably has a solid form at 25° C. This allows the sealing epoxy resin composition to be prepared at room temperature (about 25° C.) and has excellent storage stability, thereby reducing the possibility of causing any changes in the chemical composition of the prepared sealing epoxy resin composition, thereby making the sealing epoxy resin composition easy to handle. In addition, when a cured product is made from the sealing epoxy resin composition, the sealing portion 4 can be formed by heating and melting the sealing epoxy resin composition that has been prepared and stored.
[0075] In the epoxy resin composition for sealing, when measured under conditions including a temperature of 170°C, the time required for 1.67ml of the epoxy resin composition for sealing to reach a torque value of 0.1kgf·cm is preferably 30 seconds or more and 100 seconds or less. Specifically, the torque value can be measured by using a tester such as Curelastometer 7P manufactured by JSR Corporation, setting the upper and lower surface temperatures of the mold of the tester to 170°C and injecting 1.67ml of the sample. In the following description, "the time required for 1.67ml of the sample to reach a torque value of 0.1kgf·cm when measured under conditions including a temperature of 170°C" will be referred to as "gel time" hereinafter. Although 1.67ml of the epoxy resin composition for sealing is used as a sample for measurement to measure the torque value and the gel time, this should not be interpreted as limiting the amount of the epoxy resin composition for sealing that forms the cured product according to the present disclosure. The gel time is set to a value of 30 seconds or more, so that when the sealing portion 4 is made of the epoxy resin composition for sealing, it is easier to maintain sufficient fluidity. Setting the gel time to a value of 100 seconds or less makes it easier for the encapsulated epoxy resin composition to maintain a sufficiently high curing speed. The gel time is more preferably 40 seconds or more and 70 seconds or less.
[0076] In the epoxy resin composition for sealing, when the torque value of 1.67 ml of the epoxy resin composition for sealing is measured under conditions including a temperature of 170° C., the torque value is given by T n / T 300s The time required for the curing rate given by ×100 to become 90% or more is preferably 200 seconds or less, where T 300s is the torque value at the time point 300 seconds after the start of measurement, T n It is the torque value at a time point of any length from the start of measurement. This allows the epoxy resin composition for sealing to have an even higher curing speed and an even higher curability. The time required for the cure rate to become more than 90% is more preferably less than 180 seconds, and even more preferably less than 160 seconds. The testing machine can be the same as the testing machine for measuring torque value and gel time. In the present embodiment, in the same manner as when measuring gel time, 1.67 ml of the epoxy resin composition for sealing is used as a sample for measurement. However, this amount of the epoxy resin composition for sealing is only an example, and should not be interpreted as limiting the amount of the epoxy resin composition for sealing used to make a cured product according to the present disclosure.
[0077] In the epoxy resin composition for sealing, in the spiral flow test method conforming to the ASTM D3123 standard, the test results are as follows: 2 The flow distance measured under the conditions of an injection pressure of 100 and a molding time of 180 seconds is preferably 50 cm or more. This makes it easier to improve the filling property when the sealing portion 4 is made of the sealing epoxy resin composition. The flow distance is more preferably 100 cm or more, and even more preferably 150 cm or more. The upper limit of the flow distance is not limited to any specific value, but can be adjusted appropriately.
[0078] The epoxy resin composition for sealing according to the present embodiment has high potential. As used herein, "potential" refers to the property that fluidity is less likely to decrease at a relatively low temperature (such as a normal temperature of 25°C) and maintains fluidity at any temperature until the temperature reaches the forming temperature. The epoxy resin composition for sealing according to the present embodiment has such high storage stability, and therefore has high potential, and cures quickly once the temperature reaches the forming temperature.
[0079] More specifically, these beneficial properties of the above-mentioned epoxy resin composition for sealing are achievable by appropriately adjusting the components of the above-mentioned chemical composition. However, the above-mentioned physical properties of the epoxy resin composition for sealing are merely examples and should not be construed as limiting.
[0080] <Electronic Devices>
[0081] As described above, the sealing epoxy resin composition according to this embodiment is suitable for manufacturing the sealing portion 4 of the electronic device 1. The electronic device 1 includes a semiconductor element 3 and a sealing portion 4 that seals the semiconductor element 3. The sealing portion 4 is a cured product of the above-mentioned sealing epoxy resin composition (see Figure 1 ). The electronic device 1 and an exemplary method of manufacturing the electronic device 1 will be described.
[0082] Examples of the electronic device 1 include plug-in packages, such as Mini, D package, D2 package, To22O, To3P and dual in-line package (DIP), and surface mount packages, such as quad flat package (QFP), small outline package (SOP), J-lead small outline package (SOJ), plastic ball grid array (PBGA), fine pitch ball grid array (FBGA), wafer level package (WLP), panel level package (PLP), fan-out wafer level package (FO-WLP), fan-out panel level package (FO-PLP), flip chip ball grid array (FC-BGA), package antenna (AiP) and system-level package (SiP).
[0083] Figure 1 1 is a cross-sectional view of an electronic device 1 according to the present embodiment. The electronic device 1 includes a metal lead frame 2, a semiconductor element 3 mounted on the lead frame 2, a wire 5 for electrically connecting the semiconductor element 3 to the lead frame 2, and a sealing portion 4 sealing the semiconductor element 3.
[0084] In the present embodiment, the lead frame 2 includes a die pad 6, an inner lead 21 and an outer lead 22. The lead frame 2 can be made of, for example, copper or an iron alloy such as 42 alloy. The lead frame 2 preferably includes a body 23 made of copper or an iron alloy such as 42 alloy and a plating 24 covering the body 23. This can reduce the corrosion of the lead frame 2. The plating 24 preferably contains at least one component selected from the group consisting of silver, nickel and palladium. The plating 24 may contain only one metal selected from the group consisting of silver, nickel and palladium, or contain an alloy including at least one metal selected from the group consisting of silver, nickel and palladium. Optionally, the plating 24 may have a multilayer structure. Specifically, the plating 24 may have a multilayer structure consisting of a palladium layer, a nickel layer and a gold layer. The plating 24 may have, but is not limited to, a thickness falling within the range of 1 μm to 20 μm.
[0085] The semiconductor element 3 is fixed to the die pad 6 of the lead frame 2 with an appropriate die bonding material 7. This allows the semiconductor element 3 to be mounted on the lead frame 2. The semiconductor element 3 can be, for example, an integrated circuit, a large-scale integrated circuit, a transistor, a thyristor, a diode or a solid-state image sensor. Optionally, the semiconductor element 50 can also be a new power device such as a SiC device or a GaN device.
[0086] Next, the semiconductor element 3 and the inner lead 21 of the lead frame 2 are connected together via the wire 5. The wire 5 may be a gold wire or may contain at least one of copper or silver. For example, the wire 5 may be made of, for example, silver or copper. If the wire 5 contains at least one of copper or silver, the wire 5 may be coated with a thin film of a metal such as palladium.
[0087] Subsequently, a sealing portion 4 that seals the semiconductor element 3 is formed by molding the epoxy resin composition for sealing. The sealing portion 4 also seals the wire 5. The sealing portion 4 also seals the die pad 6 and the inner lead 21. Therefore, the sealing portion 4 is in contact with the lead frame 2. If the lead frame 2 includes a plating layer 24, the sealing portion 4 is in contact with the plating layer 24.
[0088] The sealing portion 4 is preferably formed by molding the sealing epoxy resin composition by press molding, such as injection molding, transfer molding, or compression molding.
[0089] The conditions for molding the epoxy resin composition for sealing by press molding can be appropriately set according to the chemical composition of the epoxy resin composition for sealing. When molding the epoxy resin composition for sealing by press molding, the molding pressure can be, for example, 3.0 MPa or more, and the molding temperature can be 120° C. or more.
[0090] In particular, in the case of transfer molding, the injection pressure of the epoxy resin composition for sealing into the mold can be, for example, 3 MPa or more, preferably 4 MPa or more and 710 MPa or less. In addition, the heating temperature (mold temperature) is preferably 120° C. or more, more preferably 160° C. or more and 190° C. or less. In addition, the heating time is preferably 30 seconds or more and 300 seconds or less, more preferably 60 seconds or more and 180 seconds or less.
[0091] According to the transfer molding method, after the sealing portion 4 is formed inside the mold, post-curing is preferably performed by heating the sealing portion 4 while the mold remains closed, and then the mold is preferably opened to remove the electronic device 1. The heating conditions for post-curing include, for example, a heating temperature of 160° C. or higher and 190° C. or lower, and a heating time of 2 hours or higher and 8 hours or lower.
[0092] In this way, the electronic device 1 including the sealing portion 4 made of the sealing epoxy resin composition is manufactured. Note that the above-mentioned method for manufacturing the electronic device 1 is only an example and should not be construed as limiting. Alternatively, the electronic device 1 may be manufactured by any other method as long as an electronic component such as the semiconductor element 3 can be sealed by filling the gap with the above-mentioned sealing epoxy resin composition.
[0093] 3. Summary
[0094] As can be seen from the description of the above embodiments, the present disclosure has the following aspects. In the following description, in order to clarify the correspondence between the following aspects of the present disclosure and the constituent elements of the above exemplary embodiments, the reference numerals are inserted in parentheses.
[0095] The encapsulated epoxy resin composition according to the first aspect contains an epoxy resin (A), a curing agent (B), a curing accelerator (C), and an inorganic filler (D). The curing accelerator (C) contains an amidine silicate (C1) represented by the following formula (1):
[0096]
[0097] In formula (1), R1 and R2 are each independently a hydrogen atom or an aliphatic hydrocarbon group having 1 or more and 5 or less carbon atoms, R3 and R4 are each independently a phenylene group or a naphthylene group, and R5 is at least one group selected from the group consisting of a phenyl group and a group represented by the following formula (2):
[0098] -C n H 2n -X…(2).
[0099] In formula (2), n is 3 or more and 8 or less, and X is at least one functional group selected from the group consisting of -SH, -NH, -NH-Ph, -Ph-CH=CH2, -NH-C2H4-NH2, -N=C=O, a glycidyl ether group, and a group represented by the following formula (3):
[0100]
[0101] According to the present invention, it is possible to provide a sealing epoxy resin composition which has high storage stability and can increase the curing speed during curing.
[0102] In the encapsulated epoxy resin composition according to the second aspect which can be implemented in combination with the first aspect, in formula (1), R1 and R2 are each independently a hydrocarbon group having 1 or 2 carbon atoms, and R5 is a phenyl group or C3H6SH.
[0103] This aspect can further improve the storage stability of the epoxy resin composition for sealing, and can achieve higher curability during curing.
[0104] In the encapsulated epoxy resin composition according to the third aspect which can be implemented in combination with the first or second aspect, the amidine silicate (C1) contains at least one selected from the group consisting of a compound represented by the following formula (11), a compound represented by the following formula (12), and a compound represented by the following formula (13):
[0105]
[0106] This aspect can further improve the storage stability of the epoxy resin composition for sealing, and can achieve higher curability during curing.
[0107] In the encapsulated epoxy resin composition according to the fourth aspect which can be implemented in combination with any one of the first to third aspects, the proportion of the curing accelerator (C) is 1 part by mass or more and 35 parts by mass or less relative to 100 parts by mass of the total of the epoxy resin (A) and the curing agent (B).
[0108] This aspect makes it easier to further increase the curing speed of the sealing epoxy resin composition when curing, and allows the sealing epoxy resin composition to maintain even higher storage stability.
[0109] In the sealing epoxy resin composition according to the fifth aspect which can be implemented in combination with any one of the first to fourth aspects, the proportion of the inorganic filler (D) is 60% by mass or more and 93% by mass or less relative to the total amount of the epoxy resin (A), the curing agent (B), the curing accelerator (C) and the inorganic filler (D).
[0110] This aspect makes it easier for the encapsulating epoxy resin composition to maintain sufficient fluidity in a molten state, and ensures sufficient filling properties of the encapsulating epoxy resin composition.
[0111] In the sealed epoxy resin composition according to the sixth aspect which can be implemented in combination with any one of the first to fifth aspects, the average particle diameter of the inorganic filler (D) is 0.5 μm or more and 15 μm or less.
[0112] This aspect makes it easier for the epoxy resin composition for sealing to maintain good fluidity without causing a significant decrease in fluidity.
[0113] In the sealing epoxy resin composition according to the seventh aspect which can be implemented in combination with any one of the first to sixth aspects, the inorganic filler (D) includes inorganic particles each having a particle size of 0.1 μm or less, and the proportion of the inorganic particles is 0.1 parts by mass or more and 30 parts by mass or less relative to 100 parts by mass of the inorganic filler (D).
[0114] This aspect can maintain even better fluidity of the epoxy resin composition for sealing in a molten state.
[0115] The sealing epoxy resin composition according to the eighth aspect, which may be implemented in combination with any one of the first to seventh aspects, is in a solid form at 25°C.
[0116] The present invention allows the preparation of the epoxy resin composition for sealing at room temperature (about 25° C.) and ensures good storage stability, thereby reducing the possibility of causing changes in the chemical composition in the prepared state and achieving excellent workability.
[0117] In the sealing epoxy resin composition according to the ninth aspect, which can be implemented in combination with any one of the first to eighth aspects, when measured under conditions including a temperature of 170° C., the time required for 1.67 ml of the sealing epoxy resin composition to reach a torque value of 0.98 N is 30 seconds or more and 100 seconds or less.
[0118] This aspect makes it easier to maintain good fluidity when the sealing portion (4) is made of the sealing epoxy resin composition, and ensures a sufficiently high curing speed of the sealing epoxy resin composition.
[0119] In the sealing epoxy resin composition according to the tenth aspect which can be implemented in combination with any one of the first to ninth aspects, when the torque value of 1.67 ml of the sealing epoxy resin composition is measured under conditions including a temperature of 170° C., the torque value is n / T 300s The time required for the curing rate given by ×100 to become 90% or more is less than 200 seconds, where T 300s is the torque value at the time point 300 seconds after the start of measurement, T n It is the torque value at any time point after the measurement starts.
[0120] This aspect allows the encapsulating epoxy resin composition to have an even higher curing speed and an even higher curability.
[0121] In the sealing epoxy resin composition according to the eleventh aspect which can be implemented in combination with any one of the first to tenth aspects, in the spiral flow test method conforming to the ASTM D3123 standard, the test results are as follows: 2 Under the conditions of injection pressure of 100 and molding time of 180 seconds, the flow distance is more than 50 cm.
[0122] This aspect makes it easier to further improve the filling property when the sealing portion (4) is produced from the sealing epoxy resin composition.
[0123] The electronic device (1) according to the twelfth aspect comprises a semiconductor element and a sealing portion for sealing the semiconductor element. The sealing portion is a cured product of the sealing epoxy resin composition according to any one of the first to eleventh aspects.
[0124] Example
[0125] Next, specific embodiments of the present disclosure will be presented. Note that the specific embodiments described below are merely examples of the present disclosure and should not be interpreted as limiting the scope of the present disclosure.
[0126] 1. Preparation of resin composition
[0127] [Examples 1-7 and Comparative Examples 1-3]
[0128] The materials are compounded and mixed together using a mixer for 10 minutes to have any chemical composition shown in Table 1 (given later). Then, the thus mixed material is kneaded using a biaxial roll while being heated to a temperature falling within the range of 90°C to 140°C, thereby obtaining a mixture. Next, the thus obtained mixture is allowed to cool to room temperature (about 25°C) and then pulverized. In this way, a powdery resin composition is formed. Then, the powdery resin composition is tableted to obtain a sheet-like resin composition. The following are the details of each component.
[0129] Note that the unit "phr" shown in "the ratio of curing accelerator (C) to epoxy resin (A) + curing agent (B) + curing accelerator (C)" means "parts per hundred resin", that is, in the case of a resin component (i.e., resin) composed of epoxy resin (A), curing agent (B) and curing accelerator (C), the ratio of the curing accelerator (C) to the resin component.
[0130] (Epoxy resin)
[0131] Epoxy resin 1: manufactured by Nippon Kayaku Co., Ltd., product name: NC3000L;
[0132] Epoxy resin 2: manufactured by Mitsubishi Chemical Corporation, product name: YX4000H; and
[0133] · Epoxy resin 3: manufactured by Mitsubishi Chemical Corporation, product name: YX8800UH.
[0134] (Curing agent)
[0135] Curing agent 1: phenolic curing agent (manufactured by Meiwa Kasei Ltd., product name: MEH7851-SS); and
[0136] Curing agent 2: phenolic curing agent (manufactured by Meiwa Kasei Ltd., product name: MEH7841-4S)
[0137] (Curing accelerator)
[0138] Curing accelerator 1: amidine silicate represented by formula (11) (melting point: 235° C.);
[0139] Curing accelerator 2: amidine silicate represented by formula (12);
[0140] Curing accelerator 3: amidine silicate represented by formula (13);
[0141] Curing accelerator 4: a phosphonium salt represented by the following formula (100); and
[0142]
[0143] Curing accelerator 5: phosphonium-organic carboxylate represented by the following formula (101):
[0144]
[0145] (Inorganic filler)
[0146] Silica 1: manufactured by Denka Co., Ltd., product name: FB300MDC (spherical silica, average particle size: 5.0 μm, content of particles with a particle size of 0.1 μm or less: 1.8%);
[0147] Silica 2: manufactured by Denka Co., Ltd., product name: SFP10MK (spherical silica, average particle size: 0.8 μm, content of particles with a particle size of 0.1 μm or less: 7.8%);
[0148] Silica 3: manufactured by Tokuyama Corporation, product name: SS01 (spherical silica, average particle size: 0.1 μm, content of particles with a particle size of 0.1 μm or less: 7.4%); and
[0149] Silica 4: manufactured by Micron Inc., product name: ST7030-20 (spherical silica, average particle size: 9 μm, content of particles with a particle size of 0.1 μm or less: 3.6%).
[0150] (additive)
[0151] Silane coupling agent 1: manufactured by Shin-Etsu Silicones Co., Ltd., product name: KBM573 (N-phenyl-3-aminopropyltrimethoxysilane);
[0152] Silane coupling agent 2: manufactured by Shin-Etsu Silicones Co., Ltd., product name: KBM803 (3-mercaptopropyltrimethoxysilane);
[0153] Pigment: manufactured by Mitsubishi Chemical Corporation, product name: MA100 (carbon black); and Release agent: manufactured by Dainichi Chemical Industry Co., Ltd., product name: Carnauba F-100.
[0154] 2. Evaluation
[0155] 2.1 Fine filling rate (the proportion of fine particles with a particle size of 0.1 μm or less in the inorganic filler)
[0156] If a plurality of inorganic fillers having average particle diameters different from each other are compounded to prepare a resin composition, a mixture of inorganic fillers is prepared by mixing only the inorganic fillers together before mixing the inorganic fillers with other components, and the average particle diameter of the mixture of inorganic fillers is measured.
[0157] The average particle size was calculated by measuring the volume-based particle size distribution of the mixture of inorganic fillers using a laser diffraction scattering particle size analyzer. In addition, the proportion of the filling rate of particles with a particle size of 0.1 μm or less was calculated as the "fine filling rate" based on the particle size distribution. The results are summarized in Table 1. Note that in Table 1, "the average particle size D50 of the entire inorganic filler (D)" refers to the average particle size (median diameter D50) of the mixture of inorganic fillers.
[0158] 2.2 Spiral Flow
[0159] The spiral flow mold conforming to ASTM 3123 was used under the following conditions: mold temperature of 170°C, 70kgf·cm 2 The resin composition was molded under the conditions of an injection pressure of 1000 and a molding time of 180 seconds, and the distance (i.e., flow distance) of the resin composition flow within 180 seconds from the start of the molding process was measured. The values obtained by the measurement are summarized in Table 1. If the flow distance is more than 50 cm, it can be determined that the resin composition has excellent fluidity in the molten state.
[0160] 2.3 Gel time
[0161] Using a Curelastometer tester (manufactured by JSR Corporation, model: Curelastometer 7P), the torque value was measured by starting timing at the time when 1.67 ml of the sample resin composition was injected while setting the upper and lower temperatures of the mold to 170°C. Then, the torque value was measured to reach 0.1 kgf / cm 2 The time required (ie, gel time) is summarized in Table 1. If the gel time is 50 seconds or more, it can be determined that the resin composition has high fluidity in a molten state.
[0162] 2.4 Evaluation of melt residue
[0163] The resin composition was melt-kneaded at a temperature of 170°C, and a sheet was made from the resin composition thus melt-kneaded. A sheet having a thickness of 1 mm and a width of 150 cm was cut out from the sheet thus formed, and its cross section was observed with the naked eye. Next, a hand press and a Φ13 mm tabletting die were combined to form the sheet under conditions including a forming pressure of 50 MPa to form a sheet-like test piece having a thickness of 20 mm and a diameter of 13 mm. The sheet-like test piece was cut off. The cross section of the test piece was observed by a VHX-600 device manufactured by Keyence Corporation to count the number of white spots having a diameter or the longest side length of 100 μm or more on the cross section. The number of white spots thus counted is shown in Table 1. In Table 1, "10<" indicates that the number of white spots is 10 or more. It can be determined that the smaller the number of white spots, the higher the dispersibility in the molten state.
[0164] 2.5 Curing time
[0165] The curing rate is calculated based on the torque curve drawn by connecting the torque values obtained from the measurements described in Section 2.3. The curing rate can be calculated by the following equation:
[0166] Curing rate at any time point (%) = T n / T 300s ×100
[0167] Where T n is the torque value [kgf·cm] at any time point, T 300s It is the torque value [kgf·cm] at the time point when 300 seconds have passed. Note that the torque value at the time point when 300 seconds have passed is considered to be 100%.
[0168] According to the calculation results, the time required for the curing rate to reach 90% for the first time is shown as "90% curing time [sec]" in the following Table 1. If the 90% curing time is 200 seconds or more, it can be determined that the resin composition has a high curing speed.
[0169] 2.6 Storage stability
[0170] The resin composition was allowed to stand at 25° C. for 72 hours, and then the gel time was measured under the same conditions as in Section 2.3. The difference calculated by subtracting the gel time obtained by this measurement from the gel time obtained in Section 2.3 was divided by the gel time obtained in Section 2.3, and then the quotient was multiplied by 100. The values thus calculated are shown in Table 1 below. If the reduction rate of the gel time is 10% or less, it can be determined that the resin composition has high storage stability.
[0171] [Table 1]
[0172]
[0173] Reference numerals list
[0174] 1 Electronic devices
[0175] 3 Semiconductor components
[0176] 4 Sealing part
Claims
1. A sealing epoxy resin composition comprising Epoxy resin (A), Curing agent (B), a curing accelerator (C), and Inorganic filler (D), The curing accelerator (C) contains amidine silicate (C1) represented by the following formula (1): wherein R1 and R2 are each independently a hydrogen atom or an aliphatic hydrocarbon group having 1 or more and 5 or less carbon atoms, R3 and R4 are each independently a phenylene group or a naphthylene group, and R5 is at least one group selected from the group consisting of a phenyl group and a group represented by the following formula (2), —CnH2n—X(2) wherein n is greater than or equal to 3 and less than or equal to 8, and X is selected from -SH, -NH, -NH-Ph, -Ph-CH=CH2, -NH-C2H4-NH2, -N=C=O, at least one functional group selected from the group consisting of a glycidyl ether group and a group represented by the following formula (3), 2. The epoxy resin composition for sealing according to claim 1, wherein In the formula (1), R1 and R2 are each independently a hydrocarbon group having 1 or 2 carbon atoms, and R5 is a phenyl group or C3H6SH.
3. The sealing epoxy resin composition according to claim 1 or 2, wherein The amidine silicate (C1) contains at least one selected from the group consisting of a compound represented by the following formula (11), a compound represented by the following formula (12), and a compound represented by the following formula (13):
4. The sealing epoxy resin composition according to any one of claims 1 to 3, wherein The ratio of the curing accelerator (C) is 1 part by mass or more and 35 parts by mass or less relative to 100 parts by mass of the total of the epoxy resin (A) and the curing agent (B).
5. The sealing epoxy resin composition according to any one of claims 1 to 4, wherein The ratio of the inorganic filler (D) is 60% by mass or more and 93% by mass or less relative to the total amount of the epoxy resin (A), the curing agent (B), the curing accelerator (C) and the inorganic filler (D).
6. The sealing epoxy resin composition according to any one of claims 1 to 5, wherein The average particle size of the inorganic filler (D) is 0.5 μm or more and 15 μm or less.
7. The sealing epoxy resin composition according to any one of claims 1 to 6, wherein The inorganic filler (D) includes inorganic particles each having a particle size of 0.1 μm or less, and The ratio of the inorganic particles is 0.1 parts by mass or more and 30 parts by mass or less relative to 100 parts by mass of the inorganic filler (D).
8. The sealing epoxy resin composition according to any one of claims 1 to 7, wherein The sealing epoxy resin composition is in a solid form at 25°C.
9. The sealing epoxy resin composition according to any one of claims 1 to 8, wherein When measured under conditions including a temperature of 170° C., the time required for 1.67 ml of the sealing epoxy resin composition to reach a torque value of 0.98 N is 30 seconds or more and 100 seconds or less.
10. The sealing epoxy resin composition according to any one of claims 1 to 9, wherein When the torque value of 1.67 ml of the epoxy resin composition for sealing is measured under conditions including a temperature of 170° C., the torque value of n / T 300s The time required for the curing rate given by ×100 to become 90% or more is less than 200 seconds, where T 300s is the torque value at the time point 300 seconds after the start of measurement, T n is the torque value at any time point after the start of measurement.
11. The sealing epoxy resin composition according to any one of claims 1 to 10, wherein In the spiral flow test method in accordance with ASTM D3123, the test conditions include a mold temperature of 170°C, a pressure of 686.5 N / cm 2 Under the conditions of injection pressure of 100 and molding time of 180 seconds, the flow distance is more than 50 cm.
12. An electronic device comprising: Semiconductor components; and a sealing portion for sealing the semiconductor element, The sealing portion is a cured product of the sealing epoxy resin composition according to any one of claims 1 to 11.
Citation Information
Patent Citations
Epoxy resin curing accelerator
JP6917707B2
Epoxy resin composition for sealing, and electronic component device
WO2012102336A1