Gas black derived from rubber-derived pyrolysis oil
By using rubber-derived pyrolytic oil in the gas black reactor for thermal oxidation and decomposition, the problem of fossil raw materials is solved, and environmentally friendly carbon black with the same characteristics is produced, achieving efficient utilization of resources and environmental protection goals.
Patent Information
- Application Number
- CN202380029195.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-29
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-05
AI Technical Summary
The existing carbon black production process relies on fossil raw materials, resulting in environmental pollution and resource depletion, which is difficult to replace, and cannot effectively solve the problems of environmental protection and resource utilization.
Rubber-derived pyrolytic oil is used as the carbon black raw material, and carbon black is produced in the gas black reactor through thermal oxidation and decomposition, replacing traditional fossil raw materials, achieving environmental protection and efficient utilization of resources.
The carbon black produced has characteristics comparable to traditional carbon black, and through the use of recyclable materials, environmental pollution and resource waste are reduced, supporting the realization of a circular economy.
Smart Images

Figure BDA0005052511790000281 
Figure BDA0005052511790000282 
Figure BDA0005052511790000291
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing carbon black, the carbon black obtained by the method and the use of the carbon black. The present invention also relates to a composition containing the carbon black, the use of the composition and an article prepared from the composition. Background Art
[0002] Carbon black produced by the gas black process offers beneficial properties in many applications, such as use as pigments.
[0003] However, gas black is usually produced using fossil raw materials such as coal and crude oil. Fossil raw materials are limited and are being depleted rapidly. In addition, fossil raw materials have a major negative impact on the environment because their extraction and transportation have a great impact on the environment. For example, there have been oil spills in the past, which have led to water pollution and the death of aquatic animals (including those near the coast). In addition, it is well known that the combustion of fossil raw materials and the resulting production of carbon dioxide is one of the main factors causing global warming. The unstable price of fossil raw materials and the dependence on politically unstable areas for transportation are further reasons for seeking alternatives to fossil raw materials.
[0004] We want to avoid the disadvantages of using fossil raw materials. Recyclable materials used as raw materials for carbon black production are more environmentally friendly. Using recycled raw materials helps to protect limited fossil resources and creates opportunities for a circular economy. However, it is difficult to replace fossil raw materials with other raw materials in the gas black process because the feed lines and burners of the gas black reactor are easily blocked, which requires shutdown and disassembly of the equipment for cleaning.
[0005] Depending on the application, it is desirable to have carbon black materials produced from recycled feedstocks that exhibit certain properties comparable to known carbon blacks.
[0006] It is therefore an object of the present invention to provide a process for producing carbon black which creates opportunities for the implementation of a circular economy and provides carbon black having properties comparable to those of known and established carbon blacks. Summary of the invention
[0007] Surprisingly, the objects of the present invention are solved by the process disclosed in the independent claims and the carbon black obtained by the process. Particular or preferred variants of the invention are set out in the dependent claims.
[0008] The following statements summarize some aspects of the invention.
[0009] A first aspect of the present invention relates to a method for producing carbon black by thermal oxidative decomposition of a carbon black feedstock, wherein the carbon black feedstock comprises rubber-derived pyrolysis oil, and wherein the production of the carbon black is carried out in a gas black reactor.
[0010] A second aspect of the present invention relates to the method according to the first aspect, wherein the rubber-derived pyrolysis oil comprises tire-derived pyrolysis oil (TPO).
[0011] A third aspect of the present invention relates to the method according to the first aspect or the second aspect, wherein the rubber-derived pyrolysis oil consists of tire-derived pyrolysis oil (TPO).
[0012] A fourth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has
[0013] Total carbon in the range of 80.0 mass % to 90.0 mass %;
[0014] Total hydrogen in the range of 8.0 mass % to 15.0 mass %; and
[0015] a C / H atomic ratio in the range of 0.60 to 1.0;
[0016] wherein mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0017] A fifth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has
[0018] Total carbon in the range of 85.0 mass % to 90.0 mass %;
[0019] Total hydrogen in the range of 8.0 mass % to 11.0 mass %; and
[0020] a C / H atomic ratio in the range of 0.65 to 1.0;
[0021] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0022] A sixth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has the following characteristics
[0023] Total carbon in the range of 86.0 mass % to 90.0 mass %;
[0024] Total hydrogen in the range of 8.5 mass % to 10.5 mass %; and
[0025] a C / H atomic ratio in the range of 0.70 to 0.90;
[0026] wherein mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0027] A seventh aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has
[0028] Total carbon in the range of 87.0 mass % to 90.0 mass %;
[0029] Total hydrogen in the range of 9.0 mass % to 10.0 mass %; and
[0030] a C / H atomic ratio in the range of 0.70 to 0.85;
[0031] wherein mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0032] An eighth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has
[0033] Up to 1.00 mass % total nitrogen; and / or
[0034] Up to 1.35 mass % total sulfur;
[0035] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0036] A ninth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has:
[0037] Up to 0.80 mass % total nitrogen; and / or
[0038] Up to 1.25 mass % total sulfur;
[0039] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0040] A tenth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has
[0041] Up to 0.65 mass % total nitrogen; and / or
[0042] Up to 1.20 mass % total sulfur;
[0043] Wherein, mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0044] An eleventh aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has:
[0045] An ash content of less than 0.04 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil, and wherein the ash content is determined according to ASTM D2415-20.
[0046] A twelfth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has:
[0047] An ash content of less than 0.03 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil, and wherein the ash content is determined according to ASTM D2415-20.
[0048] A thirteenth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has:
[0049] A sieve residue of up to 250 mg / kg based on the total weight of the rubber derived pyrolysis oil and determined according to ASTM D4870-18 (25 μm sieve size).
[0050] A fourteenth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber derived pyrolysis oil has:
[0051] Up to 230 mg / kg sieve residue based on the total weight of the rubber derived pyrolysis oil and determined according to ASTM D4870-18 (25 μm mesh size).
[0052] A fifteenth aspect of the present invention relates to the method according to any one of the second to fourteenth aspects, wherein the tire-derived pyrolysis oil (TPO) has:
[0053] Total carbon in the range of 85.0 mass % to 90.0 mass %;
[0054] Total hydrogen in the range of 8.0 mass % to 11.0 mass %; and
[0055] a C / H atomic ratio in the range of 0.65 to 1.0;
[0056] Wherein, mass % is based on the total mass of TPO excluding water and ash content, and wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0057] A sixteenth aspect of the present invention relates to a method according to any one of the second to fifteenth aspects, wherein the TPO has:
[0058] Total carbon in the range of 86.0 mass % to 90.0 mass %;
[0059] Total hydrogen in the range of 8.5 mass % to 10.5 mass %; and
[0060] a C / H atomic ratio in the range of 0.70 to 0.90;
[0061] Wherein, mass % is based on the total mass of TPO excluding water and ash content, and wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0062] The seventeenth aspect of the present invention relates to the method according to any one of the second to sixteenth aspects, wherein the TPO has the following characteristics:
[0063] Total carbon in the range of 87.0 mass % to 90.0 mass %;
[0064] Total hydrogen in the range of 9.0 mass % to 10.0 mass %; and
[0065] a C / H atomic ratio in the range of 0.70 to 0.85;
[0066] Wherein, mass % is based on the total mass of TPO excluding water and ash content, and wherein total carbon and total hydrogen are determined according to ASTM D5291C-21.
[0067] The eighteenth aspect of the present invention relates to a method according to any one of the second to seventeenth aspects, wherein the TPO has
[0068] 0.40 mass % to 0.65 mass % total nitrogen; and / or
[0069] Up to 1.35 mass % total sulfur;
[0070] Wherein, mass % is based on the total mass of TPO excluding water and ash content, and wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0071] The nineteenth aspect of the present invention relates to a method according to any one of the second to eighteenth aspects, wherein the TPO has
[0072] 0.45 mass % to 0.65 mass % total nitrogen; and / or
[0073] Up to 1.25 mass % total sulfur;
[0074] Wherein, mass % is based on the total mass of TPO excluding moisture and ash content, and wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0075] The twentieth aspect of the present invention relates to the method according to any one of the second to nineteenth aspects, wherein the TPO has:
[0076] 0.45 mass % to 0.60 mass % total nitrogen; and / or
[0077] Up to 1.20 mass % total sulfur;
[0078] Wherein, mass % is based on the total mass of TPO excluding water and ash content, and wherein total nitrogen and total sulfur are determined according to ASTM D5291C-21.
[0079] The twenty-first aspect of the present invention relates to the method according to any one of the second to twentieth aspects, wherein the TPO has:
[0080] An ash content of less than 0.04 mass %, wherein the mass % is based on the total mass of the TPO, and wherein the ash content is determined according to ASTM D2415-20.
[0081] The twenty-second aspect of the present invention relates to the method according to any one of the second to twenty-first aspects, wherein the TPO has:
[0082] An ash content of less than 0.03 mass %, wherein the mass % is based on the total mass of the TPO, wherein the ash content is determined according to ASTM D2415-20.
[0083] The twenty-third aspect of the present invention relates to the method according to any one of the second to twenty-second aspects, wherein the TPO has:
[0084] Up to 250 mg / kg sieve residue based on the total weight of TPO and determined according to ASTM D4870-18 (25 μm mesh size).
[0085] The twenty-fourth aspect of the present invention relates to the method according to any one of the second to twenty-third aspects, wherein the TPO has:
[0086] Up to 230 mg / kg sieve residue based on total TPO weight and determined according to ASTM D4870-18 (25 μm mesh size).
[0087] The twenty-fifth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the carbon black raw material further comprises a conventional carbon black raw material, wherein the conventional carbon black raw material includes coal tar distillate oil, residual oil produced during the catalytic cracking process of petroleum fractions, residual oil produced during the production of olefins by cracking naphtha or gas oil, or a mixture of any combination of the foregoing, preferably coal tar distillate oil.
[0088] The twenty-sixth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the carbon black raw material contains at least 10 weight percent, preferably at least 30 weight percent, more preferably at least 50 weight percent, even more preferably at least 70 weight percent, and most preferably at least 90 weight percent of rubber-derived pyrolysis oil, based on the total weight of the carbon black raw material.
[0089] A twenty-seventh aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the carbon black feedstock consists of rubber derived pyrolysis oil.
[0090] The twenty-eighth aspect of the present invention relates to a method according to any one of the preceding aspects, wherein the rubber-derived pyrolysis oil comprises at least 10 wt. %, preferably at least 30 wt. %, more preferably at least 50 wt. %, even more preferably at least 70 wt. %, and most preferably at least 90 wt. % of tire-derived pyrolysis oil (TPO), based on the total weight of the rubber-derived pyrolysis oil.
[0091] The twenty-ninth aspect of the present invention relates to a method according to any one of the preceding aspects, comprising gasifying a carbon black feedstock in a carrier gas flow, burning the carrier gas flow loaded with the carbon black feedstock in a burner in the presence of air to form carbon black, and terminating the formation of carbon black.
[0092] The thirtieth aspect of the present invention relates to carbon black obtained by the method according to any one of the preceding aspects, wherein the carbon black is gas black.
[0093] The thirty-first aspect of the present invention relates to the carbon black according to the thirtieth aspect, wherein the carbon black has:
[0094] An Oil Absorption Number (OAN) equal to or greater than 110 mL / 100 g, wherein OAN is determined according to ASTM D2414-21.
[0095] The thirty-second aspect of the present invention relates to the carbon black according to the thirtieth aspect or the thirty-first aspect, wherein the carbon black has:
[0096] A volatile content equal to or greater than 6%, wherein the volatile content (at 950° C.) is determined according to DIN 53552:1977-09.
[0097] The thirty-third aspect of the present invention relates to the carbon black according to any one of the 30th to 32nd aspects, wherein the OAN of the carbon black ranges from 110-180 mL / 100 g, preferably 115-165 mL / 100 g; wherein the OAN is measured according to ASTM D2414-21.
[0098] The thirty-fourth aspect of the present invention relates to the carbon black according to any one of the thirtieth to thirty-third aspects, wherein the volatile content of the carbon black is 6%-10%; wherein the volatile content (at 950°C) is measured according to DIN 53552:1977-09.
[0099] The thirty-fifth aspect of the present invention relates to the carbon black according to any one of the thirtieth to thirty-fourth aspects, wherein the STSA of the carbon black is in the range of 70-300 m 2 / g, preferably 70-270m 2 / g, more preferably 80-250m 2 / g; wherein STSA is measured according to ASTM D6556-19a.
[0100] The thirty-sixth aspect of the present invention relates to the carbon black according to any one of the 30th to 35th aspects, wherein the BET surface area of the carbon black is in the range of 80-350 m 2 / g, preferably 80-320m 2 / g, more preferably 90-300m 2 / g; wherein the BET specific surface area is measured according to ASTM D6556-19a.
[0101] The thirty-seventh aspect of the present invention relates to the carbon black according to any one of the 30th to 36th aspects, wherein the tint strength of the carbon black ranges from 30% to 250%, preferably from 50% to 160%; wherein the tint strength is measured according to ASTM D3265-21.
[0102] The thirty-eighth aspect of the present invention relates to a carbon black according to any one of aspects 30 to 37, wherein the pMC (percent of modern carbon) of the carbon black ranges from 1-65%, preferably 5-60%, more preferably 10-60%, and even more preferably 15-55%, wherein the pMC is determined according to ASTM D6866-20 Method B (AMS).
[0103] The thirty-ninth aspect of the present invention relates to the carbon black according to the thirtieth to thirty-eighth aspects, wherein the carbon black is oxidized and / or functionalized.
[0104] The 40th aspect of the present invention relates to the use of the carbon black according to the 30th to 39th aspects as a reinforcing filler or additive, a UV stabilizer, a conductive carbon black or a pigment, preferably as a pigment.
[0105] The 41st aspect of the present invention relates to the use of the carbon black according to the 30th to 39th aspects in rubber and rubber mixtures, plastics, inks (such as printing inks, inkjet inks or other inks), toners, paints, coatings, paper, adhesives, batteries or black matrix applications, preferably in inks, paints and coatings.
[0106] The forty-second aspect of the present invention is directed to a composition comprising the carbon black according to the thirtieth to thirty-ninth aspects.
[0107] The forty-third aspect of the present invention relates to the composition according to the forty-second aspect, wherein the composition is an ink composition, a coating composition or a paint composition.
[0108] The forty-fourth aspect of the present invention relates to an article prepared from the composition according to the forty-third aspect.
[0109] The forty-fifth aspect of the present invention relates to the product according to the forty-fourth aspect, which is a coated product or a colored product or a printed product. DETAILED DESCRIPTION
[0110] The present invention relates to a method for producing carbon black by thermal oxidative decomposition of a carbon black feedstock. The carbon black feedstock of the present invention comprises rubber-derived pyrolysis oil. The production of carbon black is carried out in a gas black reactor. Therefore, the method of the present invention is a gas black process.
[0111] As used herein, the term "carbon black" refers to a material consisting essentially of carbon, e.g., a carbon content greater than 80 wt%, or greater than 90 wt%, or greater than 95 wt%, based on the total weight of the material. The production of carbon black by the gas black process is well known in the art, e.g., J.-B. Donnet et al., "Carbon Black: Science and Technology", 2 nd pp. 57 and 58 in ed., Marcel Dekker, Inc., New York (1993); H. Ferch "Pigmentruβe", 1 st ed., Curt R. Vincentz Verlag, Hannover (1995), pp. 31-33; and "Ullmann's Encyclopedia of Chemical Engineering", 3 rdpp. 798 and 799 of IEEE International Edition, Volume 14 (1963), and DE 845 683 C, DE 504 428 C and US Pat. No. 3,978,019.
[0112] H. Ferch "Pigmentruβe",1 st ed., Curt R. Vincentz Verlag, Hannover (1995), p. 33 and in “Ullmann's Encyclopedia of Chemical Engineering”, 3 rd Page 799 of IEEE International Standards Institute, Vol. 14 (1963) shows a conventional gas black reactor.
[0113] The process of the present invention may include gasifying a carbon black feedstock in a carrier gas stream, combusting the carrier gas stream loaded with the carbon black feedstock in a combustor in the presence of air to form carbon black, and terminating the formation of carbon black.
[0114] The carbon black raw material of the present invention can be heated in a gasifier, and the generated steam is carried to the burner by a carrier gas. The carrier gas flow may include hydrogen, oxygen, nitrogen, methane, natural gas, CO 2 and mixtures thereof. The carrier gas may be loaded with gasified carbon black raw materials so that each m 3 The carrier gas contains 400-2200 g of gasified carbon black feedstock. The carrier gas can, for example, flow directly or countercurrently through the carbon black feedstock, or the carrier gas can be directed to flow through the carbon black at rest. The carrier gas is preferably heated to a suitable temperature, for example, to the gasification temperature of the carbon black feedstock, for example, to a temperature range of 200-400° C. When the mixture comprising the carrier gas and the gasified carbon black feedstock is delivered to the burner, the temperature of the carrier gas and the gasified carbon black feedstock mixture can be within a range such that the carbon black feedstock does not deposit or prematurely decompose in the pipeline or burner. The temperature of the burner is preferably maintained so that it does not exceed 350-400° C.
[0115] The carrier gas loaded with the gasified carbon black feedstock can be combusted in the presence of air in a burner to form carbon black. The formation of carbon black is usually completed by depositing the formed carbon black on a cooling device (e.g., a cylinder, a movable sledge-like conduit, a disc-shaped device, etc.). The deposition device can be cooled by water.
[0116] In conventional gas black reactors, the gas black burner and the deposition device (e.g., deposition roller) are usually installed together in a housing. The water-cooled deposition roller can have a diameter of 0.4-0.7 m, a length of 3-7 m, and a rotation speed of usually 0.8-1.25 rpm. In the upper part of the housing, the exhaust gas can be sucked away and guided to the filter plant through a pipeline. The carrier gas generally enters from the open bottom of the housing. In conventional gas black reactors, individual cast iron burners can be placed side by side, and fan-shaped diffusion flames are generated by flat nozzles perpendicular to the axis of the deposition roller. The burner is usually installed at the connection of the gas supply pipe jacket. The gas supply pipe can be arranged below the cooling roller parallel to the axis of the cooling roller. The distance of the burner nozzle can be selected so that the flame burns against the rotating roller and is thereby cooled.
[0117] As used herein, the term "rubber-derived pyrolysis oil" refers to the liquid fraction produced during the pyrolysis of rubber products. Rubber-derived pyrolysis oil generally contains a mixture of saturated and unsaturated hydrocarbons and may contain polar compounds including sulfur, nitrogen and oxygen.
[0118] The pyrolysis of rubber products generally includes heating the rubber products to a temperature of, for example, at least 300° C. under anaerobic conditions to volatilize and decompose the rubber products, producing oil, gas and char. As used herein, the term "rubber product" refers to a product composed of rubber, for example, a product composed of at least 50% by weight of rubber based on the total weight of the rubber product. Examples of rubber products include, but are not limited to, tires, conveyor belts, washers (e.g., door washers), transmission belts, floor mats, soles, conveyor belts, cable sheaths, hoses, and the like. Preferably, the rubber product includes a tire. The term "rubber" includes natural rubber and synthetic rubber or mixtures thereof. Natural rubber can be obtained from Helvea brasiliensis, guayule and dandelion. The synthetic rubber may include styrene-butadiene rubber, such as emulsion-polymerized styrene-butadiene rubber and solution-polymerized styrene-butadiene rubber, polybutadiene, polyisoprene, ethylene-propylene-diene rubber, ethylene-propylene-diene rubber, butyl rubber, halogenated butyl rubber, chlorinated polyethylene, chlorosulfonated polyethylene, nitrile rubber, hydrogenated nitrile rubber, polychloroprene, acrylate rubber, ethylene-vinylacetate rubber, ethylene-acrylic acid rubber, epichlorohydrin rubber, silicone rubber, fluorosilicone rubber, fluorocarbon rubber, or a mixture or combination of any of the above rubbers.
[0119] According to the present invention, rubber-derived pyrolysis oil may include tire-derived pyrolysis oil (TPO). As used herein, the term "tire-derived pyrolysis oil" ("TPO") refers to a liquid fraction obtained by pyrolyzing a tire under anaerobic conditions. TPO typically contains a mixture of saturated and unsaturated hydrocarbons and may contain polar compounds including sulfur, nitrogen and oxygen. Typically, waste tires (also known as "end-of-life" tires (ELT)) are used for pyrolysis to obtain TPO. As used herein, "waste tires" or "end-of-life tires" refer to tires that are unsuitable for use on vehicles due to, for example, wear or irreparable damage (e.g., punctures), such as truck tires, passenger car tires, off-road tires, aircraft tires, agricultural tires, and earth-moving machinery tires.
[0120] Pyrolysis processes for rubber products (e.g., tires) are well known in the art and include heating the tire in the absence of oxygen. Suitable methods for obtaining rubber-derived pyrolysis oils, particularly TPO, include, but are not limited to, those described in US2002 / 0072641A1, US2002 / 0072640A1, US2005 / 0101812A1, and EP2427533A1.
[0121] The rubber-derived pyrolysis oil may comprise at least 5 wt %, such as at least 10 wt %, or at least 10 wt %, or at least 15 wt %, or at least 20 wt %, or at least 25 wt %, or at least 30 wt %, or at least 35 wt %, or at least 40 wt %, or at least 45 wt %, or at least 50 wt %, or at least 55 wt %, or at least 60 wt %, or at least 65 wt %, or at least 70 wt %, or at least 75 wt %, or at least 80 wt %, or at least 85 wt %, or at least 90 wt %, or at least 95 wt %, or at least 99 wt % of tire-derived pyrolysis oil (TPO), based on the total weight of the rubber-derived pyrolysis oil. According to the present invention, the rubber-derived pyrolysis oil may comprise at least 10 wt %, preferably at least 30 wt %, more preferably at least 50 wt %, even more preferably at least 70 wt %, and most preferably at least 90 wt % of TPO, based on the total weight of the rubber-derived pyrolysis oil. The rubber-derived pyrolysis oil of the present invention may consist of TPO.
[0122] Suitable examples of rubber derived pyrolysis oils, particularly TPOs, include, but are not limited to, ThermoTireOil RR commercially available from Pyrum Innovations AG (Germany).
[0123] According to the present invention, the flash point of the rubber-derived pyrolysis oil may be at least 3°C, preferably at least 5°C, more preferably 50°C, and most preferably at least 65°C. As used herein, the term "flash point" refers to the lowest temperature at which a volatile substance vaporizes in air to form a flammable mixture. The flash point may be measured according to ASTM D93D. The rubber-derived pyrolysis oil may be treated by distillation (e.g., atmospheric fractionation, thin film distillation, etc.) to obtain a fraction having a higher flash point, e.g., at least 65°C.
[0124] According to the present invention, the total carbon of the rubber-derived pyrolysis oil may be at least 80.0% by mass, such as at least 81.0% by mass, or at least 82.0% by mass, or at least 83.0% by mass, or at least 84.0% by mass, or at least 85.0% by mass, or at least 85.5% by mass, or at least 86.0% by mass, or at least 86.5% by mass, or at least 87.0% by mass, or at least 87.5% by mass, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The total carbon of the rubber-derived pyrolysis oil may be 90.0% by mass or less, such as 89.5% by mass or less or 89.0% by mass or less, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The moisture content may be measured according to ASTM D4928-12R18, and the ash content may be measured according to ASTM D2415-20 (at 550°C). It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the total carbon of the rubber derived pyrolysis oil may be in the range of 80.0-90.0 mass %, preferably 85.0-90.0 mass %, more preferably 86.0-90.0 mass %, most preferably 87.0-90.0 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content. The total carbon is determined according to ASTM D5291C-21.
[0125] According to the present invention, the total hydrogen of the rubber-derived pyrolysis oil may be at least 8.0 mass %, such as at least 8.5 mass %, or at least 9.0 mass %, or at least 9.5 mass %, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The moisture content may be measured according to ASTM D4928-12R18, and the ash content may be measured according to ASTM D2415-20 (at 550° C.). The total hydrogen of the rubber-derived pyrolysis oil may be 15.0 mass % or less, such as 14.0 mass % or less, or 13.0 mass % or less, or 12.0 mass % or less, or 11.0 mass % or less, or 10.5 mass % or less, or 10.0 mass % or less, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the total hydrogen of the rubber derived pyrolysis oil may be in the range of 8.0-15.0 mass %, preferably 8.0-11.0 mass %, more preferably 8.5-10.5 mass %, most preferably 9.0-10.0 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content. The total hydrogen is determined according to ASTM D5291C-21.
[0126] According to the present invention, the C / H atomic ratio of the rubber derived pyrolysis oil can be at least 0.60, such as at least 0.65, or at least 0.70, or at least 0.75. The C / H atomic ratio of the rubber derived pyrolysis oil can be less than 1.0, such as less than 0.95, or less than 0.90, or less than 0.85, or less than 0.80. Those skilled in the art will understand that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, the C / H atomic ratio of the rubber derived pyrolysis oil can be in the range of 0.60-1.0, preferably 0.65-1.0, preferably 0.70-0.90, and more preferably 0.70-0.85. The C / H atomic ratio is calculated based on the total carbon and total hydrogen determined according to ASTM D5291C-21 as described above.
[0127] Rubber derived pyrolysis oil can have:
[0128] Total carbon in the range of 80.0-90.0 mass %, preferably 85.0-90.0 mass %, more preferably 86.0-90.0 mass %, most preferably 87.0-90.0 mass %;
[0129] Total hydrogen in the range of 8.0-15.0 mass %, preferably 8.0-11.0 mass %, more preferably 8.5-10.5 mass %, most preferably 9.0-10.0 mass %; and
[0130] a C / H atomic ratio in the range of 0.60-1, preferably 0.65-1.0, more preferably 0.70-0.90, most preferably 0.70-0.85;
[0131] Wherein, mass % is based on the total mass of rubber derived pyrolysis oil excluding water and ash content. Total carbon and total hydrogen are determined according to ASTM D5291C-21. C / H atomic ratio is calculated based on total carbon and total hydrogen. Water content can be measured according to ASTMD4928-12R18, and ash content can be measured according to ASTM D2415-20 (at 550°C).
[0132] According to the present invention, the total nitrogen of the rubber-derived pyrolysis oil may be at least 0.01 mass%, such as at least 0.02 mass%, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The moisture content may be measured according to ASTM D4928-12R18, and the ash content may be measured according to ASTM D2415-20 (at 550°C). The total nitrogen of the rubber-derived pyrolysis oil may be at most 1.00 mass%, such as at most 0.90 mass%, or at most 0.80 mass%, or at most 0.70 mass%, or at most 0.65 mass%, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the total nitrogen of the rubber derived pyrolysis oil may be in the range of 0.01-1.00 mass %, such as 0.01-0.80 mass %, or 0.01-0.65 mass %, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content. The total nitrogen is determined according to ASTM D5291C-21.
[0133] According to the present invention, the total sulfur of the rubber-derived pyrolysis oil may be at most 1.35 mass %, such as at most 1.30 mass %, or at most 1.25 mass %, or at most 1.20 mass %, or at most 1.15 mass %, or at most 1.10 mass %, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil excluding water and ash content. The moisture content may be determined according to ASTM D4928-12R18, and the ash content may be determined according to ASTM D2415-20 (at 550° C.). The total sulfur is determined according to ASTM D5291C-21.
[0134] Rubber derived pyrolysis oil can have:
[0135] Up to 1.00 mass %, preferably up to 0.80 mass %, more preferably up to 0.65 mass % of total nitrogen; and
[0136] Up to 1.35 mass %, preferably up to 1.25 mass %, more preferably up to 1.20 mass % total sulfur;
[0137] Wherein, mass % is based on the total mass of rubber derived pyrolysis oil excluding water and ash content. Total nitrogen and total sulfur are determined according to ASTM D5291C-21. Moisture content can be determined according to ASTM D4928-12R18, and ash content can be determined according to ASTM D2415-20 (at 550°C).
[0138] According to the present invention, the rubber derived pyrolysis oil may have the following characteristics:
[0139] Total carbon in the range of 80.0-90.0 mass %, preferably 85.0-90.0 mass %, more preferably 86.0-90.0 mass %, most preferably 87.0-90.0 mass %;
[0140] Total hydrogen in the range of 8.0-15.0, preferably 8.0-11.0 mass %, more preferably 8.5-10.5 mass %, most preferably 9.0-10.0 mass %;
[0141] a C / H atomic ratio in the range of 0.60-1.0, preferably 0.65-1.0, more preferably 0.70-0.90, most preferably 0.70-0.85;
[0142] Up to 1.00 mass %, preferably up to 0.80 mass %, more preferably up to 0.65 mass % of total nitrogen; and
[0143] Up to 1.35 mass %, preferably up to 1.25 mass %, more preferably up to 1.20 mass % total sulfur;
[0144] Wherein, mass % is based on the total mass of rubber derived pyrolysis oil excluding water and ash content. Total carbon, total hydrogen, total nitrogen and total sulfur are determined according to ASTM D5291C-21. C / H atomic ratio is calculated based on total carbon and total hydrogen. Water content can be determined according to ASTM D4928-12R18, and ash content can be determined according to ASTM D2415-20 (at 550°C).
[0145] According to the present invention, the ash content of the rubber-derived pyrolysis oil may be less than 0.04 mass %, such as less than 0.03 mass %, or less than 0.02 mass %, or less than 0.01 mass %, wherein the mass % is based on the total mass of the rubber-derived pyrolysis oil. The ash content is measured according to ASTM D2415-20 (at 550°C).
[0146] The rubber derived pyrolysis oil may have a sieve residue of 250 mg / kg or less, such as 230 mg / kg or less, based on the total weight of the rubber derived pyrolysis oil. The sieve residue is determined according to ASTM D4870-18 (25 μm mesh size).
[0147] According to the present invention, the TPO may have at least 85.0% by mass, such as at least 85.5% by mass, or at least 86.0% by mass, or at least 86.5% by mass, or at least 87.0% by mass, or at least 87.5% by mass of total carbon, wherein the mass % is based on the total mass of the TPO excluding water and ash content. The moisture content can be determined according to ASTM D4928-12R18, and the ash content can be determined according to ASTM D2415-20 (at 550° C.). The TPO may have a total carbon of 90.0% by mass or less, such as 89.5% by mass or less, or 89.0% by mass or less, wherein the mass % is based on the total mass of the TPO excluding water and ash content. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Thus, the TPO may have a total carbon in the range of 85.0-90.0 mass %, preferably 86.0-90.0 mass %, more preferably 87.0-90.0 mass %, wherein the mass % is based on the total mass of the TPO excluding moisture and ash. The total carbon is determined according to ASTM D5291C-21.
[0148] According to the present invention, TPO can have at least 8.0 mass %, such as at least 8.5 mass %, or at least 9.0 mass %, or at least 9.5 mass % of total hydrogen, wherein the mass % is based on the total mass of TPO excluding water and ash content. The moisture content can be determined according to ASTM D4928-12R18, and the ash content can be determined according to ASTM D2415-20 (at 550 ° C). TPO can have 11.0 mass % or less, such as 10.5 mass % or less, or 10.0 mass % or less of total hydrogen, wherein the mass % is based on the total mass of TPO excluding water and ash content. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, TPO can have 8.0-11.0 mass %, preferably 8.5-10.5 mass %, and more preferably 9.0-10.0 mass % of total hydrogen, wherein the mass % is based on the total mass of TPO excluding water and ash content. Total hydrogen is determined according to ASTM D5291C-21.
[0149] According to the present invention, TPO can have a C / H atomic ratio of at least 0.65, such as at least 0.70, or at least 0.75. TPO can have a C / H atomic ratio of less than 1.0, such as less than 0.95, or less than 0.90, or less than 0.85, or less than 0.80. It will be understood by those skilled in the art that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, TPO can have a C / H atomic ratio in the range of 0.65-1.0, preferably 0.70-0.90, and more preferably 0.70-0.85. The C / H atomic ratio is calculated based on the total carbon and total hydrogen determined according to ASTM D5291C-21 as described above.
[0150] TPO can have:
[0151] Total carbon in the range of 85.0-90.0 mass %, preferably 86.0-90.0 mass %, more preferably 87.0-90.0 mass %;
[0152] Total hydrogen in the range of 8.0-11.0 mass %, preferably 8.5-10.5 mass %, more preferably 9.0-10.0 mass %; and
[0153] a C / H atomic ratio in the range of 0.65-1.0, preferably 0.70-0.90, more preferably 0.70-0.85;
[0154] Wherein, mass % is based on the total mass of TPO excluding water and ash content. The water content can be measured according to ASTM D4928-12R18, and the ash content can be measured according to ASTM D2415-20 (at 550°C). The total carbon and total hydrogen are measured according to ASTM D5291C-21. The C / H atomic ratio is calculated based on the total carbon and total hydrogen.
[0155] According to the present invention, TPO may have at least 0.40% by mass, such as at least 0.45% by mass, or at least 0.50% by mass of total nitrogen, wherein the mass % is based on the total mass of TPO excluding water and ash content. The moisture content may be determined according to ASTM D4928-12R18, and the ash content may be determined according to ASTM D2415-20 (at 550° C.). TPO may have a total nitrogen of less than 0.65% by mass, such as less than 0.60% by mass, or less than 0.55% by mass, wherein the mass % is based on the total mass of TPO excluding water and ash content. Those skilled in the art will understand that any range between any explicitly disclosed lower and upper limits is disclosed herein. Therefore, TPO may have a total nitrogen in the range of 0.40-0.65% by mass, preferably 0.45-0.65% by mass, and more preferably 0.45-0.60% by mass, wherein the mass % is based on the total mass of TPO excluding water and ash content. Total nitrogen is determined according to ASTM D5291C-21.
[0156] According to the present invention, the TPO may have a total sulfur content of at most 1.35 mass%, such as at most 1.30 mass%, or at most 1.25 mass%, or at most 1.20 mass%, or at most 1.15 mass%, or at most 1.10 mass%, wherein the mass% is based on the total mass of the TPO excluding water and ash content. The moisture content may be determined according to ASTM D4928-12R18, and the ash content may be determined according to ASTM D2415-20 (at 550°C). The total sulfur is determined according to ASTM D5291C-21.
[0157] TPO can have:
[0158] Total nitrogen within 0.40-0.65 mass %, preferably 0.45-0.65 mass %, more preferably 0.45-0.60 mass %; and
[0159] Up to 1.35 mass %, preferably up to 1.25 mass %, more preferably up to 1.20 mass % total sulfur;
[0160] Wherein, mass % is based on the total mass of TPO excluding water and ash content. The water content can be measured according to ASTM D4928-12R18, and the ash content can be measured according to ASTM D2415-20 (at 550°C). Total nitrogen and total sulfur are measured according to ASTM D5291C-21.
[0161] According to the present invention, TPO can have the following properties:
[0162] Total carbon in the range of 85.0-90.0 mass %, preferably 86.0-90.0 mass %, more preferably 87.0-90.0 mass %;
[0163] Total hydrogen in the range of 8.0-11.0 mass %, preferably 8.5-10.5 mass %, more preferably 9.0-10.0 mass %;
[0164] a C / H atomic ratio in the range of 0.65-1.0, preferably 0.70-0.90, more preferably 0.70-0.85;
[0165] Total nitrogen within 0.40-0.65 mass %, preferably 0.45-0.65 mass %, more preferably 0.45-0.60 mass %; and
[0166] Up to 1.35 mass %, preferably up to 1.25 mass %, more preferably 0.90-1.20 mass % total sulfur;
[0167] Wherein, mass % is based on the total mass of TPO excluding water and ash content. The water content can be measured according to ASTM D4928-12R18, and the ash content can be measured according to ASTM D2415-20 (at 550°C). The total carbon, total hydrogen, total nitrogen and total sulfur are measured according to ASTM D5291C-21. The C / H atomic ratio is calculated based on the total carbon and total hydrogen.
[0168] According to the present invention, the TPO may have an ash content of less than 0.04 mass %, such as less than 0.03 mass %, or less than 0.02 mass %, or less than 0.01 mass %, wherein the mass % is based on the total mass of the TPO. The ash content is measured according to ASTM D2415-20 (at 550°C).
[0169] The TPO may have a sieve residue of 250 mg / kg or less, for example 230 mg / kg or less, based on the total weight of the TPO. The sieve residue is determined according to ASTM D4870-18 (25 μm mesh size).
[0170] According to the present invention, the carbon black feedstock may further comprise conventional carbon black feedstock, in particular conventional carbon black feedstock for gas black process. Conventional carbon black feedstock may comprise coal tar fractions, residual oil produced in the catalytic cracking process of petroleum fractions, residual oil produced in the process of producing olefins by cracking naphtha or gas oil, or a mixture of any combination of the above feedstocks, preferably comprising coal tar fractions.
[0171] Based on the total weight of the carbon black raw material, the carbon black raw material of the present invention may contain up to 90 wt%, such as up to 85 wt%, or up to 80 wt%, or up to 75 wt%, or up to 70 wt%, or up to 65 wt%, or up to 60 wt%, or up to 55 wt%, or up to 50 wt%, or up to 45 wt%, or up to 40 wt%, or up to 35 wt%, or up to 30 wt%, or up to 25 wt%, or up to 20 wt%, or up to 15 wt%, or up to 10 wt%, or up to 5 wt% of conventional carbon black raw material. Therefore, based on the total weight of the carbon black raw material, the carbon black raw material of the present invention may contain up to 70 wt%, preferably up to 50 wt%, more preferably 30 wt%, and most preferably up to 10 wt% of conventional carbon black raw material.
[0172] According to the present invention, the carbon black feedstock may contain at least 5 wt%, such as at least 10 wt%, or at least 15 wt%, or at least 20 wt%, or at least 25 wt%, or at least 30 wt%, or at least 35 wt%, or at least 40 wt%, or at least 45 wt%, or at least 50 wt%, or at least 55 wt%, or at least 60 wt%, or at least 65 wt%, or at least 70 wt%, or at least 75 wt%, or at least 80 wt%, or at least 85 wt%, or at least 90 wt%, or at least 95 wt%, or at least 99 wt% of rubber derived pyrolysis oil, based on the total weight of the carbon black feedstock. Thus, the carbon black feedstock of the present invention may contain at least 10 wt%, preferably at least 30 wt%, more preferably at least 50 wt%, even more preferably at least 70 wt%, and most preferably at least 90 wt% of rubber derived pyrolysis oil, based on the total weight of the carbon black feedstock. The carbon black feedstock of the present invention may consist of rubber derived pyrolysis oil.
[0173] The present invention further relates to a carbon black obtained by the above-mentioned inventive method. The inventive carbon black obtained by the inventive method may have an oil absorption value (OAN) equal to or greater than 100 mL / 100 g, such as equal to or greater than 105 mL / 100 g, or equal to or greater than 110 mL / 100 g, or equal to or greater than 115 mL / 100 g. Preferably, the inventive carbon black may have an oil absorption value (OAN) equal to or greater than 110 mL / 100 g, more preferably equal to or greater than 115 mL / 100 g. The inventive carbon black may have an oil absorption value (OAN) equal to or less than 180 mL / 100 g, such as equal to or less than 175 mL / 100 g, or equal to or less than 170 mL / 100 g, or equal to or less than 165 mL / 100 g, or equal to or less than 160 mL / 100 g. The carbon black according to the present invention may have an OAN within the range between any stated lower and upper limits. Therefore, the carbon black of the present invention may have an oil absorption value (OAN) in the range of 110 mL / 100 g to 180 mL / 100 g, preferably 110 mL / 100 g to 170 mL / 100 g, more preferably 110 mL / 100 g to 165 mL / 100 g, even more preferably 115 mL / 100 g to 165 mL / 100 g. OAN is measured according to ASTM D2414-21.
[0174] The carbon black of the present invention may have a volatile content of 6% or more, such as 7% or more. The carbon black of the present invention may have a volatile content of 12% or less, such as 11% or less, or 10% or less. The carbon black according to the present invention may have a volatile content in the range between any of the lower and upper limits. Therefore, the carbon black of the present invention may have a volatile content in the range of 6%-12%, preferably 6%-10%, and more preferably 7%-10%. The volatile content (at 950°C) is determined according to DIN 53552:1977-09. The volatile content refers to the carbon black of the present invention that has not been oxidized or functionalized after production. Compared with the gas black process using traditional carbon black raw materials, the process of the present invention can provide carbon black with a higher volatile content. A high volatile content, i.e., a high surface oxide concentration, can reduce the vulcanization rate and improve the flow characteristics of the ink. In addition, the gloss and jetness of paints and coatings containing carbon black with a higher volatile content will also increase. In order to improve the color characteristics of carbon black, the carbon black can be post-treated by oxidation. The method of the present invention can avoid such post-treatment.
[0175] The STSA of the carbon black of the present invention may be equal to or greater than 70 m 2 / g, for example, equal to or greater than 80m 2 / g, or equal to or greater than 90m 2 / g. The STSA of carbon black can be equal to or less than 300m 2 / g, for example, equal to or less than 290m 2 / g, or equal to or less than 270m 2 / g, or equal to or less than 250m 2 / g. The STSA of the carbon black according to the present invention may be within the range between any of the lower limit and the upper limit. Thus, the STSA of the carbon black may be within the range of 70-300 m 2 / g, preferably 70-270m 2 / g, more preferably 80-250m 2 STSA is measured according to ASTM D6556-19a.
[0176] The BET of the carbon black of the present invention may be equal to or greater than 80 m 2 / g, for example, equal to or greater than 90m 2 / g, or equal to or greater than 95m 2 / g. The BET of carbon black can be equal to or less than 350m 2 / g, for example, equal to or less than 320m 2 / g, or equal to or less than 300m 2 / g. The BET of the carbon black according to the present invention may be within the range between any of the lower limit and the upper limit. Therefore, the BET of the carbon black may be in the range of 80-350 m 2 / g, preferably 80-320m 2 / g, more preferably 90-300m 2 STSA is measured according to ASTM D6556-19a.
[0177] The tinting strength of the carbon black of the present invention may be equal to or greater than 30%, such as equal to or greater than 40%, or equal to or greater than 50%. The tinting strength of the carbon black of the present invention may be equal to or less than 250%, such as equal to or less than 230%, or equal to or less than 200%, or equal to or less than 160%. The tinting strength of the carbon black according to the present invention may be within the range between any of the lower and upper limits. Thus, the tinting strength of the carbon black may be within the range of 30%-250%, preferably 40%-200%, and more preferably 50%-160%. The tinting strength is determined according to ASTM D3265-21.
[0178] The pMC (percentage of modern carbon) of the carbon black of the present invention may be 1% or more, for example, 2% or more, or 3% or more, or 4% or more, or 5% or more, or 6% or more, or 7% or more, or 8% or more, or 9% or more, or 10% or more, or 12% or more, or 13% or more, or 14% or more, or 15% or more. The pMC (percentage of modern carbon) of the carbon black of the present invention may be 95% or less, for example, 90% or less, or 80% or less, or 70% or less, or 60% or less, or 55% or less, or 50% or less, or 45% or less. The pMC of the carbon black according to the present invention may be in the range between any of the lower and upper limits. Therefore, the pMC of the carbon black may be in the range of 1%-65%, preferably 5%-60%, more preferably 10%-60%, and most preferably 15%-55%. pMC is determined according to ASTM D6866-20 Method B (AMS). Calculate the pMC of each sample. 14 C / 13 The C ratio was calculated and compared with the measured value of oxalic acid II standard (NIST-4990C). The measured value (pMC) was corrected by d13C measured using an isotope ratio mass spectrometer (IRMS).
[0179] According to the present invention, carbon black can be oxidized. Herein, the term "oxidation" refers to that carbon black is oxidized and therefore contains oxygen-containing functional groups. Therefore, unlike non-oxidized carbon black, oxidized carbon black generally has a significant oxygen content and has oxygen-containing functional groups, such as, but not limited to, quinone groups, carboxyl groups, phenolic groups, lactol groups, lactone groups, anhydride groups, and ketone groups. For example, based on the gross weight of the oxidized carbon black material, the oxygen content of the oxidized carbon black can be more than 0.5 wt %, such as more than 1 wt % or more than 2 wt %. Typically, the oxygen content is no more than 20 wt % based on the gross weight of the oxidized carbon black material. For example, based on the gross weight of the oxidized carbon black material, the oxidized carbon black can contain 0.5-20 wt %, or 1-15 wt %, or 2-10 wt %, or 2-5 wt % of oxygen.
[0180] Oxidized carbon black can be produced by various methods known in the art, such as those disclosed in US Pat. No. 6,120,594 and US Pat. No. 6,471,933. Suitable methods include oxidizing the carbon black material with an oxidizing agent such as a peroxide, such as hydrogen peroxide; a persulfate, such as sodium persulfate and potassium persulfate; a hypochlorite, such as sodium hypochlorite; ozone or oxygen; a transition metal-containing oxidant, such as permanganate, osmium tetroxide, chromium oxide, cerium ammonium nitrate; or an oxidizing acid, such as nitric acid or perchloric acid; and mixtures or combinations thereof.
[0181] According to the present invention, carbon black can also be further functionalized. Carbon black can be functionalized by treatment with a functionalizing agent. As described in WO2021 / 001156A1, functionalized carbon black can be obtained, for example, by treating oxidized carbon black with a sulfur-containing primary or secondary amine or a salt thereof. Thus, the treatment chemically changes the oxidized carbon black by the sulfur-containing amine, which imparts functional groups (e.g., sulfur-containing moieties and / or amine groups) from the treating agent to the oxidized carbon black.
[0182] The invention further relates to the use of the carbon black according to the invention as reinforcing filler or additive, UV stabilizer, conductive carbon black or pigment, preferably as pigment.
[0183] Furthermore, the present invention relates to the use of the carbon black according to the invention in rubber and rubber mixtures, plastics, inks (e.g. printing inks, inkjet inks or other inks), toners, paints, coatings, paper, adhesives, batteries or black matrix applications, preferably in inks (e.g. printing inks, inkjet inks or other inks), toners, paints or coatings, preferably in inks, paints or coatings.
[0184] The present invention further relates to a composition comprising the carbon black of the present invention. The composition of the present invention may be an ink composition, a coating composition or a paint composition.
[0185] Composition of the present invention can further comprise polymer component.Polymer component can comprise thermoplastic polymer, duroplastic (duroplastic) or thermosetting polymer and their mixture or combination.For example, polymer component that can be used for composition of the present invention comprises epoxy resin, acrylic resin, polyurethane, polyester, polycarbonate, polysulfone, polyimide, polyether (for example polyether sulfone) and polyolefin (for example low density polyethylene, medium density polyethylene and high density polyethylene), ethylene-propylene copolymer (random or block configuration), polypropylene-maleic anhydride, polystyrene, styrene-acrylonitrile copolymer, acrylonitrile-butadiene-styrene copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, vinyl chloride-polypropylene copolymer, polyisobutylene, polybutadiene, and crosslinked polyethylene (no matter by chemical, heat, UV or electron beam (EB) crosslinking), polyphenylene sulfide, polyether ether ketone, polyether imide, polyaryl sulfone and polypropylene oxide modified polyether sulfone, or the mixture or combination of above-mentioned any material.
[0186] The composition according to the present invention may optionally further comprise water and / or one or more organic solvents. For example, water and / or organic solvents may be used as dissolving or dispersing media for the polymer component of the present invention and carbon black. For example, the composition according to the present invention may be a liquid composition, such as an aqueous or organic dispersion. The organic solvent may comprise alcohols, ketones, esters, aliphatic or aromatic hydrocarbons or mixtures thereof. The composition according to the present invention may be a powder composition.
[0187] The composition according to the invention may contain 0.1 to 30% by weight, preferably 0.5 to 20% by weight, more preferably 1 to 15% by weight of the carbon black according to the invention, based on the total weight of the composition.
[0188] The present invention further relates to the use of the composition according to the invention in printing and coating applications.
[0189] Furthermore, the present invention relates to an article prepared from the composition of the present invention. The article of the present invention may be a coated article or a colored article or a printed article.
[0190] Example
[0191] The present invention will be further illustrated by the following examples. Unless otherwise specified, all parts and percentages mentioned herein are on a weight basis.
[0192] Carbon Black Production
[0193] Carbon black was produced according to the gas black process as described above using a conventional gas black reactor as shown on page 33 of H. Ferch "Pigmentruβe", 1st edition, Curt R. Vincentz Verlag, Hannover (1995). A procedure similar to that described in Example 1 of US 3,978,019 A was used, except that a rubber-derived pyrolysis oil was used instead of Russoel. ThermoTireOil RR (available from Pyrum Innovations AG (Germany)) was used as rubber-derived pyrolysis oil. ThermoTireOil RR was fractionated. The ThermoTireOil RR distillation fractions having a flash point of at least 65° C. were used. The flash point was determined according to ASTM D93B.
[0194] The properties of carbon black produced by the gas black process using rubber derived pyrolysis oil as the carbon black feedstock were measured and are shown in Table 1.
[0195] Table 1:
[0196] characteristic standard Example 1 OAN[mL / 100g] ASTM D2414-21 132.7 Volatile matter content [%] DIN 53552:1977-09 (at 950°C) 7.1 <![CDATA[STSA[m 2 / g]]]> ASTM D6556-19a 102.7 <![CDATA[BET[m 2 / g]]]> ASTM D6556-19a 116.2 Tinting strength [%] ASTM D3265-21 128.6
[0197] Waterborne and solventborne coating compositions were prepared using the carbon black of Example 1 and the following commercially available gas black (obtained using conventional raw materials).
[0198] U: OAN value is 115mL / 100g, volatile content is 5%, BET value is 92m 2 / g of gas black, available from Orion Engineered Carbons GmbH.
[0199] Colour Black S160: OAN value is 128mL / 100g, volatile content is 5%, BET value is 180m 2 / g of gas black, available from Orion Engineered Carbons GmbH.
[0200] Preparation of waterborne coating compositions ("reference waterborne coating systems")
[0201] a) Preparation of aqueous dispersions of various carbon blacks:
[0202] Aqueous dispersions of various carbon blacks were prepared as shown in Table 2.
[0203] Table 2:
[0204]
[0205] 1 Nonionic wetting and dispersing additive (available from Evonik Operations GmbH (Germany))
[0206] 2 Organic polymer, silicone-free defoamer containing fumed silica (available from Evonik Operations GmbH (Germany))
[0207] In a Skandex dispersion beaker (180 mL, 5.3 cm in diameter, 12.5 cm in height) add Dispers 760W and deionized water, stirring with a spatula. Add Foamex 830 and stir the mixture with a spatula. Add the respective carbon black and stir the mixture with a spatula until the carbon black is completely wet. Then, disperse with a Pendraulik LR 34 dissolver for 5 minutes using a dispersing disk with a diameter of 40 mm at a speed of 4000 rpm. Measure the pH of the dispersion. If the pH of the dispersion is below the required range of 8.5-9.2, adjust the pH with DMEA. Use 540 g of chrome steel balls with a diameter of 3 mm and use a Skandex disperser DAS 200 for 60 minutes of dispersion with colling on the 2nd level. Subsequently, filter out the steel balls and measure the pH of the dispersion. If the pH of the dispersion is below the required range of 8.2-8.7, adjust the pH with DMEA (50 wt. % aqueous solution).
[0208] b) Preparation of Reference Paint A:
[0209] Reference paint A was prepared as shown in Table 3.
[0210] Table 3:
[0211]
[0212]
[0213] 1 Solvent-free aliphatic polyester polyurethane dispersion (available from Alberdingk Boley GmbH (Germany))
[0214] 2 VOC-free silicone defoamer (available from BYK-Chemie GmbH (Germany))
[0215] 3 Liquid polyether siloxane copolymer (available from Evonik Operations GmbH (Germany))
[0216] Will U 9800 was added to the container and stirred with a Pendraulik LR 34 dissolver. Butanediol, WET 280, DMEA and deionized water were premixed and added U 9800. The mixture was dispersed using a dispersion disk with a diameter of 40 mm at a rotation speed of 1000 rpm. Subsequently, the mixture was homogenized at 1500 rpm for 5 minutes. After the reference paint was prepared, the reference paint was left to stand overnight.
[0217] The quality of the reference paint A was controlled by applying the reference paint A on a glass plate (130×90×1 mm) and drawing down the reference paint A with a film drawing bar with a slot height of 200 μm under wet conditions with uniform tension and pressure. Care was taken to ensure that there were no bubbles in the stripe of the reference paint A. The drawdown bar was placed on the stripe of the reference paint A and drawn down evenly on the plate. A drawdown of approximately 10 cm in length and 6 cm in width was produced.
[0218] After the knife coating step was completed, the wet coating film on the glass plate was flashed off at room temperature (20° C.) for 15 minutes, and then the coated glass plate was dried at 60° C. for 15 minutes.
[0219] The coatings prepared from Reference Paint A were inspected for defects such as pits, spots and irregularities. In cases where a large number of defects were present, the reference paint was re-prepared for use in formulating the coating compositions described subsequently.
[0220] c) Preparation of waterborne coating composition
[0221] According to the formulation of Table 4 below, waterborne coating compositions were prepared using Reference Paint A and aqueous dispersions of various carbon blacks (Table 2).
[0222] Table 4:
[0223]
[0224] The aqueous dispersions prepared from the various carbon blacks and the reference paint A were weighed according to the above amounts, added into a 80 mL beaker, and vigorously homogenized with a spatula until uniform, to obtain the corresponding aqueous coating composition.
[0225] Preparation of solvent-based coating compositions
[0226] a) Preparation of solvent dispersions from various carbon blacks:
[0227] Solvent-based dispersions of various carbon blacks were prepared as shown in Table 5 below.
[0228] Table 5:
[0229]
[0230] 1 Short oil alkyd resin based on saturated fatty acids (available from Allnex (Germany))
[0231] 2 Solvent (available from Kremer Pigmente GmbH (Germany))
[0232] In a Skandex dispersion beaker (180 mL, 5.3 cm in diameter, 12.5 cm in height) add F 310SN and A and homogenize vigorously with a spatula. Add the corresponding carbon black and stir the mixture with a spatula until the carbon black is completely wet. Subsequently, disperse with a Pendraulik LR 34 dissolver at 4000 rpm using a dispersing disk with a diameter of 40 mm for 5 minutes. Use 550 g of steel balls with a diameter of 2 mm and disperse with a Skandex disperser DAS200 for 60 minutes while finishing on the 2nd level. Subsequently, filter out the steel balls.
[0233] b) Preparation of solvent-based coating composition:
[0234] A solvent-based coating composition was prepared from the obtained solvent-based dispersion according to the following formulation (see Table 6).
[0235] Table 6:
[0236]
[0237] 1 Short oil alkyd resin based on saturated fatty acids (available from Allnex (Germany))
[0238] 2 Isobutylated melamine formaldehyde resin (available from Prefere Resins (Germany))
[0239] 3 Solvent mixture, consisting of 545.5 g of xylene, 109.1 g of 1-ethoxy-2-propanol, 72.7 g of butanol; 36.4 g of - coating additive OL 17 (10% in xylene) (available from OM Group, Inc. (USA)); and 36.4 g of butylene acetate.
[0240] The ingredients were weighed into a 180 mL beaker according to the indicated amounts and homogenized vigorously with a spatula for 10 minutes to obtain the corresponding solvent-based coating composition.
[0241] Preparation of thin films from coating compositions
[0242] Thin films were prepared from the waterborne coating composition and the solventborne coating composition as follows.
[0243] The corresponding coating composition is applied to a glass plate (130×90×1 mm) and then scraped with a scraper bar having a slit height of 200 μm (in the case of waterborne coating compositions) or 100 μm (in the case of solventborne coating compositions) under wet conditions with uniform tension and pressure. Care is taken to ensure that there are no bubbles in the stripes of the coating composition. The scraper bar is placed on the stripes of the coating composition and scraped evenly over the plate. A scrape sample of about 10 cm in length and about 6 cm in width is produced.
[0244] After the knife coating step was completed, the wet coating film obtained on the glass plate was flashed at room temperature (20° C.) for 15 minutes, and then the coated glass plate was dried at 130° C. for 15 minutes (in the case of a solvent-based coating composition), and the wet coating film obtained on the glass plate was flashed at room temperature (20° C.) for 15 minutes and then dried at 60° C. for 15 minutes (in the case of an aqueous coating composition).
[0245] The coating composition thus prepared was analyzed for its coloring properties.
[0246] The coloration properties of films obtained from waterborne and solventborne coating compositions were measured using a Pausch Q-Color 35 spectrophotometer (45° / 0° spectrophotometer) and BCSWIN software. The measurements were performed through glass after calibration using a white calibration tile and a black hollow body. The spectrophotometer averaged five measurements for each sample.
[0247] Black value M is independent of hue Y and the blackness value M related to the hue c It is calculated based on the tristimulus (XYZ) data measured as follows:
[0248] Black value M is independent of hue Y It is calculated according to formula 1 based on the three primary color components Y measured (light source D65 / 10°):
[0249]
[0250] Then, the blackness value related to the hue is calculated according to Formula 2:
[0251]
[0252] Among them, based on illuminance and observer (DIN5033 / Part 7 / Illuminance D65 / 10°), X n / Z n / Y n (DIN6147) is the three primary color value of the coordinate origin, where
[0253] Xn =94.81Z n =107.34Y n =100.0.
[0254] According to formula 3, the black value M c and M Y The absolute hue contribution dM is calculated:
[0255] dM=M c -M Y (3).
[0256] Haze and gloss 20° were determined according to DIN EN ISO 2813:2015.
[0257] To determine the relative tinting strength, a white pigment (TiO 2 ) and a coating composition of an aqueous or solvent-based dispersion of a corresponding carbon black.
[0258] Preparation of waterborne coating compositions
[0259] a) Preparation of Reference Paint B:
[0260] Reference Paint B was prepared as shown in Table 7 below.
[0261] Table 7:
[0262]
[0263] 1 Nonionic wetting and dispersing additive (available from Evonik Operations GmbH (Germany))
[0264] 2 VOC-free silicone defoamer (available from BYK-Chemie GmbH (Germany))
[0265] 3 Titanium dioxide pigment (available from Kronos Incorporated (USA))
[0266] 4 Solvent-free aliphatic polyester polyurethane dispersion (available from Alberdingk Boley GmbH (Germany))
[0267] Add in a dispersion beaker (850 mL) Dispers 760W and Use a spatula to homogenize vigorously. Add 5g of butanediol and DMEA and use a spatula to homogenize the mixture vigorously. 2064, stir the mixture with a spatula until 2064 was completely wetted. Subsequently, the dispersion was carried out with a Pendraulik LR 34 dissolver at 4000 rpm using a dispersing disk with a diameter of 60 mm for 5 minutes. The dissolver was covered with aluminum foil to prevent the solvent from evaporating. The beaker was then checked for attached pigment agglomerates with a spatula. The dispersion was cooled to a maximum of 30°C.
[0268] Will U 9800 was added to the container. 33.7 g of butanediol and deionized water were premixed and added U 9800, using a dispersion disc with a diameter of 60 mm at a speed of 1000 rpm to disperse the mixture. Subsequently, the mixture was homogenized at a speed of 1000 rpm for 5 minutes. The mixture thus prepared was added to the Dispers760W, Butanediol, DMEA and 2064, a dispersion disc with a diameter of 60 mm was used to disperse the mixture at a speed of 1000 rpm. Subsequently, the mixture was homogenized at a speed of 2000 rpm for 5 minutes. The pH value of the dispersion was measured. If the pH value of the dispersion was lower than the required range of 8.5-9.0, DMEA was used to adjust the pH value. After the reference paint B was prepared, it was left overnight.
[0269] The reference paint B was applied on a glass plate (130×90×1 mm) and the reference paint B was scraped with a slit height of 200 μm under wet conditions with uniform tension and pressure to control the quality of the reference white paint B. Care was taken to ensure that there were no bubbles in the stripes of the reference paint B. The scraping bar was placed on the stripes of the reference paint B and scraped evenly on the plate. A scraping sample of about 10 cm in length and 6 cm in width was produced.
[0270] After the knife coating step was completed, the wet coating film on the glass plate was flashed at room temperature (20° C.) for 15 minutes, and then the coated glass plate was dried at 60° C. for 15 minutes.
[0271] The coatings prepared from Reference Paint B were inspected for defects such as pits, spots and irregularities. In cases where a large number of defects were present, the reference paint was re-prepared for use in formulating the coating compositions described subsequently.
[0272] b) Preparation of waterborne coating composition
[0273] Aqueous coating compositions were prepared from Reference Paint B and the aqueous dispersion of Table 2 according to the formulation of Table 8 below.
[0274] Table 8:
[0275]
[0276] The aqueous dispersions prepared from each carbon black and the reference paint B were weighed according to the above amounts, added to a beaker, and vigorously homogenized with an enamel paint brush. Subsequently, the mixture was homogenized for 2 minutes at a speed of 2000 rpm using a speed mixer.
[0277] Preparation of solvent-based coating compositions
[0278] a) Preparation of Reference Paint C:
[0279] Reference paint C was produced as shown in Table 9 below:
[0280] Table 9:
[0281]
[0282] 1 Short oil alkyd resin based on saturated fatty acids (available from Allnex (Germany))
[0283] 2 Titanium dioxide pigment (available from Kronos Incorporated (USA))
[0284] 3 Isobutylated melamine formaldehyde resin (available from Prefere Resins (Germany))
[0285] In a dispersion beaker (180 mL), add 60.0 g of F 310SN. Join 2301, and vigorously homogenize the mixture with a spatula until the Kronos 2310 is completely wetted. Subsequently, disperse with a Pendraulik LR 34 dissolver at 4000 rpm for 5 minutes using a dispersing disk with a diameter of 40 mm. Check the beaker for attached pigment agglomerates with a spatula. Disperse further for 10 minutes using a Pendraulik LR 34 dissolver at 4000 rpm using a dispersing disk with a diameter of 40 mm. The dissolver is covered with aluminum foil to prevent the solvent from evaporating. The dispersion is cooled to a maximum of 30°C.
[0286] Add 7.35 g of F310SN, MF800 / 55IB and xylene were added and homogenized with a spatula. Then, a dispersing disk with a diameter of 40 mm was used to disperse the mixture at a speed of 1500 rpm for 5 minutes using a Pendraulik LR 34 dissolver.
[0287] b) Preparation of solvent-based coating composition
[0288] A solventborne coating composition was prepared from Reference Paint C and the solventborne dispersion of Table 5 according to the formulation of Table 10 below.
[0289] Table 10:
[0290]
[0291] The aqueous dispersions prepared from the respective carbon blacks and the reference paint B were weighed in the above amounts, added to a beaker, and vigorously homogenized with a scraper and then with a rubber wiper.
[0292] Preparation of thin films from coating compositions
[0293] Thin films were prepared from the waterborne coating composition and the solventborne coating composition as follows.
[0294] The corresponding coating composition is applied to a glass plate (130×90×1 mm) and then scraped with a scraper bar with a slit height of 150 μm under wet conditions with uniform tension and pressure. Care is taken to ensure that there are no bubbles in the stripes of the coating composition. The scraper bar is placed on the stripes of the coating composition and scraped evenly on the plate. A scrape sample of about 10 cm in length and about 6 cm in width is produced.
[0295] After the knife coating step was completed, the wet coating film obtained on the glass plate was flashed at room temperature (20°C) for 15 minutes, and then the coated glass plate was dried at 130°C for 15 minutes (in the case of a solvent-based coating composition); the wet coating film obtained on the glass plate was flashed at room temperature (20°C) for 15 minutes and then dried at 60°C for 15 minutes (in the case of an aqueous coating composition).
[0296] The coating compositions thus prepared were subjected to a relative tinting strength analysis. The relative tinting strength was determined in accordance with DIN EN ISO 787-24:1995-10.
[0297] Table 11 summarizes the tinting performance results for waterborne coating compositions containing carbon black, and Table 12 summarizes the tinting performance results for solventborne coating compositions.
[0298] Table 11: Waterborne coating composition
[0299]
[0300]
[0301] Table 12: Solvent-based coating compositions
[0302]
Claims
1. A method for producing carbon black by thermal oxidative decomposition of a carbon black feedstock, wherein the carbon black feedstock comprises rubber-derived pyrolysis oil, and wherein the production of the carbon black is carried out in a gas black reactor.
2. The method of claim 1, wherein the rubber derived pyrolysis oil comprises tire derived pyrolysis oil (TPO).
3. The method according to claim 1 or 2, wherein the rubber derived pyrolysis oil consists of tire derived pyrolysis oil (TPO).
4. The method according to any one of the preceding claims, wherein the rubber derived pyrolysis oil has: Total carbon in the range of 80.0 mass % to 90.0 mass %; Total hydrogen in the range of 8.0 mass % to 15.0 mass %; and a C / H atomic ratio in the range of 0.60 to 1.0; in, The mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and wherein the total carbon and the total hydrogen are determined according to ASTM D5291C-21; and / or The rubber-derived pyrolysis oil has Up to 1.00 mass % total nitrogen; and Up to 1.35 mass % total sulfur, wherein the mass % is based on the total mass of the rubber derived pyrolysis oil excluding water and ash content, and wherein the total nitrogen and the total sulfur are determined according to ASTM D5291C-21.
5. The method according to any one of claims 2 to 4, wherein the tire derived pyrolysis oil (TPO) has Total carbon in the range of 85.0 mass % to 90.0 mass %; Total hydrogen in the range of 8.0 mass % to 11.0 mass %; and C / H ratio in the range of 0.65 to 1.0; in, The mass % is based on the total mass of the TPO excluding water and ash content, and wherein the total carbon and the total hydrogen are determined according to ASTM D5291C-21.
6. The method according to any one of the preceding claims, wherein the carbon black feedstock further comprises a conventional carbon black feedstock, the conventional carbon black feedstock comprising a coal tar fraction, a residual oil produced during the catalytic cracking of a petroleum fraction, a residual oil produced during the production of olefins by cracking naphtha or gas oil, or a mixture of any combination of the foregoing, preferably a coal tar fraction.
7. The process according to any one of the preceding claims, wherein the carbon black feedstock comprises at least 10 wt. %, preferably at least 30 wt. %, more preferably at least 50 wt. %, even more preferably at least 70 wt. %, most preferably at least 90 wt. % of the rubber derived pyrolysis oil, based on the total weight of the carbon black feedstock, or The carbon black raw material is composed of the rubber-derived pyrolysis oil.
8. A method according to any one of the preceding claims, comprising gasifying the carbon black raw material in a carrier gas stream, Combusting a carrier gas stream loaded with a carbon black feedstock in a burner in the presence of air to form carbon black, and terminate the formation of the carbon black.
9. Carbon black obtainable according to the process of any one of the preceding claims, wherein the carbon black is gas black.
10. The carbon black according to claim 9, wherein the carbon black has Oil Absorption Number (OAN) equal to or greater than 110 mL / 100 g; and / or A volatile matter content equal to or greater than 6%; The OAN is measured according to ASTM D2414-21, and the volatile content (at 950° C.) is measured according to DIN 53552:1977-09.
11. The carbon black according to claim 9 or 10, wherein the carbon black has at least one, more than one or all of the following characteristics: OAN in the range of 110 mL / 100 g to 180 mL / 100 g, preferably 115 mL / 100 g to 165 mL / 100 g; wherein the OAN is determined according to ASTM D2414-21; A volatile content in the range of 6% to 25%; wherein the volatile content (at 950° C.) is determined according to DIN 53552:1977-09; At 70m 2 / g to 300m 2 / g, preferably 70m 2 / g to 270m 2 / g, more preferably 80m 2 / g to 250m 2 / g range; wherein the STSA is determined according to ASTM D6556-19a; At 80m 2 / g to 350m 2 / g, preferably 80m 2 / g to 320m 2 / g, more preferably 90m 2 / g to 300m 2 / g range; wherein the BET specific surface area is measured according to ASTM D6556-19a, a tinting strength ranging from 30% to 250%, preferably from 50% to 160%; Where sulfur content is determined according to ASTM D3265-21, and A pMC (percent modern carbon) in the range of 1% to 65%, preferably 5% to 60%, more preferably 10% to 60%, even more preferably 15% to 55%, wherein the pMC is determined according to ASTM D6866-20 Method B (AMS).
12. Use of the carbon black according to any one of claims 9 to 11 as reinforcing filler or additive, UV stabilizer, conductive carbon black or pigment, preferably as pigment.
13. Use of the carbon black according to any one of claims 9 to 11 in rubber and rubber mixtures, plastics, inks, such as printing inks, inkjet inks or other inks, toners, paints, coatings, paper, adhesives, batteries or black matrix applications, preferably in inks, paints or coatings.
14. A composition comprising the carbon black according to any one of claims 9 to 11, wherein the composition is preferably an ink composition, a coating composition or a paint composition.
15. An article prepared from the composition according to claim 14.