Powder coating material, coating film, and article

By adjusting the composition of the copolymer, powder coatings containing specific PPVE and TFE units were prepared, which solved the problem of insufficient wear resistance and tensile creep resistance of the coating film in the prior art, and achieved high-performance coating film Preparation has excellent water vapor and liquid permeability and durability.

CN118900904APending Publication Date: 2024-11-05DAIKIN INDUSTRIES LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380028922.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-26
Filing Date
2023-03-30
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing powder coatings have shortcomings in wear resistance, low water vapor permeability, low permeability of the pharmaceutical liquid and tensile creep resistance, and it is difficult to simultaneously improve the durability and stability of the coating film.

Method used

By adjusting the content, melt flow rate and number of functional groups in the copolymer, the content of tetrafluoroethylene (TFE) and perfluoropropyl vinyl ether (PPVE) units, the melt flow rate and the number of functional groups, the PPVE were prepared, and 5.0 to 6.2% PPVE, 20.0 to 35.0 g/10 minutes. A copolymer of melt flow rate and 100 or less functional groups are used to prepare powder coatings.

Benefits of technology

It has achieved a coating film with excellent wear resistance of 60°C, low permeability of water vapor, low permeability of medicine liquid and tensile creep resistance of 230°C, which can maintain low permeability for a long time and protect the coated object. Moreover, the coating film has good wear resistance and shape stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005051316070000051
    Figure BDA0005051316070000051
  • Figure BDA0005051316070000121
    Figure BDA0005051316070000121
  • Figure BDA0005051316070000141
    Figure BDA0005051316070000141
Patent Text Reader

Abstract

Provided is a powder coating material which contains a copolymer that contains tetrafluoroethylene units and perfluoro (propyl vinyl ether) units, the content of the perfluoro (propyl vinyl ether) units in the copolymer being 5.0-6.2 mass% with respect to the total monomer units, the melt flow rate of the copolymer at 372 DEG C being 20.0-35.0 g / 10 minutes, and the melt flow rate of the copolymer at 372 DEG C being 20.0-35.0 g / 10 minutes. The number of functional groups in the copolymer is 100 or less per 106 main chain carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to powder coating, coating film and articles. Background Art

[0002] Patent document 1 records a powder coating, which is a powder coating containing a tetrafluoroethylene copolymer, characterized in that the above-mentioned tetrafluoroethylene copolymer is a copolymer of 5 to 25 mass% of hexafluoropropylene and 0.01 to 5 mass% of perfluoro(vinyl ether) and tetrafluoroethylene, and the melt flow rate is 1 to 30 g / 10 minutes.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2003 / 006566 Summary of the invention

[0006] Problems to be solved by the invention

[0007] An object of the present invention is to provide a powder coating material capable of obtaining a coating film having excellent abrasion resistance at 60°C, low water vapor permeability, low chemical liquid permeability, tensile creep resistance at 230°C, and durability against tensile force applied at 180°C.

[0008] Means for solving problems

[0009] According to the present invention, a powder coating is provided, which contains a copolymer, the copolymer contains tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, wherein the content of the perfluoro(propyl vinyl ether) units in the copolymer is 5.0 to 6.2% by mass relative to all monomer units, the melt flow rate of the copolymer at 372° C. is 20.0 to 35.0 g / 10 minutes, and the number of functional groups of the copolymer is 10 6 The number of carbon atoms in the main chain is 100 or less.

[0010] Effects of the Invention

[0011] According to the present invention, a powder coating material can be provided which can obtain a coating film having excellent 60°C abrasion resistance, low water vapor permeability, low chemical liquid permeability, 230°C tensile creep resistance, and durability against tensile force applied at 180°C. DETAILED DESCRIPTION

[0012] The specific embodiments of the present invention are described in detail below, but the present invention is not limited to the following embodiments.

[0013] The powder coating material of the present invention contains a copolymer comprising tetrafluoroethylene (TFE) units and perfluoro(propyl vinyl ether) (PPVE) units.

[0014] Conventionally, a copolymer (PFA) containing TFE units and PPVE units has been used as a component of a powder coating. Patent Document 1 discloses a powder coating that can obtain a coating film having excellent surface smoothness and excellent durability against chemicals, etc. The powder coating contains a tetrafluoroethylene-based copolymer, which is a copolymer of 5 to 25% by mass of hexafluoropropylene and 0.01 to 5% by mass of perfluoro(vinyl ether) with tetrafluoroethylene, and has a melt flow rate of 1 to 30 g / 10 minutes.

[0015] However, the conventional powder coating described in Patent Document 1 has the problem that the abrasion resistance, durability to tensile force, and low permeability to chemical liquid of the obtained coating film are insufficient. In-depth research has been conducted on means for solving such problems, and the results show that it is not easy to simultaneously improve the abrasion resistance and durability to tensile force of the obtained coating film, and the low permeability to water vapor, low permeability to chemical liquid, and 230°C tensile creep resistance of the obtained coating film.

[0016] It was found that by appropriately adjusting the PPVE unit content, melt flow rate (MFR) and number of functional groups of a copolymer containing TFE units and PPVE units of the copolymer, a coating film having excellent 60°C wear resistance, low water vapor permeability, low chemical liquid permeability, 230°C tensile creep resistance, and durability against tensile force applied at 180°C can be obtained by using such a copolymer as a powder coating. Therefore, for example, when a coating film is formed by applying the powder coating of the present invention to a coated object, a beautiful coating film can be easily formed on the coated object. Furthermore, not only can water vapor or chemical liquid be suppressed from penetrating the coating film to reach the coated object, but the coating film also has excellent wear resistance and shape stability, so such low permeability can be maintained for a long time, and thus the coated object can be protected for a long time.

[0017] The copolymer contained in the powder coating material of the present invention is a melt-processable fluororesin. Melt-processability means that the polymer can be melted and processed using existing processing equipment such as an extruder and an injection molding machine.

[0018] The content of the PPVE unit in the copolymer is 5.0 to 6.2% by mass relative to all monomer units. The content of the PPVE unit in the copolymer is preferably 5.1% by mass or more, preferably 6.1% by mass or less, more preferably 6.0% by mass or less, further preferably 5.8% by mass or less, and particularly preferably 5.7% by mass or less. If the content of the PPVE unit in the copolymer is too much, the low water vapor permeability, low drug liquid permeability, and 230°C tensile creep resistance will be poor. If the content of the PPVE unit in the copolymer is too little, the 60°C wear resistance and the durability to the tensile force applied at 180°C will be poor.

[0019] The content of the TFE unit in the copolymer is preferably 93.8% by mass or more, more preferably 93.9% by mass or more, further preferably 94.0% by mass or more, further preferably 94.2% by mass or more, particularly preferably 94.3% by mass or more, and preferably 95.0% by mass or less, more preferably 94.9% by mass or less. If the content of the TFE unit in the copolymer is too small, low water vapor permeability, low drug liquid permeability, and 230°C tensile creep resistance may be poor. If the content of the TFE unit in the copolymer is too large, 60°C abrasion resistance and durability against tensile force applied at 180°C may be poor.

[0020] In the present invention, the content of each monomer unit in the copolymer is determined by 19 Determined by F-NMR method.

[0021] The copolymer may also contain monomer units derived from monomers copolymerizable with TFE and PPVE. In this case, the content of the monomer units copolymerizable with TFE and PPVE is preferably 0 to 1.2% by mass, more preferably 0.05 to 0.5% by mass, and further preferably 0.1 to 0.3% by mass relative to all monomer units of the copolymer. The content of the monomer units copolymerizable with TFE and PPVE may be 0.1% by mass or less relative to all monomer units of the copolymer.

[0022] Examples of monomers copolymerizable with TFE and PPVE include hexafluoropropylene (HFP), CZ 1 Z 2 =CZ 3 (CF 2 ) n Z 4 (Where Z 1 , Z 2 and Z 3 Same or different, means H or F, Z 4 represents H, F or Cl, and n represents an integer of 2 to 10. ) represents a vinyl monomer, CF 2 =CF-ORf 1 (Where Rf 1 Perfluoro(alkyl vinyl ether) [PAVE] (excluding PPVE) represented by a perfluoroalkyl group having 1 to 8 carbon atoms, and CF 2 =CF-OCH 2 -Rf 1 (Where Rf 1 represents a perfluoroalkyl group having 1 to 5 carbon atoms. ) and the like. Among them, HFP is preferred.

[0023] The copolymer is preferably at least one selected from the group consisting of a copolymer consisting only of a TFE unit and a PPVE unit and a TFE / HFP / PPVE copolymer, and more preferably a copolymer consisting only of a TFE unit and a PPVE unit.

[0024] The melt flow rate (MFR) of the copolymer is 20.0 to 35.0 g / 10 minutes. The MFR of the copolymer is preferably 21.0 g / 10 minutes or more, more preferably 22.0 g / 10 minutes or more, and further preferably 23.0 g / 10 minutes or more, preferably 34.0 g / 10 minutes or less, more preferably 33.0 g / 10 minutes or less, and further preferably 32.0 g / 10 minutes or less. If the MFR of the copolymer is too high, the wear resistance at 60°C and the durability to the tensile force applied at 180°C will be poor. If the MFR of the copolymer is too low, the low water vapor permeability and the low drug liquid permeability will be poor.

[0025] In the present invention, MFR is a value obtained as the mass (g / 10 minutes) of a polymer flowing out from a nozzle having an inner diameter of 2.1 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes using a melt flow indexer in accordance with ASTM D1238.

[0026] The MFR can be adjusted by adjusting the type and amount of the polymerization initiator, the type and amount of the chain transfer agent, etc., used when polymerizing the monomers.

[0027] Each 10 6 The number of functional groups per main chain carbon atom is 100 or less. 6 The number of functional groups per main chain carbon atom is preferably 80 or less, more preferably 70 or less, further preferably 60 or less, further preferably 50 or less, particularly further preferably 40 or less, particularly preferably 30 or less, and most preferably less than 20. If the number of functional groups is too large, a molded body having low permeability to chemical solutions and excellent 230° C. tensile creep resistance cannot be obtained.

[0028] The identification of the types of the functional groups and the measurement of the number of the functional groups can be performed using infrared spectroscopy.

[0029] The number of functional groups is specifically determined by the following method. First, the copolymer is formed by cold pressing to produce a film with a thickness of 0.25 mm to 0.30 mm. The film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the copolymer and a differential spectrum from a background spectrum of complete fluorination without the presence of functional groups. The number of functional groups per 1×10 6 The number of functional groups N per carbon atom.

[0030] N=I×K / t(A)

[0031] I: Absorbance

[0032] K: Correction coefficient

[0033] t: film thickness (mm)

[0034] For reference, absorption frequencies, molar absorption coefficients, and correction coefficients for some functional groups are shown in Table 1. The molar absorption coefficients were determined from FT-IR measurement data of low-molecular model compounds.

[0035] [Table 1]

[0036] Table 1

[0037]

[0038] -CH 2 CF 2 H, -CH 2 COF, -CH 2 COOH, -CH 2 COOCH 3 、-CH 2 CONH 2 The absorption frequency ratios are shown in Table -CF 2 H, -COF, free -COOH and bonded -COOH, -COOCH 3 、-CONH 2 The absorption frequency is several tens of cm lower. -1 ).

[0039] For example, the functional group number of -COF refers to the number of functional groups derived from -CF 2 The absorption frequency of COF is 1883 cm -1 The number of functional groups obtained from the absorption peak at -CH 2 The absorption frequency of COF is 1840 cm -1 The total number of functional groups found from the absorption peak at .

[0040] The functional groups are the functional groups present at the ends of the main chain or the side chains of the copolymer and the functional groups present in the main chain or the side chains. The number of functional groups can be -CF=CF 2 , -CF 2 H, -COF, -COOH, -COOCH 3 、-CONH 2 and -CH 2 The total number of OH.

[0041] The functional groups are introduced into the copolymer by, for example, a chain transfer agent or a polymerization initiator used when producing the copolymer. For example, alcohol is used as a chain transfer agent, or a -CH 2 When the peroxide with OH structure is used as the polymerization initiator, -CH 2 OH is introduced into the main chain terminal of the copolymer. In addition, by polymerizing a monomer having a functional group, the above functional group is introduced into the side chain terminal of the copolymer.

[0042] By fluorinating the copolymer having such functional groups, a copolymer having the number of functional groups within the above range can be obtained. That is, the copolymer is preferably fluorinated. The copolymer also preferably has -CF 3 Terminal group.

[0043] The melting point of the copolymer is preferably 295 to 315° C., more preferably 298° C. or higher, further preferably 300° C. or higher, particularly preferably 301° C. or higher, most preferably 302° C. or higher, and more preferably 308° C. or lower. When the melting point is within the above range, a copolymer can be obtained that can provide a coating film that is particularly excellent in 60° C. abrasion resistance, low water vapor permeability, low chemical liquid permeability, 230° C. tensile creep resistance, and durability against a tensile force applied at 180° C.

[0044] In the present invention, the melting point can be measured using a differential scanning calorimeter [DSC].

[0045] The average particle size of the powder coating (copolymer particles) of the present invention is preferably 10 to 1000 μm. When the average particle size is within the above range, the powder coating can be easily applied and a smooth coating film can be obtained. The average particle size is the median diameter and can be measured using a laser diffraction particle size distribution measuring machine.

[0046] The apparent density of the powder coating material of the present invention is preferably 0.5 to 1.2 g / ml. The apparent density can be measured according to JIS K6891.

[0047] The powder coating of the present invention may also contain other resins other than the above-mentioned copolymer. As other resins, generally, as long as they can be used for powder coatings, there is no particular limitation, and they may be any of thermoplastic resins and thermosetting resins. The above-mentioned other resins are preferably heat-resistant resins. As the above-mentioned heat-resistant resins, for example, fluororesins, silicone resins, fluorosilicone resins, polyamide resins, polyamideimide resins, polyimide resins, polyester resins, epoxy resins, polyphenylene sulfide resins, phenol resins, acrylic resins, polyether sulfone resins, etc. other than the above-mentioned copolymers may be cited. One or more of the above-mentioned other resins may be used.

[0048] The powder coating of the present invention may contain additives. As additives, there are no particular limitations as long as they are substances added to general powder coatings, and examples thereof include coloring pigments such as titanium oxide and cobalt oxide for coloring; other pigments such as rust-proof pigments and burnt pigments for rust prevention; fillers such as carbon fibers, glass fibers, glass flakes, and mica for reducing the shrinkage of the coating film and improving the scratch resistance in order to increase the hardness of the coating film; and conductive carbon and other conductive materials for imparting conductivity. The above-mentioned additives may also be leveling agents, antistatic agents, ultraviolet absorbers, free radical supplements, and the like.

[0049] The powder coating material of the present invention can be produced, for example, by a production method in which a copolymer is produced and then treated to obtain a powder having a desired shape.

[0050] The copolymer can be produced by a polymerization method such as suspension polymerization, solution polymerization, emulsion polymerization, bulk polymerization, etc. As the polymerization method, emulsion polymerization or suspension polymerization is preferred. In these polymerizations, various conditions such as temperature and pressure, polymerization initiator, and other additives can be appropriately set according to the composition and amount of the copolymer.

[0051] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical polymerization initiator can be used.

[0052] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, and the following may be cited as representative examples:

[0053] Dialkyl peroxydicarbonates such as di-n-propyl peroxydicarbonate, di-isopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate and di-2-ethoxyethyl peroxydicarbonate;

[0054] Peroxyesters such as tert-butyl peroxyisobutyrate and tert-butyl peroxypivalate;

[0055] Dialkyl peroxides such as di-tert-butyl peroxide;

[0056] Di[fluoro(or chlorofluoro)acyl]peroxides; etc.

[0057] Examples of di[fluoro(or chlorofluoro)acyl]peroxides include [(RfCOO)-] 2 (Rf is a perfluoroalkyl group, an ω-hydroperfluoroalkyl group or a fluorochloroalkyl group).

[0058] Examples of the di[fluoro(or chlorofluoro)acyl]peroxides include di(ω-hydro-dodecafluoroheptanoyl)peroxide, di(ω-hydro-tetrafluorooctanoyl)peroxide, di(ω-hydro-hexafluorononanoyl)peroxide, di(perfluoropropionyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluoropentanoyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, di(ω-chloro-hexafluorobutyryl)peroxide, di(perfluorohexanoyl ... (ω-chloro-decafluorohexanoyl) peroxide, bis(ω-chloro-tetrafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-perfluorobutyryl-peroxide, bis(dichloropentafluorobutyryl) peroxide, bis(trichlorooctafluorohexanoyl) peroxide, bis(tetrachloroundecanoyl) peroxide, bis(pentachlorotetrafluorodecanoyl) peroxide, bis(undecachlorotriacontafluorodocosanoyl) peroxide, and the like.

[0059] The water-soluble free radical polymerization initiator may be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., organic peroxides such as disuccinic acid peroxide and diglutaric acid peroxide, tert-butyl permaleate, tert-butyl hydroperoxide, etc. A reducing agent such as sulfite may be used in combination with the peroxide, and the amount used may be 0.1 to 20 times that of the peroxide.

[0060] A surfactant, a chain transfer agent, and a solvent may be used in the polymerization, and conventionally known surfactants may be used.

[0061] As the surfactant, known surfactants can be used, such as nonionic surfactants, anionic surfactants, cationic surfactants, etc. Among them, fluorinated anionic surfactants are preferred, and more preferred are fluorinated anionic surfactants that may contain ether-bonded oxygen (i.e., oxygen atoms may be inserted between carbon atoms) and have a linear or branched carbon number of 4 to 20. The amount of surfactant added (relative to polymerization water) is preferably 50 to 5000 ppm.

[0062] Examples of chain transfer agents include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol and ethanol; mercaptans such as methyl mercaptan; halogenated hydrocarbons such as carbon tetrachloride, chloroform, dichloromethane, and chloromethane, etc. The amount of chain transfer agent added can vary depending on the chain transfer constant of the compound used, and is usually used in the range of 0.01 to 20% by mass relative to the polymerization solvent.

[0063] Examples of the solvent include water and a mixed solvent of water and alcohol.

[0064] In suspension polymerization, a fluorinated solvent may be used in addition to water. Examples of the fluorinated solvent include CH 3 CClF 2 , CH 3 CCl 2 F. CF 3 CF 2 CCl 2 H.CF 2 CCF 2 CFHCl and other hydrochlorofluoroalkanes; CF 2 ClCFClCF 2 CF 3 CF 3 CFClCFClCF 3 Chlorofluoroalkanes; CF 3 CFHCFHCF 2 CF 2 CF 3 CF 2 HCF 2 CF 2 CF 2 CF 2 H.CF 3 CF 2 CF 2 CF 2 CF 2 CF 2 CF 2 H and other hydrofluoroalkanes; CH 3 OC 2 F 5 , CH 3 OC 3 F 5 CF 3 CF 2 CH 2 OCHF 2 CF 3 CHF 2 OCH 3 , CHF 2 CF 2 OCH 2 F, (CF 3 ) 2 CHCF 2 OCH 3 CF 3 CF 2 CH 2 OCH 2 CHF 2 CF3 CHF 2 OCH 2 CF 3 Hydrofluoroethers, such as perfluorocyclobutane, CF 3 CF 2 CF 2 CF 3 CF 3 CF 2 CF 2 CF 2 CF 3 CF 3 CF 2 CF 2 CF 2 CF 2 CF 3 The amount of the fluorinated solvent used is preferably 10 to 100% by mass relative to the aqueous medium from the viewpoint of suspending properties and economic efficiency.

[0065] The polymerization temperature is not particularly limited and may be 0 to 100° C. The polymerization pressure is appropriately determined depending on the type and amount of the solvent used and other polymerization conditions such as vapor pressure and polymerization temperature, and may generally be 0 to 9.8 MPaG.

[0066] In the case of obtaining an aqueous dispersion comprising a copolymer by polyreaction, the copolymer can be recovered by precipitating, cleaning, and drying the copolymer contained in the aqueous dispersion. In addition, in the case of obtaining a copolymer in the form of a slurry by polyreaction, the copolymer can be recovered by taking out the slurry from a reaction vessel and cleaning and drying. By drying, the copolymer can be recovered in the form of a powder.

[0067] The copolymer obtained by polymerization may also be subjected to fluorination treatment. Fluorination treatment may be carried out by contacting the copolymer that has not been subjected to fluorination treatment with a fluorine-containing compound. Fluorination treatment can reduce the -COOH and -COOCH 3 、-CH 2 OH, -COF, -CF=CF 2 、-CONH 2 Thermally unstable functional groups and thermally stable -CF 2 H and other functional groups are converted into extremely thermally stable -CF 3 As a result, the COOH and -COOCH 3 、-CH 2 OH, -COF, -CF=CF 2 、-CONH 2 and -CF 2 The total number of H (the number of functional groups) is adjusted to fall within the above range.

[0068] The fluorine-containing compound is not particularly limited, and examples thereof include a fluorine radical source that generates fluorine radicals under fluorination treatment conditions. Examples of the fluorine radical source include F 2 Gas, CoF 3 , AgF 2 、UF 6 、OF 2 、N 2 F 2 CF 3 OF, fluorinated halogens (such as IF 5 , ClF 3 )wait.

[0069] F 2 The fluorine radical source such as gas can be 100% concentration, but from the aspect of safety, it is preferably mixed with an inert gas and diluted to 5% to 50% by mass for use, and more preferably diluted to 15% to 30% by mass for use. As the above-mentioned inert gas, nitrogen, helium, argon, etc. can be cited, and nitrogen is preferred from the aspect of economy.

[0070] The conditions for the fluorination treatment are not particularly limited, and the molten copolymer may be brought into contact with the fluorine-containing compound. However, the fluorination treatment may be carried out at a temperature below the melting point of the copolymer, preferably at 20°C to 240°C, and more preferably at 100°C to 220°C. The fluorination treatment is generally carried out for 1 to 30 hours, preferably for 5 to 25 hours. The fluorination treatment is preferably carried out by bringing the unfluorinated copolymer into contact with fluorine gas (F 2 Gas) contact treatment.

[0071] The powder coating material can be produced, for example, by producing a copolymer as described above, compressing the obtained copolymer into a sheet with a roller, and then pulverizing and classifying the sheet with a pulverizer.

[0072] Powder coatings are usually applied to the object to be coated and then heated to form a film. The coating film thus obtained can be used for various purposes such as corrosion-resistant linings.

[0073] The method for applying the powder coating is not particularly limited, and examples thereof include spray coating, electrostatic spray coating, electrostatic spray coating, fluid dip coating, electrostatic fluid dip coating, liner molding, and the like.

[0074] The coating film formed by the powder coating is usually formed by applying the powder coating to the object to be coated and then heating and firing to form a film. The temperature for heating and firing the powder coating applied to the object to be coated is, for example, 295 to 400°C. The heating and firing time is, for example, 20 to 180 minutes. The heating and firing time indicates the firing time for one time when the powder coating is applied and fired multiple times.

[0075] The thickness of the coating film formed by the powder coating material may be appropriately determined according to the application, and may be, for example, 20 to 10000 μm. The film thickness is the film thickness after heating and firing, and may be the film thickness of the coating film obtained by one coating or by two or more coatings.

[0076] The water vapor permeability of the coating film formed by the powder coating is preferably 18.0 g·cm / m 2 The powder coating material contains a copolymer in which the content of PPVE units, melt flow rate (MFR) and number of functional groups of a copolymer containing TFE units and PPVE units are appropriately adjusted, and thus a coating film having excellent low water vapor permeability can be obtained.

[0077] In the present invention, the water vapor permeability can be measured under the conditions of a temperature of 95° C. and a period of 45 days. The water vapor permeability can be specifically measured by the method described in the Examples.

[0078] The methyl ethyl ketone (MEK) permeability of the coating film formed by the powder coating is preferably 65.0 mg·cm / m 2 The powder coating material contains a copolymer in which the content of PPVE units, melt flow rate (MFR) and number of functional groups of the copolymer containing TFE units and PPVE units are appropriately adjusted, so that a coating film having excellent low permeability to chemical liquids such as MEK can be obtained.

[0079] In the present invention, the MEK permeability can be measured under the conditions of a temperature of 60° C. and a period of 45 days. The MEK permeability can be specifically measured by the method described in the Examples.

[0080] The article of the present invention comprises a coating film formed of a powder coating. The article of the present invention generally comprises a coating film and an object to be coated, and the coating film is present on the surface of the object to be coated.

[0081] The object to be coated is not particularly limited, and any object to which corrosion resistance is desired can be cited. Examples of such objects to be coated include boxes, containers, towers, valves, pumps, joints, other piping materials, etc., which are coated with corrosion-resistant linings; chemical and medical instruments, wafer baskets, coil frame tower gaskets, valves for pharmaceuticals, pump impellers, and other objects to be coated with corrosion-resistant processing.

[0082] The object to be coated can be cleaned, surface treated by sandblasting, or primed as needed.

[0083] Although the embodiments have been described above, it should be understood that various changes in the embodiments and details can be made without departing from the spirit and scope of the claims.

[0084] <1> According to a first aspect of the present invention, there is provided a powder coating comprising a copolymer comprising tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, wherein:

[0085] The content of the perfluoro(propyl vinyl ether) unit in the copolymer is 5.0% to 6.2% by mass based on the total monomer units.

[0086] The melt flow rate of the copolymer at 372°C is 20.0 g / 10 min to 35.0 g / 10 min.

[0087] The number of functional groups of the above copolymer is relative to every 10 6 The number of carbon atoms in the main chain is 100 or less.

[0088] <2> According to a second aspect of the present invention, there is provided a powder coating according to the first aspect, wherein:

[0089] The content of the perfluoro(propyl vinyl ether) unit in the copolymer is 5.1% by mass to 6.0% by mass based on all monomer units.

[0090] <3> According to a third aspect of the present invention, there is provided a powder coating according to the first or second aspect, wherein the melt flow rate of the copolymer at 372° C. is 23.0 to 32.0 g / 10 min.

[0091] <4> According to a fourth aspect of the present invention, there is provided a coating film formed from the powder coating material according to any one of the first to third aspects.

[0092] <5> According to a fifth aspect of the present invention, there is provided an article comprising a coating film formed from the powder coating material according to any one of the first to third aspects.

[0093] Example

[0094] Next, embodiments of the present invention will be described with reference to examples, but the present invention is not limited to the examples.

[0095] Each numerical value in the examples was measured by the following method.

[0096] (Content of monomer units)

[0097] The content of each monomer unit is measured using an NMR analyzer (for example, AVANCE300 high temperature probe manufactured by Bruker BioSpin).

[0098] (Melt Flow Rate (MFR))

[0099] The mass (g / 10 min) of the polymer flowing out from a nozzle having an inner diameter of 2.1 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes was determined using a melt flow indexer G-01 (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with ASTM D1238.

[0100] (Number of functional groups)

[0101] The fluorinated copolymer powder was cold pressed to produce a film with a thickness of 0.25 mm to 0.30 mm. The film was scanned 40 times by a Fourier transform infrared spectrometer [FT-IR (Spectrum One, manufactured by PerkinElmer)] and analyzed to obtain an infrared absorption spectrum, which was a difference spectrum from the background spectrum of complete fluorination without the presence of functional groups. From the absorption peak of the specific functional group appearing in the differential spectrum, the following formula (A) was used to calculate the absorption peak of each 1×10 6 The number of functional groups N per carbon atom.

[0102] N=I×K / t(A)

[0103] I: Absorbance

[0104] K: Correction coefficient

[0105] t: film thickness (mm)

[0106] For reference, regarding the functional groups in the present invention, the absorption frequency, molar absorption coefficient and correction coefficient are shown in Table 2. The molar absorption coefficient is determined from the FT-IR measurement data of a low molecular weight model compound.

[0107] [Table 2]

[0108] Table 2

[0109]

[0110] (Melting Point)

[0111] Using a differential scanning calorimeter (trade name: X-DSC7000, manufactured by Hitachi High-Tech Science Co., Ltd.), the temperature was increased from 200°C to 350°C for the first time at a heating rate of 10°C / min, then cooled from 350°C to 200°C at a cooling rate of 10°C / min, and the temperature was increased from 200°C to 350°C for the second time at a heating rate of 10°C / min. The melting point was determined from the peak of the melting curve generated in the second heating process.

[0112] Comparative Example 1

[0113] 51.8L of pure water was put into a 174L autoclave with a stirrer. After fully replacing with nitrogen, 40.9kg of perfluorocyclobutane, 1.17kg of perfluoro(propyl vinyl ether) (PPVE) and 4.19kg of methanol were added, and the temperature in the system was maintained at 35°C. Next, tetrafluoroethylene (TFE) was pressed into 0.64MPa, and 0.103kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added to initiate polymerization. As the polymerization proceeded, the pressure in the system decreased, so TFE was continuously supplied to keep the pressure constant. For every 1kg of TFE supplied, 0.031kg of PPVE was added. The polymerization was terminated when the additional amount of TFE reached 40.9kg. The unreacted TFE was released, and after returning the pressure in the autoclave to atmospheric pressure, the obtained reaction product was washed with water and dried to obtain 42.2kg of powder.

[0114] The obtained copolymer powder was compressed into a flake shape using a roll compactor, and then crushed into flakes having a size of about several mm to obtain a copolymer powder.

[0115] The obtained flaky copolymer powder was placed in a vacuum vibration reactor VVD-30 (manufactured by Ohkawara Manufacturing Co., Ltd.) and heated to 210°C. After evacuation, N 2 The gas was diluted to 20% by volume of F 2 Gas to atmospheric pressure. From F 2 0.5 hours after the gas was introduced, temporarily evacuate the air and introduce F again. 2 After 0.5 hours, the vacuum was evacuated again and F 2 Gas. Then, the above F 2 The gas introduction and vacuuming were continued once every hour, and the reaction was carried out at a temperature of 210°C for 10 hours. After the reaction was completed, the reactor was fully replaced with N 2 gas, ending the fluorination reaction.

[0116] The fluorinated flaky copolymer powder was pulverized with a hammer mill to obtain a copolymer powder having an average particle size of 20 to 40 μm and an apparent density of 0.60 to 0.70 g / ml.

[0117] Comparative Example 2

[0118] A fluorinated copolymer powder was obtained in the same manner as in Comparative Example 1 except that 4.00 kg of PPVE, 1.92 kg of methanol, 0.051 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate, and 0.080 kg of PPVE was added per kg of TFE supplied to obtain 44.2 kg of dry powder.

[0119] Comparative Example 3

[0120] A fluorinated copolymer powder was obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.75 kg, methanol was changed to 3.02 kg, and 0.058 kg of PPVE was additionally charged per 1 kg of TFE supplied to obtain 43.3 kg of dry powder.

[0121] Comparative Example 4

[0122] A fluorinated copolymer powder was obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.75 kg, methanol to 2.44 kg, 50% methanol solution of di-n-propyl peroxydicarbonate to 0.051 kg, and 0.058 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 43.3 kg of dry powder.

[0123] Comparative Example 5

[0124] Unfluorinated copolymer powder was obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 3.01 kg, methanol to 4.62 kg, 50% methanol solution of di-n-propyl peroxydicarbonate to 0.051 kg, and 0.063 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 43.5 kg of dry powder.

[0125] Example 1

[0126] The fluorinated copolymer powder was obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.49 kg, methanol to 4.53 kg, 50% methanol solution of di-n-propyl peroxydicarbonate to 0.051 kg, and 0.054 kg of PPVE was added for every 1 kg of TFE supplied. The heating temperature of the vacuum vibration reactor was changed to 160°C, and the reaction was carried out at 160°C for 5 hours to obtain 43.1 kg of dry powder.

[0127] Example 2

[0128] A fluorinated copolymer powder was obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.69 kg, methanol to 0.22 kg, and 0.057 kg of PPVE was additionally charged per 1 kg of TFE supplied to obtain 43.2 kg of dry powder.

[0129] Example 3

[0130] A fluorinated copolymer powder was obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.88 kg, methanol to 4.50 kg, 50% methanol solution of di-n-propyl peroxydicarbonate to 0.051 kg, and 0.060 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 43.4 kg of dry powder.

[0131] Example 4

[0132] A fluorinated copolymer powder was obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 3.07 kg, methanol to 4.38 kg, 50% methanol solution of di-n-propyl peroxydicarbonate to 0.051 kg, and 0.064 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 43.5 kg of dry powder.

[0133] The various physical properties of the copolymer powders obtained in Examples and Comparative Examples were measured by the above-mentioned methods.

[0134] [Table 3]

[0135] Table 3

[0136]

[0137] The expression “<6” in Table 3 means that the number of functional groups is less than 6.

[0138] (Method for preparing coating film for evaluation)

[0139] After applying the copolymer powder by electrostatic coating on a degreased, smooth SUS316 substrate (200mm×200mm×5mm), the substrate was vertically hung in a drying furnace and calcined at 380°C for 30 minutes to obtain a coating film with a thickness of about 100 μm. The SUS316 substrate with the coating film was placed in water together with the coating film and heated at 95°C for 20 hours, and the coating film peeled off from the SUS316 substrate was recovered as an evaluation coating film (thickness of about 0.1 mm).

[0140] (Abrasion test)

[0141] A 10 cm × 10 cm test piece was cut from the coating film for evaluation. The test piece was fixed on the test bench of a Taber abrasion tester (No. 101 Special Taber Wear Tester, manufactured by Yasuda Seiki Co., Ltd.), and the abrasion test was performed using the Taber abrasion tester under the conditions of a test piece surface temperature of 60°C, a load of 500 g, a wear wheel CS-10 (grinded with abrasive paper #240 for 20 turns), and a rotation speed of 60 rpm. The weight of the test piece after 1000 turns was measured, and the weight of the test piece was further measured after 8000 turns of the test using the same test piece. The amount of wear was calculated using the following formula.

[0142] Wear amount (mg) = M1 - M2

[0143] M1: Weight of test piece after 1000 revolutions (mg)

[0144] M2: Test piece weight after 8000 revolutions (mg)

[0145] (Water vapor transmission rate)

[0146] A sheet test piece was prepared from the coating film for evaluation. 2 ) was filled with 18g of water, covered with a sheet test piece, and sealed with a PTFE gasket. The sheet test piece was kept in contact with water at 95°C for 45 days, then taken out and left at room temperature for 2 hours to measure the mass loss. The water vapor permeability (g·cm / m 2 ).

[0147] Water vapor permeability (g·cm / m 2 ) = mass loss (g) × thickness of sheet test piece (cm) / penetration area (m 2 )

[0148] (Methyl ethyl ketone (MEK) permeability)

[0149] A sheet test piece with a thickness of about 0.1 mm was prepared from the coating film for evaluation. 2 ) was placed in a container, covered with a sheet test piece, and sealed with a PTFE gasket. The sheet test piece was kept at 60°C for 45 days, then taken out and left at room temperature for 1 hour to measure the mass loss. The MEK permeability (mg·cm / m 2 ·sky).

[0150] MEK permeability (mg·cm / m 2 ·day) = [mass loss (mg) × thickness of sheet test piece (cm)] / [permeation area (m 2 )·Days (days)]

[0151] (Tensile creep test)

[0152] The tensile creep strain was measured using a TMA-7100 manufactured by Hitachi High-Technologies Corporation. A sample with a width of 2 mm and a length of 22 mm was prepared from the coating for evaluation. The sample was mounted in a measuring fixture with a distance of 10 mm between the fixtures. For the sample, a cross-sectional load of 2.63 N / mm 2 The sample was loaded in a manner of 230°C and placed at 230°C. The displacement (mm) of the length of the sample was measured from 70 minutes after the start of the test to 555 minutes after the start of the test. The ratio of the displacement (mm) of the length to the initial sample length (10 mm) was calculated (tensile creep strain (%)). The sheet with a small tensile creep strain (%) measured at 230°C and 555 minutes is not easy to elongate even when a tensile load is applied in a very high temperature environment, and has excellent high temperature tensile creep resistance.

[0153] (180℃ tensile strength)

[0154] Dumbbell-shaped test pieces were punched out from the coating film using a V-shaped dumbbell according to ASTM D1708. The tensile strength of the dumbbell-shaped test pieces was measured at 180°C at 50 mm / min using Autograph (AG-X500N manufactured by Shimadzu Corporation).

[0155] The coating film with high tensile strength at 180°C is not easily damaged even when tensile force is applied at high temperature.

[0156] [Table 4]

[0157] Table 4

[0158]

Claims

1. A powder coating, which is a powder coating containing a copolymer, the copolymer containing tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, wherein: The content of the perfluoro(propyl vinyl ether) unit in the copolymer is 5.0% to 6.2% by mass based on the total monomer units. The melt flow rate of the copolymer at 372° C. is 20.0 g / 10 min to 35.0 g / 10 min. The number of functional groups of the copolymer is relative to every 10 6 The number of carbon atoms in the main chain is 100 or less.

2. The powder coating according to claim 1, wherein: The content of the perfluoro(propyl vinyl ether) unit in the copolymer is 5.1% by mass to 6.0% by mass based on the total monomer units.

3. The powder coating according to claim 1 or 2, wherein: The melt flow rate of the copolymer at 372° C. is 23.0 g / 10 min to 32.0 g / 10 min. 4 . A coating film formed from the powder coating material according to claim 1 . 5 . An article comprising a coating film formed from the powder coating material according to claim 1 .

Citation Information

Patent Citations

  • Powder coating material

    WO2003006566A1

  • Laminate body and method for producing laminate body

    CN103826845A

  • Ethylene / tetrafluoroethylene copolymer, method for producing same, powder coating, and molded article

    CN106459233A

  • Powder, powder paint, and laminate production method

    CN111372976A

  • Electricity storage body and gasket

    CN114223086A