Method for coating component
By using coatings of praseodymium or terbium in metal-supported solid oxide fuel cells, the problem of chromium volatility in chromium-containing materials at high temperatures is solved, and the protection and performance of components are improved.
Patent Information
- Application Number
- CN202380027825.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-17
- Filing Date
- 2023-03-17
- Publication Date
- 2024-11-05
AI Technical Summary
The chromium-containing materials in existing metal-supported solid oxide fuel cells may cause chromium volatility, causing corrosion and toxicity during manufacturing and operation, and the existing coating solutions have not completely solved this problem.
The coating mixture containing a praseodymium and/or terbium source is coated on the surface of the chromium-containing component and heated in an oxidative atmosphere at a temperature of 450°C or higher to form a coating of praseodymium or terbium material with barrier function to Reduce or prevent chromium volatilization.
Effectively reduce or prevent chromium volatility, protect components from chromium contamination, improve the stability and performance of fuel cells, and significantly reduce the chromium evaporation rate when operating at high temperatures.
Smart Images

Figure CN118900933A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a coated component, a coated component for a device, and an electrochemical device comprising a coated component. Background Art
[0002] Coatings based on rare earth compounds have been used to reduce corrosion of substrates as well as to provide substrates with specific surface properties.
[0003] Yan Yan et al. (Surface and Coatings Technology; Vol. 272, (2015), pp. 415-427) disclose the fabrication of lanthanum oxide, yttrium oxide, and cerium oxide coatings on porous stainless steel for use in metal-supported solid oxide fuel cells. The paper explains that the suitability of rare earth oxides as coatings is highly dependent on the rare earth oxide used.
[0004] US-A-2004 / 186201 discloses an anti-corrosion coating (including carbon pigment) for a substrate that may contain rare earths. US-A-2005 / 0061664 discloses an electrolytic cell, more specifically, an interconnector-supported electrolytic cell assembly, a preform, and a method of manufacturing. ES2359550 discloses a glass coating composition and a method for obtaining a glass coating obtained by a sol-gel process that is stable at temperatures up to 250°C. KR 1020200131553 discloses a method for obtaining a glass coating having Pr x O 2x-δ Interconnector for coated solid oxide batteries. KR 1020200132500 discloses a battery module.
[0005] WO-A-05 / 071021 discloses a corrosion inhibiting coating composition as a self-priming topcoat which contains a fluorinated resin and may include a corrosion inhibiting rare earth compound.
[0006] US-A-2013 / 251942 and WO-A-2012 / 021822 each disclose a substrate having a hydrophobic coating of a rare earth element material (oxide, carbide, nitride, fluoride, and / or boride) having a dynamic water contact angle of at least about 90 degrees.
[0007] Fontana et al. (Journal of Power Sources 171 (2007), pp. 652-662) discloses corrosion resistance and electrical conductivity evaluation studies of alloys using La, Y, and Nd oxide coatings deposited by metal organic chemical vapor deposition.
[0008] Electrochemical cells formed of oxide layers, which may include rare earth oxide layers (commonly referred to as solid oxide cells: SOCs) can be used as fuel cells or electrolyzer cells.
[0009] The SOC fuel cell unit generates electricity using an electrochemical conversion process of an oxidizable fuel. The SOC fuel cell unit can also (or instead) operate as a regenerative fuel cell (or reverse fuel cell) unit, commonly known as a solid oxide electrolyzer fuel cell unit, for example to separate hydrogen and oxygen from water, or to separate carbon monoxide and oxygen from carbon dioxide.
[0010] Solid oxide fuel cells (SOFCs) generate electrical energy by electrochemical oxidation of a fuel gas (usually hydrogen-based), and the device is typically ceramic-based, using ceramic-containing oxygen-ion conducting metal oxides as its electrolyte. Many ceramic oxygen-ion conductors (e.g., doped zirconia or doped ceria) have useful ionic conductivity at temperatures exceeding 450°C or 500°C (for ceria-based electrolytes) or 650°C (for zirconia-based ceramics), so SOFCs tend to operate at high temperatures. The fuel electrode, electrolyte, and air electrode of the SOC can each form one or more layers to optimize operation.
[0011] In operation, the electrolyte of the SOFC conducts oxygen ions from the cathode to the anode located on the opposite side of the electrolyte. The fuel contacts the anode (commonly referred to as the "fuel electrode"), while the oxidant (such as air or an oxygen-rich fluid) contacts the cathode (commonly referred to as the "air electrode"). Conventional ceramic-supported (e.g., anode-supported) SOFCs have low mechanical strength and are prone to fracture. Therefore, metal-supported SOFCs have been developed, which have active fuel cell component layers supported on a metal substrate. In these cells, the ceramic layers can be very thin because they only perform electrochemical functions: that is, the ceramic layers are not self-supporting, but are thin coatings / films laid on and supported by the metal substrate. Such metal-supported SOFC stacks are stronger, less expensive, have better thermal performance than ceramic-supported SOFCs, and can be sealed using conventional metal welding techniques.
[0012] WO-A-2015 / 136295 of the applicant discloses a metal supported SOFC, wherein a metal support plate has a porous region surrounded by a non-porous region, wherein an active layer is deposited on the porous region, so that gas can pass through the holes from one side of the metal support plate to the other side to access the active layer coated thereon. The porous region contains small holes (holes drilled through the metal foil substrate) extending through the support plate.
[0013] WO-A-2016 / 128721 discloses an interconnect for a low-temperature solid oxide fuel cell, in particular an interconnect comprising a chromium oxide layer (chromium (III) oxide / chromium oxide).
[0014] Components in SOFCs (and other devices) including metal supports and interconnects and other components may be formed from SOFC specific materials including steel. However, it is desirable to use chromium containing materials that may be less costly or may have other advantageous properties. However, it has been observed that materials (e.g. metal alloys) may exhibit chromium volatilization. Volatile chromium compounds may cause problems during manufacturing and may poison SOFC electrodes during operation. Attempts have been made to coat components (e.g. using alumina or CoCe) to reduce chromium problems, but these have not been entirely successful.
[0015] Therefore, there is a need to reduce or prevent the problems associated with the use of chromium containing materials.
[0016] The present invention aims to address this need. Summary of the invention
[0017] In a first aspect, the present invention provides a method for producing a coated component, the method comprising: a) providing a chromium-containing component, b) providing a coating mixture comprising at least one solvent and a praseodymium source and / or a terbium source, c) contacting at least one surface of the component with the coating mixture, d) optionally, drying the component, and e) heating the component in an oxidizing atmosphere at a temperature of 450°C or higher.
[0018] Thus, in a method using a praseodymium source, a method for producing a coated component is provided, the method comprising: a) providing a chromium-containing component, b) providing a coating mixture comprising at least one solvent and a praseodymium source, c) contacting at least one surface of the component with the coating mixture, d) optionally, drying the component, and e) heating the component in an oxidizing atmosphere at a temperature of 450° C. or greater.
[0019] This method is advantageous because it produces a chromium-containing component having at least one surface coated with a coating comprising at least one layer containing a Pr or Tb material, which has been observed to unexpectedly reduce problems with chromium-containing components.
[0020] The advantage of the coating is that it acts as a barrier to reduce or prevent chromium volatilization.
[0021] The heating step may be a step for decomposing the Pr source and / or Tb source coating and oxidizing the coating in a single heating step to produce a coating having barrier layer properties. Alternatively, the method may further comprise one or more additional heating steps, optionally performed in an oxidizing atmosphere. Thus, the method may further comprise additionally heating the assembly at a temperature of 450°C to 950°C, optionally 450°C to 910°C, optionally 450°C to 870°C, optionally 450°C to 810°C, optionally 450°C to 620°C. The additional heating step may be performed during operation of the assembly.
[0022] The praseodymium source and / or terbium source may be a Pr(III) source and / or a Tb(III) source. Typically, the praseodymium source and / or terbium source may be a Pr(III) source or a Tb(III) source, thereby producing a coating comprising a material containing Pr or Tb. However, in some applications, the praseodymium source and / or terbium source may be a mixed source of praseodymium and terbium, thereby producing a mixed material comprising both Pr and Tb.
[0023] The method may further comprise repeating steps a) to c), and optionally d) and e), thereby producing a coated component having a coating comprising a plurality of layers. This has advantages if thicker coatings are desired.
[0024] The method according to the invention is advantageous in that it provides a coating with continuity (eg forms a substantially uninterrupted coating). Furthermore, it has been found that the coating is electrically conductive.
[0025] Generally speaking, the coating may have a thickness in the range of 50 nm to 1 μm, preferably the coating has a thickness in the range of 50 nm to 500 nm, more preferably 50 nm to 200 nm.
[0026] In other cases, the component may be uncoated, ie, the coating may be located directly on the surface of the component without an intervening layer.
[0027] The component may comprise a chromium-containing metal alloy. Such an alloy may be selected from Ni and / or Co superalloys.
[0028] The alloy will typically comprise a ferrochromium (ie, iron-containing) alloy.
[0029] The component may comprise stainless steel, such as ferritic stainless steel.
[0030] The alloy may contain 11 wt % or more Cr; optionally, 15 wt % or more Cr; optionally, 17 wt % or more Cr; optionally, 19 wt % or more Cr.
[0031] The alloy may have an amount of lanthanum or zirconium below 0.08 wt %.
[0032] Preferably, the coating mixture is in a liquid state, and preferably comprises a coating solution.
[0033] The solvent may comprise an alcohol, optionally a C1 to C6 alcohol. The solvent may be selected from one or more of ethanol, propanol, and / or methoxypropanol.
[0034] Liquid coating methods may be used. For example, contacting at least one surface of the component with the coating mixture may include dipping the component in the coating mixture and / or spraying the component with the coating mixture.
[0035] If the method includes dip coating, the dip coating of the assembly may be performed at a controlled dip rate to help control the thickness and other characteristics of the coating.
[0036] If the method is spraying, the method may comprise atomised spraying, optionally using a sonic or ultrasonic atomiser.
[0037] Contacting at least one surface of the component with the coating mixture may be performed at a temperature in the range of 10°C to 100°C, optionally at 12°C to 50°C, optionally at a component temperature of about room temperature.
[0038] The component surface may be cleaned / polished prior to contacting the component surface with the coating mixture.
[0039] Heating the assembly in the oxidizing atmosphere may include heating the assembly to a temperature of 480°C or more, optionally 500°C or more, optionally 520°C or more, optionally 550°C or more.
[0040] Heating the component in the oxidizing atmosphere may include heating the component to a temperature of 580°C, 610°C, 650°C, 670°C, 720°C, 770°C, 820°C, 870°C, 900°C, 910°C, or more.
[0041] The oxidizing atmosphere may comprise oxygen, and typically may comprise air.
[0042] The praseodymium source and / or terbium source may comprise a Pr(III) salt and / or a Tb(III) salt. The salt may typically be a Pr(III) nitrate and / or a Tb(III) nitrate.
[0043] The praseodymium source and / or terbium source may comprise chelated Pr(III) and / or chelated Tb(III). Optionally, the chelated Pr(III) and / or chelated Tb(III) may comprise a bidentate ligand (eg acetylacetone (acac) or ethylenediamine) or a tridentate ligand or a tetradentate ligand.
[0044] The praseodymium source and / or the terbium source may comprise a mixture of a Pr(III) salt and a chelated Pr(III); and / or a mixture of a Tb(III) salt and a chelated Tb(III).
[0045] Thus, the source of Pr(III) may include chelated Pr(III) and / or the source of Tb(III) may include chelated Tb(III).
[0046] The method according to the first aspect produces a coated component which may have a variety of uses.Thus, the coated component may comprise a coated component for use in an apparatus, optionally for operation at temperatures of 450°C or higher.
[0047] In a second aspect, the present invention may provide a coated component obtainable by a method as described above.
[0048] In a third aspect, the invention hereby provides a coated component for a device, the coated component comprising a chromium-containing component having at least one surface with a coating comprising at least one layer comprising a praseodymium material and / or a terbium material.
[0049] Thus, when the coating comprises at least one layer comprising a praseodymium material, a coated component for a device is provided, the coated component comprising a chromium-containing component having at least one surface with a coating comprising at least one layer comprising a praseodymium material.
[0050] Preferably, the apparatus is adapted to operate at temperatures of 450°C or higher.
[0051] The coating may comprise two or more layers, each layer comprising a praseodymium material and / or a terbium material. The coating may comprise three or more layers, each layer comprising a praseodymium material and / or a terbium material.
[0052] Optionally, the coating may be in direct contact with (ie, directly adjacent to) a metal surface of a component. Thus, the coating may be on a bare or otherwise uncoated surface of a component.
[0053] The coatings described herein can form a barrier coating on chromium-containing components that reduces or prevents chromium volatilization and serves to protect components that may be susceptible to chromium contamination, particularly when such susceptible components are in fluid communication with chromium-containing components, such as in a system containing an electrochemical cell stack.
[0054] In preferred aspects, the device may comprise an electrochemical cell. Thus, the components may comprise interconnects, spacers, metal plates, or substrates.
[0055] The device may be a system comprising an electrochemical cell stack. Thus, the component may comprise a system component, such as a fitting, a fastener, a valve assembly, a tube, or a heat exchanger.
[0056] In a fourth aspect, the invention hereby provides an electrochemical device comprising a coated component comprising a chromium-containing component having at least one surface with a coating comprising at least one layer comprising a praseodymium material and / or a terbium material.
[0057] Thus, when the coating comprises at least one layer comprising a praseodymium material, an electrochemical device comprising a coated component comprising a chromium-containing component having at least one surface with a coating comprising at least one layer comprising a praseodymium material is provided.
[0058] The electrochemical device may be a system comprising an electrochemical cell stack.
[0059] The electrochemical device may be (or comprise) an electrolysis cell, an oxygen separator, a sensor, or a fuel cell, preferably a SOFC.Preferably, the electrochemical cell is adapted to operate at a temperature of 450°C or higher.
[0060] In all aspects of the invention relating to methods, coated components, electrochemical devices and uses, it is preferred that the coating is not an active electrochemical layer, such as an electrode or electrolyte layer.
[0061] The coating acts as a barrier coating on the component that reduces or prevents chromium volatilization.
[0062] Thus, in a fifth aspect there is provided the use of a coating as a barrier coating on a chromium containing component in an electrochemical device, wherein the coating comprises at least one layer comprising a praseodymium material and / or a terbium material.
[0063] Thus, there is provided use of the coating as a barrier coating on a chromium-containing component in an electrochemical device when the coating comprises at least one layer comprising a praseodymium material.
[0064] Preferably, the coating is adjacent to the component surface, ie directly on the component surface.
[0065] The present invention is advantageous in its various aspects because it can protect substrates, components, and devices (including electrochemical cells) from contamination by chromium, which can otherwise evaporate from components (including stainless steel components) at higher temperatures and which can otherwise react on active surfaces of components (e.g., on electrodes of an electrochemical cell) to form stable chromate phases.
[0066] definition
[0067] In this specification, the term "source" of an element, compound, or other material means a material containing the element, compound, or other material, whether or not chemically bonded in the source. The source of an element, compound, or other material may be an elemental source (e.g., Pr, Tb, or O2), or may be in the form of a compound or mixture containing one or more of the element, compound, or material.
[0068] In the present specification, reference to a praseodymium source and / or a terbium source may refer to a praseodymium source or a terbium source; or may refer to a praseodymium source and a terbium source (e.g., a mixture of the praseodymium source and the terbium source). Similarly, in the present specification, reference to a praseodymium material and / or a terbium material may refer to a praseodymium material or a terbium material; or may refer to a praseodymium material and a terbium material (e.g., a mixture of the praseodymium material and the terbium material).
[0069] In this specification, references to electrochemical cells, SOC, SOFC and SOEC may refer to tubular cells or planar cells. Electrochemical cell units may be tubular or planar structures. Planar fuel cell units may be arranged on top of each other in a stacked arrangement, such as 100-200 fuel cell units in a stack, wherein the individual fuel cell units are arranged in electrical series.
[0070] Electrochemical cells can be fuel cells, reversible fuel cells, or electrolyzer cells. In general, these cells can have the same structure, and reference to electrochemical cells can refer to (unless the context indicates otherwise) any of these types of cells. The cell can be based on a solid oxide electrolyte, optionally a metal-supported solid oxide cell. In fuel cell mode, the fuel contacts the anode (fuel electrode) and the oxidant (such as air or an oxygen-rich fluid) contacts the cathode (air electrode), so in fuel cell mode operation, the air electrode will be the cathode. A solid oxide electrolyzer cell (SOEC) can have the same structure as a SOFC, but is essentially a SOFC operated in a reverse or regenerative mode to achieve electrolysis of water and / or carbon dioxide to produce hydrogen and / or carbon monoxide and oxygen by using a solid oxide electrolyte.
[0071] In this specification, the unit of area specific resistance (ASR) is Ωcm when not normalized. 2 or mΩcm 2 ) refers to the internal resistance of an electrochemical cell normalized by the cell's active area (often used to allow direct comparison of cells of different active areas). ASR is equal to the voltage drop due to the cell's internal resistance multiplied by the current density (in Acm -2 ).
[0072] The secant ASR is given by the voltage drop from the open circuit to the cell's operating voltage divided by the applied current density (so a cell with a lower ASR will have a higher operating voltage and power output at any given applied current density).
[0073] The ohmic / series resistance (Rs) is the component of the internal resistance of the cell without the associated capacitance (the resistance of the oxide scale of the steel components can be described by Rs).
[0074] The term "fluid flow path" is used to define the fluid flow path between various components, and it is therefore also understood that these components are in fluid communication with each other.
[0075] As will be appreciated by those skilled in the art, the various features of the aspects of the disclosure described herein may be used in combination with any other features of the same or other aspects of the disclosure, if appropriate modifications are required.
[0076] Furthermore, while all aspects of the invention or disclosure preferably "comprise / include" the features described in relation to that aspect, it is specifically contemplated that they may "consist of" or "consist essentially of" those features outlined in the claims.
[0077] The present invention will now be described with reference to the accompanying drawings and examples. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 Graph showing the normalized series resistance of a coated stainless steel interconnect as a function of temperature.
[0079] Figure 2 Graph showing the secant ASR normalized to a standard SOFC cell as a function of temperature for a stainless steel (with 22-23% Cr and 0.1% La) SOFC substrate coated according to the present invention.
[0080] Figure 3 Display Figure 2 Plot of Rs as a function of temperature for the coated stainless steel SOFC substrate normalized to a standard SOFC cell.
[0081] Figure 4 Display Figure 2 Plot of SecASR as a function of temperature for the coated stainless steel SOFC substrate normalized to a standard SOFC cell.
[0082] Figure 5 A schematic diagram showing the flow of the method.
[0083] Figure 6 A schematic diagram of a fuel cell system illustrating fluid flow paths is shown.
[0084] Figure 7 A schematic cross-section of a coated component is shown (not to scale).
[0085] Figure 8 Graph showing cumulative chromium evaporation as a function of time for coated stainless steel coupons. DETAILED DESCRIPTION
[0086] Figure 5 A schematic flow diagram illustrating a method of providing a coating on a component as in the examples is shown. Figure 5, dashed arrows indicate optional steps. A coating mixture 320 containing a solvent and a Pr source, such as, for example, a mixture of Pr nitrate and Pr acetylacetone (Pracac), is provided. The coating mixture 320 is applied to a component (which may be stainless steel) 310 in step 330. After applying the coating mixture 320 at 330, the component is optionally dried 340 and then heated 350 in an oxidizing atmosphere at 450° C. or higher. Optionally, the coating step 360 is repeated after step 330, after the optional drying step 340, or after the heating step 350 to form additional layers and thicker coatings.
[0087] Chromium contamination can affect electrochemically active components in a fuel cell system, especially when the chromium-containing components are in fluid communication with the electrochemically active components. The coatings described herein can form a barrier coating on the chromium-containing components that reduces or prevents chromium volatilization and acts to protect components that may be susceptible to chromium contamination (e.g., components in fluid communication with the chromium-containing components).
[0088] Therefore, reference Figure 6 , the fuel cell system 10 is an intermediate-temperature solid oxide fuel cell (IT-SOFC) system. The fuel cell stack 20 is a metal-supported IT-SOFC fuel cell stack, as taught in WO-A-2015 / 004419. The fuel cell system 10 has a steady-state 1kW electrical output from the fuel cell stack 20 and includes 121 metal-supported IT-SOFC fuel cells 30. Each fuel cell 30 has an anode side 40, an electrolyte layer 50, and a cathode side 60. Each fuel cell layer in the fuel cell stack is separated by a conductive, airtight metal interconnect plate (interconnector) (not shown). A fuel cell stack end plate and a clamping tool (not shown) are also provided.
[0089] The fuel cell 30 mentioned herein refers to a whole group of 121 fuel cells 30 .
[0090] An electrical load L is applied across the fuel cell 30 .
[0091] The fuel cell stack anode inlet 41 is in fluid communication with the fuel cell anode inlet 41A for anode inlet gas to flow to the anode side 40 of the fuel cell 30. The fuel cell anode outlet 42A is in fluid communication with the fuel cell stack anode exhaust outlet 42 for anode exhaust gas to flow.
[0092] The fuel cell stack cathode inlet 61 is in fluid communication with the fuel cell cathode inlet 61A to allow cathode inlet gas to flow to the cathode side 60 of the fuel cell 30. The fuel cell cathode outlet 62A is in fluid communication with the fuel cell stack cathode exhaust outlet 62 to allow cathode exhaust gas to flow.
[0093] The steam reformer 70 includes a reformer inlet 71 for the anode inlet gas and a reformer outlet 72 for exhausting the anode inlet gas.
[0094] The tail gas burner 80 is in fluid communication with the fuel cell stack anode and cathode exhaust gas outlets 42, 62 and has a tail gas burner exhaust outlet 81, an anode exhaust gas inlet 82, and a cathode exhaust gas inlet 83. The tail gas burner 80 defines a fluid flow path from the fuel cell stack anode and cathode exhaust gas outlets 42, 62 to the tail gas burner exhaust outlet 81 and is configured to burn the anode and cathode exhaust gases and generate a tail gas burner exhaust gas.
[0095] An anode inlet gas fluid flow path A is defined from the fuel source 90 to the vaporizer 100 to the steam reformer 70 to the fuel cell stack anode inlet 41 to the fuel cell anode inlet 41A, ie, the components are in fluid communication with each other.
[0096] An anode exhaust gas fluid flow path B is defined from the fuel cell anode outlet 42A to the fuel cell stack anode exhaust gas outlet 42 to the anode exhaust gas heat exchanger 110 (HX-AOG) to the condenser heat exchanger 120 to the separator 130 to the anode exhaust gas inlet 82 of the tail gas burner 80 .
[0097] The main cathode inlet gas flow path 230 and the air bypass inlet gas flow path 240 have a number of common components and share a common flow path at various locations, which is labeled cathode inlet gas fluid flow path C.
[0098] A main cathode inlet gas flow path 230 is defined from oxidant inlet 140 to blower 210 to valve / separator 220 to anode exhaust heat exchanger 110 to air preheater heat exchanger 150 (HX-APH) to reformer heat exchanger 160 (HX-Ref) to fuel cell stack cathode inlet 61 to fuel cell cathode inlet 61A.
[0099] An air bypass inlet gas flow path 240 is defined from the oxidant inlet 140 to the blower 210 to the valve / separator 220 to the air bypass inlet 190 to the reformer heat exchanger 160 to the fuel cell stack cathode inlet 61 to the fuel cell cathode inlet 61A.
[0100] The valve / separator 220 is controlled by the control device 200 to split the inlet air flow between the main cathode inlet gas flow path 230 and the air bypass inlet gas flow path 240 .
[0101] Thus, the air bypass inlet gas flow path 240 bypasses the anode exhaust heat exchanger 110 and the air preheater heat exchanger 150 .
[0102] In this embodiment, the common components of gas flow paths 230 and 240 (cathode inlet gas fluid flow path C) are therefore (a) oxidant inlet 140 to blower 210 to valve / separator 220, and (b) reformer heat exchanger 160 to fuel cell stack cathode inlet 61 to fuel cell cathode inlet 61A.
[0103] A cathode exhaust gas fluid flow path D is defined from the fuel cell cathode outlet 62A to the fuel cell stack cathode exhaust gas outlet 62 to the cathode exhaust gas inlet 83 of the tail gas burner 80 .
[0104] A tail gas burner exhaust fluid flow path E is defined from the tail gas burner exhaust port 81 to the air preheater heat exchanger 150 to the evaporator heat exchanger 170 (HX-Evap) to the fuel cell system exhaust port 180 .
[0105] The anode exhaust gas heat exchanger 110 is in fluid communication with (i) the fuel cell stack anode exhaust gas outlet 42 (i.e., the fuel cell anode outlet 42A) and the tail gas burner anode exhaust gas inlet 82, and (ii) the oxidant inlet 140 and the fuel cell stack cathode inlet 61 (i.e., the fuel cell cathode inlet 61A), and is arranged to perform heat exchange between the anode exhaust gas from the fuel cell stack 20 and the cathode inlet gas of the fuel cell stack 20.
[0106] The air preheater heat exchanger 150 is in fluid communication with (i) the exhaust gas burner exhaust port 81 and the fuel cell system exhaust port 180, and (ii) the oxidant inlet 140 and the fuel cell stack cathode inlet 61 (i.e., the fuel cell cathode inlet 61A), and is arranged to perform heat exchange between the exhaust gas of the exhaust gas burner 81 and the cathode inlet gas of the fuel cell stack 20.
[0107] The reformer heat exchanger 160 is a parallel flow heat exchanger and is in fluid communication with (i) the oxidant inlet 140 and the fuel cell stack cathode inlet 61 (i.e., the fuel cell cathode inlet 61A), and (ii) the fuel source 90 and the fuel cell stack anode inlet 41 (i.e., the fuel cell anode inlet 41A), and is arranged to perform heat exchange between the cathode inlet gas and the anode inlet gas.
[0108] The evaporator 100 has a fuel inlet 101 for anode inlet gas from a fuel source 90, a water inlet 102 for water from a water source 103, and an evaporator exhaust 104 for exhaust anode inlet gas from the evaporator 100, and is located in the anode inlet gas fluid flow path between the fuel source 90 and the steam reformer 70. The evaporator 100 additionally includes an evaporator heat exchanger 170 located in the tail gas burner exhaust fluid flow path E between the air preheater heat exchanger 150 and the fuel cell system exhaust 180.
[0109] The evaporator heat exchanger 170 is in fluid communication with (i) the tail gas burner exhaust port 81 and the fuel cell system exhaust port 180, and (ii) the fuel source 90 and the water source 103 and the fuel cell stack anode inlet 41 (i.e., the fuel cell anode inlet 41A), and is arranged to perform heat exchange between the tail gas burner exhaust gas and the anode inlet gas and water, thereby generating a steam-fuel mixture for the anode inlet gas of the steam reformer 70.
[0110] The condenser heat exchanger 120 is in fluid communication with (i) the fuel cell stack anode exhaust gas outlet 42 (i.e., the fuel cell anode outlet 42A) and the tail gas burner anode exhaust gas inlet 82, and (ii) the cooling circuit 121, and is arranged to perform heat exchange between the anode exhaust gas from the fuel cell stack 20 and the cooling fluid in the cooling circuit 121.
[0111] The separator 130 is located in the anode exhaust gas fluid flow path between the condenser heat exchanger 120 and the tail gas burner 80 and has a separator condensate outlet 131 , and is adapted to separate condensate from the anode exhaust gas fluid flow path and discharge the condensate via the condensate outlet 131 .
[0112] The control device 200 is connected to the fuel cell stack cathode inlet gas temperature sensor T1, the fuel cell stack cathode exhaust gas temperature sensor T2, the blower 210, and the valve / separator 220. During steady-state operation of the fuel cell system, the control device 200 is configured to maintain the temperature measured by the temperature sensors T1 and T2 at or about the desired temperature.
[0113] The control device 200 is adapted to operate two independent control loops which operate when the cathode inlet gas passes through the cathode inlet gas fluid flow path C.
[0114] In a first control loop, the heating of the cathode inlet gas is controlled. In a second control loop, the mass flow rate of the cathode inlet gas is controlled.
[0115] In use, the fuel cell system 10 goes through three phases: startup, steady state, and shutdown. In the startup phase, the fuel cell stack 20 is cold (or at least below its steady-state operating temperature) and must therefore be heated to reach an operational state. In the steady-state phase, the fuel cell stack 20 is maintained at an operating temperature, as measured by sensors T1 and T2. Electricity is generated and used by a load L across the fuel cell 30. The temperatures detected by the temperature sensors T1 and T2 will be different, and the control device 200 changes the inlet air mass flow rate and the air split between the flow paths 230 and 240 accordingly. In the shutdown phase, power is no longer required from the fuel cell system 10, and a controlled shutdown sequence is initiated. The power demand of the fuel cell stack 20 drops to zero, and the temperature set point of the fuel cell stack air inlet T1 drops, while the air flow rate from the blower 210 increases.
[0116] Figure 7 A schematic cross-section through the coated component is shown. Using the method described in detail below, a stainless steel (chromium-containing) component 402, which may be an interconnect, substrate, or other metal component, is coated with a Pr-containing coating that is deposited on the surface of the component.
[0117] Example
[0118] In an embodiment, the component is coated by sol-gel coating technique (dip coating) using a coating solution with a mixture of rare earth (La or Pr or Tb) salt and chelate (acetylacetone).
[0119] The coating solution used was a mixture of 75% rare earth (Pr or La or Tb) acetylacetonate and 25% rare earth (Pr or La or Tb) nitrate in a 90% by volume ethanol / 10% by volume methoxypropanol mixture.
[0120] The metal part is dipped into the solution and then hung to drain off the excess, leaving a thin film of rare earth oxide precursor after drying. It decomposes into oxides when heated to >400°C. This deposition process can be repeated one or more times.
[0121] After coating, optional drying and decomposition, the metal component is exposed to air at elevated temperatures, causing the coating to react with the natural oxide scale to form a passivation layer.
[0122] The metal components used are stainless steel containing 23% Cr (high La stainless steel specially developed for SOFC), ferritic stainless steel containing 22% Cr, SS441 and SS316 stainless steel components.
[0123] The Cr composition of stainless steel can be:
[0124] SS441: chromium 17.5-18.5%; carbon 0.03%; Si 1.00%; Mn 1.00%; P 0.04%; S 0.015%; Ti 0.1 to 0.6%; Nb (3×C+0.3) to 1.00%; Fe balance;
[0125] Ferritic stainless steel containing 22% Cr: chromium 22.1%;
[0126] SS316: chromium 18.2%; molybdenum 2.2%; carbon 0.05%; nickel 10%;
[0127] Stainless steel containing 23% Cr: Chromium 22-23%; including lanthanum 0.1%.
[0128] It is desirable to use lower cost ferritic stainless steel for the cell substrate. However, the inventors have observed that potential low cost steels not specifically designed for SOFC applications (such as ferritic stainless steel containing 22% Cr) have higher chromium volatilization at high temperatures. This can lead to problems in cell manufacturing or problems during operation that may poison the cathode. It is assumed (without wishing to be bound) that this is due to the lack of reactive elements alloyed in the steel, such as lanthanum or zirconium, which are present in steels specific to SOFCs.
[0129] The present inventors have surprisingly discovered that scale growth and chromium evaporation on 22% Cr ferritic stainless steel during simulated electrolyte firing can be strongly inhibited by coating the surface with a thin film of praseodymium oxide prior to high temperature oxidation. As discussed above, a solution of praseodymium acetylacetonate and praseodymium nitrate dissolved in a 90:10 ethanol / methoxypropanol solution was used to form a continuous film by sol-gel dip coating, followed by a heat treatment to decompose the sol-gel film into oxides.
[0130] In standard SOFC interconnects, a CoCe coating is deposited to inhibit corrosion and chromium evaporation.
[0131] The inventors have surprisingly found that the inventive praseodymium oxide sol-gel coatings deposited on otherwise uncoated SS441 interconnects inhibit oxidation of the steel during subsequent heat treatment and appear to prevent the formation of iron oxide nodules on the surface. Without wishing to be bound, it is believed that these REO coatings can achieve the same results at a lower cost than CoCe coating post-forming because REO forms an outer oxide layer of RE chromite / manganite, which has a lower chromium vapor pressure than the natural oxide scale. In addition, it is expected that the electrical resistance of this protective oxide will be lower than standard coatings, thereby improving performance and potentially reducing degradation.
[0132] Furthermore, coating stainless steels such as SS316 with a thin sol-gel coating of rare earth oxides (e.g., lanthanum oxide or praseodymium oxide or terbium oxide) greatly enhances their resistance to high temperature corrosion after simply dipping the components in solution and allowing them to dry before heat treatment. This may be applicable to balance stacks and balance equipment components, particularly since it may reduce chromium evaporation from surfaces upstream of the stack at a lower cost and process complexity than plating aluminum alloys. Furthermore, this may be more generally applicable in industry (e.g., automotive exhaust systems or chemical plant piping).
[0133] Coating SOFC interconnects
[0134] SOFC interconnects were coated with PrOx and La2O3 sol-gel coatings and then fired at 870°C or 910°C for 2 hours in dry air.
[0135] The process is as follows:
[0136] 1) Dip coating the parts in a metal organic solution of a rare earth salt in ethanol / methoxypropanol;
[0137] 2) Allow the part to stand upright to allow excess solution to drain off and dry at room temperature;
[0138] 3) Heating the component to >450°C to decompose the salt coating into oxides;
[0139] 4) Repeat as needed.
[0140] The samples prepared are shown in Table 1. Table 1 also shows the coating durability data in terms of voltage degradation rate (% / kh). The interconnects were tested at 610°C for 1000 hours in an operating SOFC stack. The voltage degradation appears to be mainly related to the increase in ohmic resistance of the oxide scale on the interconnect. The lanthanum coating has a higher degradation rate.
[0141] Table 1
[0142]
[0143] The interconnect was incorporated into a standard SOFC cell stack and the normalized resistance compared to a standard cell was determined as a function of temperature. Figure 1 shown.
[0144] The PrOx coated parts fired at 870°C had resistance comparable to the standard parts; the parts fired at 910°C had substantially higher resistance.
[0145] The La2O3 coated parts, especially those fired at 910°C, generally had higher resistance.
[0146] Coated SOFC substrate (23% chromium)
[0147] Stainless steel (23% chromium and 0.1% lanthanum) substrates were coated with La2O3 or PrOx (double coating, with IR heating between stages) or TbOx, generally as described above for the interconnects.
[0148] The substrate was incorporated into a standard SOFC cell stack and the performance was determined as a function of temperature. Figures 2 to 4 shown.
[0149] Figure 2 The secant ASR normalized to the standard cell is shown as a function of temperature. The La2O3 coated substrate (curve 1) shows higher resistance over the temperature range, the PrOx coated substrate (curve 2) has poor performance at low temperatures, but has comparable or better performance at >600°C. The TbOx coated substrate (curve 3) has good performance. These results are consistent with those obtained for the interconnects.
[0150] Figure 3 Shows the resistance normalized to a standard cell as a function of temperature.
[0151] The La2O3 coated substrate (curve 1) shows an increase in resistance at higher temperatures.
[0152] The PrOx coated substrate (curve 2) has a lower Rs than the standard cell over the temperature range; the difference increases with increasing temperature.
[0153] The TbOx coated substrate (curve 3) generally has good performance.
[0154] Figure 4 The SecASR normalized to the standard cell is shown as a function of temperature. Both the La2O3 coated substrate (curve 1) and the PrOx coated substrate (curve 2) show higher polarization resistance than the standard cell; the TbOx coated substrate (curve 3) has good or very good performance.
[0155] PrOx appears to provide better results for SOFC applications than La2O3, which appears to form a resistive oxide scale. In addition, PrOx forms a more stable deposition solution. Terbium generally has good performance and similar advantages, most likely due to its similar chemistry (Tb forms a conductive mixed valence oxide, Tb4O7).
[0156] Coated SOFC substrate (22% chromium)
[0157] A 22% chromium ferritic stainless steel substrate was coated with La2O3 or PrOx, substantially as described above for the interconnect.
[0158] The substrates were incorporated into a standard SOFC stack and the ohmic cell resistance normalized to the uncoated substrate (same stainless steel) was determined at 610°C. The PrOx coating resulted in 0.918 and the La2O3 coating 0.921. Thus, the coated substrates resulted in a reduction in ohmic resistance relative to the uncoated substrate.
[0159] Comparison of Chromium Evaporation Rates
[0160] Chromium evaporation rate measurements were performed using the method described in Froitzheim et al., J. Electrochem. Soc., 157(9), B1295 (2010) to measure chromium evaporation from three ferritic stainless steel (23% Cr, 0.1% La) samples. The method involves placing a denuder tube coated with Na2CO3 in fluid communication with the sample. CrO2(OH)2 evaporated from the sample is collected on the denuder tube and converted to thermally stable Na2CrO4. The chromate is then dissolved in water and quantitatively determined.
[0161] The samples investigated are:
[0162] a) The uncoated sample was pre-oxidized in air at 850°C for 2 hours.
[0163] b) La coated samples were pre-oxidized in air at 850°C for 2 hours.
[0164] c) The Pr coated sample was pre-oxidized in air at 850°C for 2 hours.
[0165] The coatings were applied to the specimens generally as discussed above.
[0166] The measurements were carried out at 600°C (rather than 850°C as described by Froitzheim et al.) in flowing air containing 3% water vapor for 1000 hours. Figure 8 shown.
[0167] Chromium evaporation from both coated samples was significantly reduced compared to the uncoated samples, with praseodymium being particularly effective.
[0168] Reference numerals
[0169] 1: Curve of La-based coating
[0170] 2: Curve of Pr-based coating
[0171] 3: Curve of Tb-based coating
[0172] 10: Fuel Cell System
[0173] 20: Fuel Cell Stack
[0174] 30: Fuel Cell
[0175] 41: Anode side fuel cell stack anode inlet
[0176] 41A: Fuel cell anode inlet
[0177] 42: Fuel cell stack anode exhaust gas outlet
[0178] 42A: Fuel cell anode outlet
[0179] 50: Electrolyte layer
[0180] 60: cathode side
[0181] 61: Fuel cell stack cathode inlet
[0182] 61A: Fuel cell cathode inlet
[0183] 62: Fuel cell stack cathode exhaust gas outlet
[0184] 62A: Fuel cell cathode outlet
[0185] 70: Steam reformer
[0186] 71: Recombiner entrance
[0187] 72: Recombiner outlet
[0188] 80: Exhaust burner
[0189] 81: Exhaust burner outlet
[0190] 82: Anode exhaust gas inlet
[0191] 83: Cathode exhaust gas inlet
[0192] 90: Fuel Source
[0193] 100: Evaporator
[0194] 101: Fuel inlet
[0195] 102: Water inlet
[0196] 103: Water Source
[0197] 104: Evaporator outlet
[0198] 110: Anode exhaust gas heat exchanger
[0199] 120: Condenser heat exchanger
[0200] 121: Cooling circuit
[0201] 130: Separator
[0202] 131: Separator condensate outlet
[0203] 140: Oxidant inlet
[0204] 150: Air preheater heat exchanger
[0205] 160: Recombiner heat exchanger
[0206] 161: Recombiner heat exchanger oxidant inlet
[0207] 162: Recombiner heat exchanger oxidant outlet
[0208] 170: Evaporator heat exchanger
[0209] 180: Fuel cell system outlet
[0210] 190: Air bypass inlet
[0211] 200: Control device
[0212] 210: Blower
[0213] 220: Valve / Separator
[0214] 230: Main cathode inlet gas flow path
[0215] 240: Air bypass inlet gas flow path
[0216] 250: Fuel Source
[0217] 260: Air bypass inlet gas flow path
[0218] A: Anode inlet gas flow path
[0219] B: Anode exhaust fluid flow path
[0220] C: Cathode inlet gas fluid flow path
[0221] D: Cathode exhaust fluid flow path
[0222] E: Exhaust gas flow path of tail gas burner
[0223] G: Reformer cathode exhaust fluid flow path
[0224] L: Electrical load
[0225] T1: Fuel cell stack cathode inlet gas temperature sensor
[0226] T2: Fuel cell stack cathode exhaust temperature sensor
[0227] T3: Fuel cell stack anode inlet gas temperature sensor
[0228] 310: Stainless steel components
[0229] 320: coating mixture
[0230] 330: Apply coating mixture
[0231] 340: (optionally) drying
[0232] 350: Heating
[0233] 360: (optionally) repeat step
[0234] 401: Contains Pr coating
[0235] 402: Stainless steel components.
[0236] All publications mentioned in the above specification are incorporated herein by reference. Although the illustrative embodiments of the present invention have been disclosed in detail herein with reference to the accompanying drawings, it should be understood that the present invention is not limited to the precise embodiments and that various changes and modifications may be made by those skilled in the art without departing from the scope of the invention defined by the appended claims and their equivalents.
Claims
1. A method for producing a coated component, the method comprising: a) Provide chromium-containing components, b) providing a coating mixture comprising at least one solvent and a praseodymium source and / or a terbium source, c) contacting at least one surface of the component with the coating mixture, d) optionally, drying the assembly, and e) heating the assembly in an oxidizing atmosphere at 450°C or higher.
2. The method according to claim 1, wherein the praseodymium source and / or terbium source is a Pr(III) source and / or a Tb(III) source.
3. The method of claim 2, wherein the Pr(III) source comprises a Pr(III) salt and / or chelated Pr(III), and / or the Tb(III) source comprises a Tb(III) salt and / or chelated Tb(III).
4. The method according to any one of the preceding claims, wherein the method further comprises repeating steps a) to c), and optionally steps d) and e), thereby producing a coated component having a coating comprising a plurality of layers.
5. A method as claimed in any preceding claim, wherein the coating is electrically conductive.
6. A method as claimed in any one of the preceding claims, wherein the coating has a thickness in the range of 50 nm to 1 μm, preferably the coating has a thickness in the range of 50 nm to 500 nm.
7. The method of any one of the preceding claims, wherein the component comprises a chromium-containing metal alloy.
8. The method of claim 7, wherein the component comprises a chromium-containing ferroalloy.
9. The method of claim 8, wherein the component comprises stainless steel.
10. The method of any one of claims 7 to 9, wherein the alloy comprises 11 wt% or more Cr; optionally, 15 wt% or more Cr; optionally, 17 wt% or more Cr; optionally, 19 wt% or more Cr.
11. A method as claimed in any preceding claim, wherein the coating mixture is in a liquid state and preferably comprises a coating solution.
12. A method as claimed in any one of the preceding claims, wherein the solvent comprises an alcohol, optionally a C1 to C6 alcohol.
13. The method of any one of the preceding claims, wherein the solvent is selected from one or more of ethanol, propanol, and methoxypropanol.
14. The method of any of the preceding claims, wherein contacting at least one surface of the component with the coating mixture comprises dipping the component in the coating mixture and / or spraying the component with the coating mixture.
15. The method of any one of the preceding claims, wherein heating the assembly in an oxidizing atmosphere comprises heating the assembly to a temperature of 500°C or higher, optionally 550°C or higher.
16. A method as claimed in any preceding claim, wherein the oxidizing atmosphere comprises air.
17. The method of any of the preceding claims, wherein the coated component comprises a coated component for use in an apparatus, optionally for operation at temperatures of 450°C or greater.
18. A coated component for a device, obtainable by the method according to any one of claims 1 to 17.
19. A coated component for a device, the coated component comprising a chromium-containing component having at least one surface with a coating comprising at least one layer comprising a praseodymium material and / or a terbium material.
20. The coated component of claim 19, wherein the apparatus is adapted to operate at a temperature of 450°C or greater.
21. The coated component of claim 19 or 20, wherein the coating comprises two or more layers, each layer containing a praseodymium material and / or a terbium material.
22. The coated component for a device as claimed in any one of claims 18 to 21, wherein the device comprises an electrochemical cell.
23. The coated component for a device of claim 22, wherein the component comprises an interconnect, a spacer, a metal plate, or a substrate.
24. The coated component for a device as claimed in any one of claims 18 to 23, wherein the device comprises a system comprising an electrochemical cell stack.
25. The coated component for a device of claim 24, wherein the component comprises a fitting, a fastener, a valve assembly, a pipe, or a heat exchanger.
26. An electrochemical device comprising a coated component, the coated component comprising a chromium-containing component having at least one surface with a coating, the coating comprising at least one layer comprising a praseodymium material and / or a terbium material, optionally wherein the electrochemical device is used to operate at a temperature of 450°C or higher.
27. Use of a coating as a barrier on a chromium-containing component in an electrochemical device, wherein the coating comprises at least one layer comprising a praseodymium material and / or a terbium material.