Conductive paste

By using copper and ABO3-type oxide powder with specific ion radius in the conductive paste, the problem of low internal electrode coverage is solved, and an internal electrode with high coverage is achieved, supporting the large capacity of ceramic capacitors.

CN118901111APending Publication Date: 2024-11-05MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028706.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-26
Filing Date
2023-05-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

When manufacturing laminated ceramic capacitors, the coverage rate of the internal electrodes is easily reduced, which hinders the large capacity. Although the addition of common materials in the prior art has improved, it is still impossible to sinter the sintering temperature of metal particles and ceramic sintering temperature in the conductive paste. Matching leads to insufficient coverage.

Method used

Using conductive pastes containing conductive metal powders of copper and ABO3 type oxide powders of specific ion radius, such as CuTiO3, CoTiO3 and CrTiO3, the sintering temperature of metal particles in the conductive paste of the internal electrodes is adjusted by adjusting the composition of the ceramic powder. Close to the ceramic sintering temperature and improve coverage.

Benefits of technology

The coverage of the internal electrodes is effectively improved, ensuring that even if the internal electrodes are thinned, a high coverage can be maintained, and avoiding hindering the large-capacity of the laminated ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901111A_ABST
    Figure CN118901111A_ABST
Patent Text Reader

Abstract

Provided is a conductive paste for an internal electrode, which is capable of maintaining a relatively high coverage rate even if the internal electrode of a laminated ceramic capacitor is thinned. A conductive paste for forming internal electrodes (4, 5) of a multilayer ceramic capacitor (1) manufactured through a firing step, the conductive paste comprising a conductive metal powder, a ceramic powder, an organic solvent, and an organic binder, the conductive metal powder comprising copper, at least a portion of the ceramic powder is a powder containing an ABO3-type oxide having a specific ionic radius in which the ratio of the ionic radius of an A-site element in ABO3 at the 6-coordinate to the ionic radius of copper at the 6-coordinate is 0.96-1.04.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a conductive paste, and in particular, to a conductive paste for forming internal electrodes of a multilayer ceramic capacitor. Background Art

[0002] Generally, a laminated ceramic capacitor comprises: a laminate having a plurality of laminated dielectric layers containing ceramics, and a plurality of internal electrodes respectively arranged along a plurality of interfaces between the dielectric layers; and a plurality of external electrodes provided on the outer surface of the laminate and electrically connected to the internal electrodes. The internal electrodes comprise a plurality of first internal electrodes and a plurality of second internal electrodes alternately arranged in the stacking direction of the laminate, and the external electrodes comprise a first external electrode electrically connected to the first internal electrode, and a second external electrode electrically connected to the second internal electrode.

[0003] In order to achieve the miniaturization and high capacity of the multilayer ceramic capacitor of this structure, it is required to thin the dielectric layer and the internal electrode and improve the coverage of the internal electrode (electrode continuity). Generally, in the firing process when manufacturing the multilayer ceramic capacitor, the sintering temperature of the conductive metal particles contained in the conductive paste film that should become the internal electrode is lower than the sintering temperature of the ceramic constituting the dielectric layer, so the metal particles contained in the internal electrode are sintered first. This causes the coverage of the internal electrode to decrease. In particular, in the internal electrode that is thinned to a thickness of less than 1μm, there is a problem that the coverage is easy to decrease, and such a decrease in coverage is easy to hinder the increase in capacity.

[0004] Therefore, in order to form thin-layered internal electrodes with high coverage, it is necessary to further increase the sintering temperature of the conductive metal particles contained in the conductive paste film that should become the internal electrodes during the firing process when manufacturing the laminated ceramic capacitor. As a result, the sintering temperature of the metal particles contained in the conductive paste film that should become the internal electrodes can be made close to the temperature at which the ceramic constituting the dielectric layer starts sintering, and the shrinkage timing during sintering can be made close between the internal electrode and the dielectric layer. As a result, the coverage of the internal electrode becomes higher, and a larger capacity can be achieved.

[0005] In order to increase the coverage of the internal electrode and realize a large capacity by the above-mentioned method, it is known to add a ceramic material having a composition similar to that of the ceramic constituting the dielectric layer, that is, a common material, to the conductive paste for forming the internal electrode, as described in, for example, paragraph 0004 of Patent Document 1 (Japanese Patent Publication No. 2016-31807). By adding the common material, the sintering timing of the metal particles contained in the conductive paste film to be the internal electrode can be moved to a higher temperature side, and the sintering temperature of the metal particles contained in the conductive paste film can be made close to the sintering temperature of the ceramic constituting the dielectric layer.

[0006] Prior Art Literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2016-31807 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] However, even if common materials are added to the conductive paste for forming the internal electrodes, it is undeniable that the sintering temperature of the metal particles contained in the conductive paste is still lower than the sintering temperature of the ceramic constituting the dielectric layer, and further improvement is desired. In particular, for example, with respect to the internal electrodes that are thinned to a thickness of 1 μun or less, an effective solution to the problem of reduced coverage that hinders the increase in capacity is strongly required.

[0011] Therefore, the present invention has been made in view of such a problem, and an object of the present invention is to provide a conductive paste for forming internal electrodes capable of maintaining a relatively high coverage even when the internal electrodes are thinned.

[0012] Technical solutions to solve problems

[0013] The present invention is a conductive paste for forming internal electrodes of a stacked ceramic capacitor, comprising conductive metal powder, ceramic powder, an organic solvent and an organic binder. In order to solve the above-mentioned technical problems, it is characterized in that the conductive metal powder contains copper, and at least a part of the ceramic powder is a powder of an ABO3 type oxide of a specific ionic radius, in which the ratio of the ionic radius of an element at the A position in ABO3 at a 6-coordinated state to the ionic radius of copper at a 6-coordinated state is greater than 0.96 and less than 1.04.

[0014] Effects of the Invention

[0015] If the internal electrodes of a multilayer ceramic capacitor are formed by the conductive paste of the present invention, the coverage of the internal electrodes can be increased. Therefore, even if the internal electrodes are thinned, the coverage of the internal electrodes can be maintained high, so that the increase in the capacity of the multilayer ceramic capacitor is not hindered. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 1 is a cross-sectional view schematically showing a multilayer ceramic capacitor 1 to which the conductive paste according to the present invention is applied. DETAILED DESCRIPTION

[0017] Reference Figure 1 , the structure of a multilayer ceramic capacitor 1 to which the conductive paste according to the present invention is applied will be described.

[0018] A laminated ceramic capacitor 1 includes a laminate 2. The laminate 2 includes a plurality of laminated dielectric layers 3 containing ceramics, and a plurality of internal electrodes 4 and 5 arranged along interfaces between the plurality of dielectric layers 3. The internal electrodes 4 and 5 are classified into a plurality of first internal electrodes 4 and a plurality of second internal electrodes 5 arranged alternately in the stacking direction of the laminate 3. A first external electrode 6 and a second external electrode 7 are provided on the outer surface of the laminate 2, more specifically, on each of the opposite end surfaces. The first external electrode 6 is electrically connected to the first internal electrode 4, and the second external electrode 7 is electrically connected to the second internal electrode 5.

[0019] The dielectric layer 3 includes, for example, a ceramic having ABO3 as a main component (A is at least one of Ba, Ca and Sr, and B is at least one of Ti and Zr). In addition, the ceramic may also include the above-mentioned ABO3 as a main component and further include at least one of Mn, Mg, Si, Y, Dy and Gd as a subcomponent.

[0020] The internal electrodes 4 and 5 contain copper as a conductive component. Furthermore, as a characteristic composition, the internal electrodes 4 and 5 contain at least one selected from, for example, CuTiO 3 , CoTiO 3 , and CrTiO 3 . CuTiO 3 , CoTiO 3 , and CrTiO 3 have an ilmenite crystal structure.

[0021] In addition, according to the experimental examples described later, in a preferred embodiment, the dielectric layer 3 includes a ceramic having at least one selected from BaTiO3, SrTiO3 and CaZrO3 as a main component, and the internal electrodes 4 and 5 include copper as a conductive component, and as a ceramic material, include at least one selected from CuTiO3, CoTiO3 and CrTiO3, and if necessary, also include at least one selected from BaTiO3, SrTiO3 and CaZrO3 contained in the dielectric layer 3.

[0022] The external electrodes 6 and 7 are formed, for example, by applying a conductive paste containing Ag or Cu as the main conductive component to the end faces of the stacked body 2 and then sintering it. If necessary, Ni plating, for example, may be performed on the thick film formed by sintering, and Sn plating may be performed thereon.

[0023] The multilayer ceramic capacitor 1 is manufactured, for example, through the following process. First, a ceramic slurry containing raw material powder of a ceramic having the composition as described above is prepared. Next, a suitable sheet forming method is applied to the ceramic slurry to form ceramic green sheets. Next, a conductive paste that should become each of the internal electrodes 4 and 5 is applied to a given ceramic green sheet among the plurality of ceramic green sheets by printing or the like. Next, after stacking the plurality of ceramic green sheets, they are crimped to obtain an unprocessed stack. Next, the unprocessed stack is fired. In this firing process, the ceramic green sheets become dielectric layers 3. Then, external electrodes 6 and 7 are formed on the end faces of the stack 3.

[0024] The conductive paste to be used as the internal electrodes 4 and 5 when manufacturing the above-mentioned multilayer ceramic capacitor 1 is preferably prepared as follows.

[0025] When preparing the conductive paste, a first step is implemented to prepare a ceramic powder slurry containing ceramic powder, an organic solvent and a dispersant, a second step is implemented to prepare a metal powder slurry containing conductive metal powder, an organic solvent and a dispersant, a third step is implemented to prepare an organic vehicle containing an organic resin component and an organic solvent, and a fourth step is implemented to mix the above-mentioned ceramic powder slurry, metal powder slurry and organic vehicle.

[0026] More specifically, in the first step, ceramic powder and a dispersant are mixed in an organic solvent to prepare a ceramic powder slurry.

[0027] As the above-mentioned ceramic powder, for example, a ceramic powder containing at least one selected from CuTiO3, CoTiO3 and CrTiO3 as ABO3 oxides can be used, and sometimes a ceramic powder containing at least one selected from BaTiO3, SrTiO3 and CaZrO3 as common materials can be used.

[0028] The conductive metal powder contained in the metal powder slurry prepared in the second step described later contains copper, so the above-mentioned CuTiO3, CoTiO3 and CrTiO3 as ABO3 oxides become ABO3 type oxides with a specific ionic radius, in which the ratio of the ionic radius of the element at the A position in ABO3 at the 6-coordination position to the ionic radius of copper at the 6-coordination position is greater than 0.96 and less than 1.04.

[0029] According to the ceramic powder containing at least one selected from CuTiO3, CoTiO3 and CrTiO3 as ABO3 oxides, it is possible to suppress the reaction between the copper powder contained in the metal powder slurry prepared in the second step during firing. The ceramic powder may also contain the above-mentioned ABO3 oxide as a main component, and further contain at least one of Mn, Mg, Si, Y, Dy and Gd as a secondary component. In the case of containing such secondary components, the particle growth of the ceramic particles can be further suppressed, and sometimes the sintering of the metal particles can be further effectively suppressed.

[0030] As the dispersant to be mixed with the ceramic powder in the first step, for example, an anionic polymer dispersant can be used, and as the organic solvent, for example, dihydroterpineol can be used.

[0031] In the second step, a metal powder slurry is prepared by mixing a conductive metal powder and a dispersant in an organic solvent. As the conductive metal powder, a powder containing copper or an alloy thereof can be used. As the dispersant and organic solvent used in the second step, the same dispersant and organic solvent as those used in the first step can be used.

[0032] In the third step, an organic vehicle is prepared by mixing an organic resin component with an organic solvent. As the organic resin component, for example, ethyl cellulose resin can be used. The organic solvent used in the third step can also be the same as the organic solvent used in the first step.

[0033] In the fourth step, the ceramic powder slurry, the metal powder slurry and the organic vehicle are mixed. Thus, a conductive paste to be the internal electrodes 4 and 5 is obtained. The conductive paste contains the ceramic powder slurry, and the ceramic powder slurry includes at least one ceramic powder selected from CuTiO3, CoTiO3 and CrTiO3, which are ABO3 oxides with a specific ionic radius, as described above. Therefore, the internal electrodes 4 and 5 provided in the laminated ceramic capacitor 1 manufactured through the firing step become at least one selected from CuTiO3, CoTiO3 and CrTiO3.

[0034] [Experimental example]

[0035] Next, an experimental example conducted to confirm the effects of the present invention will be described.

[0036] In this experimental example, copper powder was prepared as the conductive metal powder contained in the conductive paste for forming the internal electrode.

[0037] On the other hand, as ABO3 oxides of specific ionic radius constituting ceramic powders contained in the conductive paste for forming the internal electrode, in addition to CuTiO3, CoTiO3 and CrTiO3, BaTiO3, CaZrO3 and SrTiO3 are prepared. In Table 1, "crystal structure", "coordination number", "A-site element" and "ionic radius" are shown for these ABO3 oxides. In addition, Ba, Ca and Sr are 12-coordinated in the original perovskite structure, but Ba, Ca and Sr are also 6-coordinated when they are continuously dissolved in the position of the 6-coordinated elements (Cu, Co, Cr) of the ilmenite structure, so the "ionic radius" in Table 1 shows the value under 6-coordinated.

[0038] [Table 1]

[0039] Table 1

[0040]

[0041] Hereinafter, Experimental Examples 1, 2, and 3 which were carried out by changing the ceramic raw material constituting the dielectric layer will be described.

[0042] (Experimental Example 1) Main component of ceramic constituting dielectric layer: BaTiO3

[0043] 1. Preparation of BaTiO3-based ceramic raw materials constituting the dielectric layer

[0044] As starting materials, powders of BaCO3 and TiO2 as main components were weighed, mixed for 72 hours by ball mill, and then heat treated for 2 hours at a maximum temperature of 1000°C to obtain heat-treated powder. On the other hand, powders of MnO, Dy2O3, MgO, SiO2 and BaCO3 were prepared as auxiliary components, and the heat-treated powders were weighed so that the auxiliary component powders had a composition ratio of 100BaTiO3+0.5Mn+1.0Dy+1.0Mg+1.0Si+2.0Ba. These auxiliary component powders were added to the heat-treated powders, mixed for 24 hours by ball mill, and then dried to obtain BaTiO3-based ceramic raw material powders.

[0045] 2. Preparation of conductive paste for internal electrode formation

[0046] As ceramic powders contained in the conductive paste for forming the internal electrode, powders of "ABO 3 oxides" shown in Table 2 described later and the BaTiO 3 -based ceramic raw material powder for the dielectric layer were used.

[0047] The powders of these "ABO3 oxides" and BaTiO3-based ceramic raw material powders were weighed to obtain the "addition ratio" shown in Table 2. These powders, dihydropinene as an organic solvent, and anionic polymer dispersant as a dispersant were premixed in a medium-free stirring mill, and then dispersed in a medium stirring mill to prepare a ceramic powder slurry (first step).

[0048] Meanwhile, copper powder as a conductive metal powder, dihydroterpineol as an organic solvent, and an anionic polymer dispersant as a dispersant were dispersed using a three-roll mill to prepare a metal powder slurry (second step).

[0049] Furthermore, ethyl cellulose resin as an organic resin component and dihydroterpineol as an organic solvent were mixed to obtain an organic vehicle (third step).

[0050] Next, the metal powder slurry and the ceramic powder slurry are added to the organic vehicle and mixed and dispersed to prepare a conductive paste for forming an internal electrode (fourth step).

[0051] Table 2 shows the ratio of the ionic radius of the A-site element at 6 coordination to the ionic radius of the copper to be included in the internal electrode at 6 coordination, i.e., "ionic radius ratio (A-site element / metallic copper)". In addition, for sample 7, the ionic radius of the Ba element at 6 coordination shown in Table 1 is shown. Relative to the ionic radius of copper under hexacoordination ratio.

[0052] 3. Fabrication of multilayer ceramic capacitors

[0053] A ceramic slurry containing the BaTiO3-based ceramic raw material powder prepared in the above 1 is prepared, and then a ceramic green sheet is formed by applying a doctor blade method to the ceramic slurry. Next, the conductive paste for forming the internal electrode prepared in the above 2 is applied to a given ceramic green sheet among the plurality of ceramic green sheets by screen printing. Next, a plurality of ceramic green sheets are stacked and then crimped to obtain an unprocessed laminate. Next, the unprocessed laminate is fired. Then, external electrodes are formed on the end faces of the sintered laminate to produce a laminated ceramic capacitor as a sample.

[0054] 4. Evaluation

[0055] [Table 2]

[0056] Table 2

[0057]

[0058] The internal electrode and the dielectric layer located at the center of the stacked body in the height direction of the stacked ceramic capacitor serving as a sample were separated from each other by electric field separation.

[0059] Next, the central part (the position of 1 / 2 in the width direction and 1 / 2 in the length direction) of the exposed internal electrode was observed at a magnification of 100 times using a microscope. Then, the obtained image was analyzed to find the ratio of the area occupied by the conductor film as the internal electrode in the exposed part, which was given as the "coverage" shown in Table 2. Samples with a "coverage" of 80% or more were judged to be good and were marked with "○" in the "Evaluation" column, and samples with a "coverage" of less than 80% were judged to be poor and were marked with "×" in the "Evaluation" column.

[0060] 5. Inspection

[0061] The "evaluation" of samples 1 to 6 in Table 2 is "○". In these samples 1 to 6, the internal electrode contains any one of CuTiO3, CoTiO3 and CrTiO3 as the ABO3 oxide. In addition, the internal electrode contains copper as a conductive component.

[0062] Here, if we focus on the ionic radius, first, as shown in the item "CuTiO3" in Table 1, the ionic radius of copper under hexacoordination is On the other hand, as ABO3 oxides contained in the internal electrodes of samples 1 to 6, the ionic radii of the elements at the A-site of CuTiO3, CoTiO3, and CrTiO3 in the hexacoordination state are shown in Table 1. as well as

[0063] In samples 1 to 6 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 in hexa-coordination to the ionic radius of copper in hexa-coordination, that is, the "ionic radius ratio" was 0.96 or more and 1.04 or less.

[0064] As such, the CuTiO3, CoTiO3, and CrTiO3 as ABO3 oxides in samples 1 to 6 have an ionic radius of 6-coordinated elements at the A position in ABO3 equal to or close to the ionic radius of 6-coordinated copper, which is a conductive metal to be included in the internal electrode, and therefore have an energy difference of 0 or less with the copper in the internal electrode, so they will not be ejected from the internal electrode portion but remain, thus playing a role in improving the heat resistance of the internal electrode. As a result, in samples 1 to 6, it is estimated that the coverage rate becomes as high as 84% ​​or more.

[0065] In addition, as in samples 4 to 6, the addition ratio of CuTiO3, CoTiO3, and CrTiO3 is not necessarily 100%, and as long as it is 10% or more, the effect of improving the coverage is confirmed compared with the case where none of CuTiO3, CoTiO3, and CrTiO3 is included. In addition, in Experimental Example 1, it is also noted that the coverage of samples 4 to 6 in which the addition ratio of CuTiO3, CoTiO3, and CrTiO3 is 10% shows a value equal to the coverage of samples 1 to 3 in which the addition ratio is 100%.

[0066] In contrast to these samples, in sample 7 evaluated as "×", only BaTiO3, which is a common material, is added to the internal electrode. In this case, Ba, which is an element at the A position in ABO3 of the perovskite structure, is 12-coordinated, but when solid-dissolving in the A position of the ilmenite structure, it is necessary to compare the ionic radius at the 6-coordinated position, which is the coordination number of the A position of the ilmenite structure. The ionic radius of Ba at the 6-coordinated position is shown in Table 1. Therefore, the ratio of the ionic radius of Ba in hexacoordination to the ionic radius of copper in hexacoordination, that is, the "ionic radius ratio" is 1.75. Therefore, the "ionic radius ratio" deviates from the range of 0.96 to 1.04, and the coverage is reduced to 74%.

[0067] In Sample 7, the "ion radius ratio" deviated from the range of 0.96 to 1.04, which is presumably because BaTiO 3 was ejected from the internal electrode portion, the heat resistance of the internal electrode was not improved, and the coverage was reduced.

[0068] (Experimental Example 2) Main component of ceramic constituting dielectric layer: CaZrO3

[0069] 1. Preparation of CaZrO3-based ceramic raw materials constituting the dielectric layer

[0070] As starting materials, powders of CaCO3 and ZrO2 as main components and powders of MnO, SiO2 and MgO as auxiliary components were weighed, mixed for 72 hours in a ball mill, and then heat treated at a maximum temperature of 1000°C for 2 hours to obtain CaZrO3-based ceramic raw material powder.

[0071] 2. Preparation of conductive paste for internal electrode formation

[0072] As ceramic powders contained in the conductive paste for forming the internal electrode, powders of "ABO 3 oxides" shown in Table 3 described later and the CaZrO 3 -based ceramic raw material powder for the dielectric layer were used.

[0073] These "ABO3 oxide" powders and CaZrO3-based ceramic raw material powders were weighed so as to achieve the "addition ratio" shown in Table 3, and a conductive paste for forming internal electrodes was prepared through the same steps as in the above-mentioned Experimental Example 1.

[0074] Table 3 shows the “ion radius ratio (A-site element / metal copper)” as in Table 2. In addition, for Sample 17, the ion radius of the Ca element in the hexacoordinated state shown in Table 1 is shown. Relative to the ionic radius of copper under hexacoordination ratio.

[0075] 3. Fabrication of multilayer ceramic capacitors

[0076] A ceramic slurry containing the CaZrO3-based ceramic raw material powder prepared in the above 1 was prepared, and then a ceramic green sheet was formed by applying a doctor blade method to the ceramic slurry. Thereafter, a laminated ceramic capacitor serving as a sample was prepared through the same steps as in Experimental Example 1.

[0077] 4. Evaluation

[0078] [Table 3]

[0079] Table 3

[0080]

[0081] According to the same procedure as in Experimental Example 1, the “coverage ratio” was obtained as shown in Table 3, and evaluation was performed in the same manner.

[0082] 5. Inspection

[0083] The "evaluation" of samples 11 to 16 in Table 3 is "○". In these samples 11 to 16, the internal electrode contains any one of CuTiO3, CoTiO3 and CrTiO3 as the ABO3 oxide. In addition, the internal electrode contains copper as a conductive component.

[0084] Here, if we focus on the ionic radius, first, as shown in the item "CuTiO3" in Table 1, the ionic radius of copper under hexacoordination is On the other hand, as ABO3 oxides contained in the internal electrodes of samples 11 to 16, the ionic radii of the elements at the A-site of CuTiO3, CoTiO3, and CrTiO3 in the hexacoordination state are shown in Table 1. as well as

[0085] In samples 11 to 16 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 in hexacoordination to the ionic radius of copper in hexacoordination, that is, the "ionic radius ratio" was 0.96 or more and 1.04 or less.

[0086] As described above, the CuTiO3, CoTiO3 and CrTiO3 as ABO3 oxides in samples 11 to 16 have an ionic radius of the element at the A position in ABO3 at a 6-coordinated position that is equal to or close to the ionic radius of copper as the conductive metal to be contained in the internal electrode at a 6-coordinated position. Therefore, the energy difference with the copper in the internal electrode is 0 or becomes smaller, so they will not be ejected from the internal electrode portion but remain, thereby playing a role in improving the heat resistance of the internal electrode. As a result, in samples 11 to 16, it is estimated that the coverage rate is increased to more than 81%.

[0087] In addition, as in samples 14 to 16, the addition ratio of CuTiO3, CoTiO3 and CrTiO3 does not necessarily have to be 100%. As long as it is 10% or more, the effect of improving the coverage is confirmed compared with the case where none of CuTiO3, CoTiO3 and CrTiO3 is included.

[0088] In contrast to these samples, in sample 17, which was evaluated as "×", only CaZrO3, which is a common material, was added to the internal electrode. In this case, Ca, which is an element at the A site in ABO3 of the perovskite structure, is 12-coordinated, but when solid-dissolving in the A site of the ilmenite structure, it is necessary to compare the ionic radius at the 6-coordinated site, which is the coordination number of the A site of the ilmenite structure. The ionic radius of Ca at the 6-coordinated site is shown in Table 1. Therefore, the ratio of the ionic radius of Ca in hexacoordination to the ionic radius of copper in hexacoordination, that is, the "ionic radius ratio" is 1.30. Therefore, the "ionic radius ratio" deviates from the range of 0.96 to 1.04, and the coverage is reduced to 72%.

[0089] In Sample 17, the “ion radius ratio” deviated from the range of 0.96 to 1.04, presumably because CaZrO 3 was ejected from the internal electrode portion, the heat resistance of the internal electrode was not improved, and the coverage was reduced.

[0090] (Experimental Example 3) Main component of ceramic constituting dielectric layer: SrTiO3

[0091] 1. Preparation of SrTiO3-based ceramic raw materials constituting the dielectric layer

[0092] As starting materials, powders of SrCO3 and TiO2 as main components and powders of MnO, SiO2 and MgO as auxiliary components were weighed, mixed for 72 hours in a ball mill, and then heat treated at a maximum temperature of 1000°C for 2 hours to obtain SrTiO3-based ceramic raw material powder.

[0093] 2. Preparation of conductive paste for internal electrode formation

[0094] As ceramic powders contained in the conductive paste for forming the internal electrode, powders of "ABO 3 oxides" shown in Table 4 described later and the SrTiO 3 -based ceramic raw material powder for the dielectric layer were used.

[0095] These "ABO3 oxide" powders and SrTiO3-based ceramic raw material powders were weighed so as to achieve the "addition ratio" shown in Table 4, and a conductive paste for forming an internal electrode was prepared through the same steps as in the above-mentioned Experimental Example 1.

[0096] Table 4 shows the "ion radius ratio (A-site element / metal copper)" as in Table 2. In addition, for Sample 27, the ion radius of the Sr element in the hexacoordinated state shown in Table 1 is shown. Relative to the ionic radius of copper under hexacoordination ratio.

[0097] 3. Fabrication of multilayer ceramic capacitors

[0098] A ceramic slurry containing the SrTiO3-based ceramic raw material powder prepared in the above 1 was prepared, and then a ceramic green sheet was formed by applying a doctor blade method to the ceramic slurry. Thereafter, a laminated ceramic capacitor serving as a sample was prepared through the same steps as in Experimental Example 1.

[0099] 4. Evaluation

[0100] [Table 4]

[0101] Table 4

[0102]

[0103] According to the same procedure as in Experimental Example 1, the “coverage ratio” was obtained as shown in Table 4, and evaluation was performed in the same manner.

[0104] 5. Inspection

[0105] The "evaluation" of samples 21 to 26 in Table 4 is "○". In these samples 21 to 26, the internal electrode contains any one of CuTiO3, CoTiO3 and CrTiO3 as the ABO3 oxide. In addition, the internal electrode contains copper as a conductive component.

[0106] Here, if we focus on the ionic radius, first, as shown in the item "CuTiO3" in Table 1, the ionic radius of copper under hexacoordination is On the other hand, as ABO3 oxides contained in the internal electrodes of samples 21 to 26, the ionic radii of the elements at the A-site of CuTiO3, CoTiO3, and CrTiO3 in the hexacoordination state are shown in Table 1. as well as

[0107] In samples 21 to 26 evaluated as "○", the ratio of the ionic radius of the element at the A site in ABO3 in hexacoordination to the ionic radius of copper in hexacoordination, that is, the "ionic radius ratio" was 0.96 or more and 1.04 or less.

[0108] As described above, the CuTiO3, CoTiO3 and CrTiO3 as ABO3 oxides in samples 21 to 26 have an ionic radius of the element at the A position in ABO3 at a 6-coordinated position that is equal to or close to the ionic radius of copper as the conductive metal that should be included in the internal electrode at a 6-coordinated position. Therefore, the energy difference with the copper in the internal electrode is 0 or becomes smaller, so they will not be ejected from the internal electrode portion but remain, thereby playing a role in improving the heat resistance of the internal electrode. As a result, in samples 21 to 26, it is estimated that the coverage rate is increased to more than 80%.

[0109] In addition, as in samples 24 to 26, the addition ratio of CuTiO3, CoTiO3 and CrTiO3 does not necessarily have to be 100%. As long as it is 10% or more, the effect of improving the coverage is confirmed compared with the case where none of CuTiO3, CoTiO3 and CrTiO3 is included.

[0110] In contrast to these samples, in sample 27, which was evaluated as "×", only SrTiO3, which is a common material, was added to the internal electrode. In this case, Sr, which is an element at the A site in ABO3 of the perovskite structure, is 12-coordinated, but when solid-dissolving in the A site of the ilmenite structure, it is necessary to compare the ionic radius at the 6-coordinated site, which is the coordination number of the A site of the ilmenite structure. The ionic radius of Sr at the 6-coordinated site is shown in Table 1. Therefore, the ratio of the ionic radius of Sr in hexacoordination to the ionic radius of copper in hexacoordination, that is, the "ionic radius ratio" is 1.53. Therefore, the "ionic radius ratio" deviates from the range of 0.96 to 1.04, and the coverage is reduced to 70%.

[0111] In Sample 27, the "ion radius ratio" deviated from the range of 0.96 to 1.04, which is presumably because SrTiO 3 was ejected from the internal electrode portion, the heat resistance of the internal electrode was not improved, and the coverage was reduced.

[0112] In the above-described experimental examples 1 to 3, the powder containing an ABO3 type oxide of a specific ionic radius as at least a part of the ceramic powder contained in the conductive paste is at least one selected from CuTiO3, CoTiO3 and CrTiO3, but may be a material other than these. That is, with respect to the ABO3 type oxide of a specific ionic radius, any ABO3 type oxide may be used as long as the ratio of the ionic radius of the element at the A position in ABO3 at 6 coordination to the ionic radius of the copper contained in the conductive paste at 6 coordination is 0.96 or more and 1.04 or less.

[0113] The present invention may be implemented as follows.

[0114] <1>

[0115] A conductive paste is a conductive paste for forming internal electrodes of a multilayer ceramic capacitor, comprising conductive metal powder, ceramic powder, an organic solvent and an organic binder, wherein:

[0116] The conductive metal powder comprises copper,

[0117] At least a part of the ceramic powder is a powder of an ABO3 type oxide of a specific ionic radius, wherein the ratio of the ionic radius of the element at the A-site in ABO3 at hexacoordination to the ionic radius of copper at hexacoordination is 0.96 to 1.04.

[0118] <2>

[0119] according to <1> The conductive paste, wherein

[0120] The ABO3-type oxide having the specific ionic radius has an ilmenite crystal structure.

[0121] <3>

[0122] according to <2> The conductive paste, wherein

[0123] The ABO3-type oxide of the specific ionic radius is at least one selected from CuTiO3, CoTiO3 and CrTiO3.

[0124] <4>

[0125] according to <1> to <3> The conductive paste described in any one of the preceding claims, wherein:

[0126] More than 10 volume % of the ceramic powder is powder containing an ABO3 type oxide having the specific ionic radius, and the remainder of the ceramic powder is powder containing at least one selected from BaTiO3, SrTiO3 and CaZrO3 as a main component.

[0127] Description of Reference Numerals

[0128] 1: Multilayer ceramic capacitor;

[0129] 2: laminate;

[0130] 3: Dielectric layer;

[0131] 4, 5: internal electrodes;

[0132] 6, 7: External electrodes.

Claims

1. A conductive paste for forming an internal electrode of a multilayer ceramic capacitor, comprising conductive metal powder, ceramic powder, an organic solvent and an organic binder, wherein: The conductive metal powder comprises copper, At least a part of the ceramic powder is a powder of an ABO3 type oxide of a specific ionic radius, wherein the ratio of the ionic radius of the element at the A-site in ABO3 at hexacoordination to the ionic radius of copper at hexacoordination is 0.96 to 1.

04.

2. The conductive paste according to claim 1, wherein The ABO3-type oxide having the specific ionic radius has an ilmenite crystal structure.

3. The conductive paste according to claim 2, wherein: The ABO3-type oxide of the specific ionic radius is at least one selected from CuTiO3, CoTiO3 and CrTiO3.

4. The conductive paste according to any one of claims 1 to 3, wherein More than 10 volume % of the ceramic powder is powder containing an ABO3 type oxide having the specific ionic radius, and the remainder of the ceramic powder is powder containing at least one selected from BaTiO3, SrTiO3 and CaZrO3 as a main component.