Oxide semiconductor film, thin film transistor, sputtering target, and oxide sintered body

By using oxide semiconductor films of elements such as In, Zn, La or Nd in thin film transistors, the content and crystal phase structure of metal elements are controlled, and the problems of low carrier mobility and insufficient ambient temperature stability are solved, and the problem of low carrier mobility and insufficient ambient temperature stability is achieved. Improvement of carrier mobility and optimization of ambient temperature stability.

CN118901142APending Publication Date: 2024-11-05KOBE STEEL LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028723.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-07
Filing Date
2023-03-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing IGZO amorphous oxide semiconductor thin film transistor has low carrier mobility and insufficient ambient temperature stability, making it difficult to meet the requirements of high mobility and heat resistance.

Method used

An oxide semiconductor film with elements such as In, Zn, La or Nd is used to control the content of In, Zn and X within a specific range to form crystal phases such as Zn3In2O6 or Zn4In2O7 to improve carrier mobility and ambient temperature stability.

Benefits of technology

It achieves improved carrier mobility and excellent ambient temperature stability, and is suitable for high-performance thin film transistor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901142A_ABST
    Figure CN118901142A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide an oxide semiconductor film capable of simultaneously improving the carrier mobility of a thin film transistor and the stability with respect to ambient temperature. An oxide semiconductor film according to one embodiment of the present invention is an oxide semiconductor film used in a thin film transistor, the oxide semiconductor film containing, as metal elements, In and Zn, and an element X, which is either La or Nd, the In content, the Zn content, and the X content of all the metal elements being 30 atm% to 90 atm% inclusive, 9 atm% to 70 atm% inclusive, and 0.0001 atm% to 2 atm% inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an oxide semiconductor film, a thin film transistor, a sputtering target, and an oxide sintered body. Background Art

[0002] Thin film transistors (TFT) are becoming popular as active elements for flat panel displays such as organic EL (Organic Electro-Luminescence) displays. As such thin film transistors, top gate type (staggered type) and bottom gate type (anti-staggered type) are known.

[0003] In addition to high carrier mobility, thin film transistors are also required to have stability that is independent of ambient temperature. In particular, in recent years, thin film transistors have been used in car displays and the like, and therefore require stability in harsher environments than ever before.

[0004] As a semiconductor film constituting the thin film transistor, an amorphous oxide semiconductor film is used. Compared with general-purpose amorphous silicon, amorphous oxide semiconductors can improve carrier mobility. In addition, amorphous oxide semiconductors have a large optical band gap and can be formed at a low temperature. Therefore, it is expected that amorphous oxide semiconductors will be used in, for example, next-generation displays that require large-scale, high-resolution, and high-speed driving, and in substrates made of resins with low heat resistance (see Patent Documents 1 and 2).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2010-219538

[0008] Patent Document 2: International Publication No. 2009 / 81885 Summary of the invention

[0009] Problems to be solved by the invention

[0010] Patent Document 1 describes an In-Ga-Zn-O (IGZO) amorphous oxide semiconductor composed of In, Ga, Zn, and O. However, the carrier mobility of a TFT using this IGZO amorphous oxide semiconductor is 10 cm 2 / Vs or less.

[0011] In contrast, Patent Document 2 describes a high-mobility oxide that does not contain Ga. Patent Document 2 describes that in an oxide composed of In, Zn and X, when X = Zr, Hf, Ge, Si, Ti, Mn, W, Mo, V, Cu, Ni, Co, Fe, Cr or Nb, the amount of X added is 0.01 < X / (In+Zn+X) < 0.2, or when X = Al, B, Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, the amount of X added is 0.02 < X / (In+Zn+X) < 0.3, and high mobility can be obtained. However, Patent Document 2 does not describe stability to ambient temperature. Furthermore, in Patent Document 2, X is defined within a wide range, and even within the above range, there are problems such as low mobility and insufficient heat resistance, and it is difficult to say that an appropriate composition has been developed.

[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an oxide semiconductor film capable of improving both the carrier mobility and the stability with respect to the ambient temperature of a thin film transistor.

[0013] Means of solving the problem

[0014] An oxide semiconductor film according to one embodiment of the present invention is an oxide semiconductor film for a thin film transistor, and contains In and Zn as metal elements, and an element X which is either La or Nd, wherein the contents of the above-mentioned In, the above-mentioned Zn and the above-mentioned X in all the metal elements are In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, and X: 0.0001 atm% or more and 2 atm% or less.

[0015] Effects of the Invention

[0016] An oxide semiconductor film according to one embodiment of the present invention can improve both the carrier mobility and the stability with respect to the ambient temperature of a thin film transistor. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a schematic cross-sectional view showing a top-gate thin film transistor according to one embodiment of the present invention.

[0018] Figure 2 This is a flowchart showing a method for producing an oxide sintered body according to one embodiment of the present invention.

[0019] Figure 3 This is a flowchart showing a method for producing a sputtering target according to one embodiment of the present invention.

[0020] Figure 4This is a diagram showing the measurement results of the static characteristics (Id-Vg characteristics) of the No. 4 top-gate thin film transistor.

[0021] Figure 5 This is a diagram showing the measurement results of the static characteristics (Id-Vg characteristics) of the top-gate thin-film transistor No. 13.

[0022] Figure 6 This is a backscattered electron image of the oxide sintered body of No. 14.

[0023] Figure 7 These are the analysis results of the X-ray diffraction spectrum of the oxide sintered body No. 14.

[0024] Figure 8 This is a backscattered electron image of the oxide sintered body of No. 15.

[0025] Fig. 9 yes Figure 8 A magnified portion of a backscattered electron image.

[0026] Fig.10 These are the analysis results of the X-ray diffraction spectrum of the oxide sintered body No. 15.

[0027] Fig.11 This is a backscattered electron image of the oxide sintered body of No. 16.

[0028] Fig.12 These are the analysis results of the X-ray diffraction spectrum of the oxide sintered body No. 16.

[0029] Fig.13 This is a backscattered electron image of the oxide sintered body of No. 17.

[0030] Fig.14 These are the analysis results of the X-ray diffraction spectrum of the oxide sintered body No. 17.

[0031] Fig.15 This is a graph showing the relationship between the relative density of an oxide sintered body and the sintering temperature.

[0032] Fig.16 This is a backscattered electron image of the oxide sintered body of No. 18.

[0033] Fig.17 These are the analysis results of the X-ray diffraction spectrum of the oxide sintered body No. 18. DETAILED DESCRIPTION

[0034] [Description of Embodiments of the Invention]

[0035] First, embodiments of the present invention will be described by way of examples.

[0036] An oxide semiconductor film according to one embodiment of the present invention is an oxide semiconductor film for a thin film transistor, and contains In and Zn as metal elements, and an element X which is either La or Nd, wherein the contents of the above-mentioned In, the above-mentioned Zn and the above-mentioned X in all the metal elements are: In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, and X: 0.0001 atm% or more and 2 atm% or less.

[0037] In the above-mentioned Patent Document 2, it is described that in a field effect transistor having a semiconductor layer composed of a composite oxide, by controlling the addition amount of X to a certain amount or less, it is possible to suppress the decrease in mobility and improve thermal stability and heat resistance, wherein the composite oxide includes In and Zn, and one or more elements X selected from the group consisting of Zr, Hf, Ge, Si, Ti, Mn, W, Mo, V, Cu, Ni, Co, Fe, Cr, Nb, Al, B, Sc, Y and lanthanide elements (La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). On the other hand, the inventors of the present invention have made a discovery during their intensive research that the environmental temperature resistance varies depending on the type of X. On this basis, the inventors of the present invention have found that the elements X that can take into account both the improvement of carrier mobility and the environmental temperature resistance are La and Nd. According to the knowledge of the present inventors, the oxide semiconductor film can improve both the carrier mobility and the stability to the ambient temperature of the thin film transistor by controlling the contents of the above-mentioned In and Zn and the element X which is either La or Nd within the above-mentioned range.

[0038] As the content of the above-mentioned In and the above-mentioned Zn in all metal elements, preferably In: 55 atm% or more and 80 atm% or less, Zn: 20 atm% or more and 50 atm% or less. In this way, the content of the above-mentioned In and the above-mentioned Zn in all metal elements is within the above-mentioned range, which can promote the optimization of the carrier mobility and threshold voltage of the thin film transistor.

[0039] As a metal element, it also contains element Y which is either Sn or Ge, and the content of the above Y in all metal elements is Y: 0.0001 atm% or more and 4 atm% or less. In this way, by also containing element Y which is either Sn or Ge as a metal element, and the content of the above Y in all metal elements is within the above range, the optical band gap can be increased. As a result, the characteristics of a high-mobility material with a high carrier density can be stabilized, the threshold voltage of a thin film transistor can be optimized, and the stability to the ambient temperature can be improved.

[0040] As the content of the above-mentioned element Y in all metal elements, it is more preferable that Y: is higher than 1 atm% and less than 2 atm%. In this way, by making the content of the above-mentioned element Y in all metal elements within the above-mentioned range, the threshold voltage of the thin film transistor can be further optimized and the stability to the ambient temperature can be further improved.

[0041] A thin film transistor according to another embodiment of the present invention includes the oxide semiconductor film.

[0042] Since the thin film transistor includes the oxide semiconductor film, the carrier mobility is high and the stability with respect to the ambient temperature is excellent.

[0043] Another embodiment of the sputtering target of the present invention is a sputtering target for forming an oxide semiconductor film used for a thin film transistor, wherein the target contains In and Zn as metal elements, and an element X as either La or Nd, and the contents of the above-mentioned In, Zn and X in all the metal elements are: In: 30 atm% to 90 atm%; Zn: 9 atm% to 70 atm%; X: 0.0001 atm% to 2 atm%.

[0044] In addition, another embodiment of the sputtering target of the present invention is a sputtering target for forming an oxide semiconductor film used for a thin film transistor, wherein the sputtering target contains In and Zn as metal elements, and an element X as either La or Nd, and the contents of the above-mentioned In and the above-mentioned Zn in all metal elements are, In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, and has an In oxide crystal phase, a ZnIn oxide crystal phase and an XIn oxide crystal phase, and the composition of the above-mentioned ZnIn oxide crystal phase is Zn3In2O6 and / or Zn4In2O7.

[0045] The sputtering target can manufacture an oxide semiconductor film capable of improving both the carrier mobility and the stability with respect to the ambient temperature of a thin film transistor.

[0046] Another embodiment of the oxide sintered body of the present invention is an oxide sintered body for forming an oxide semiconductor film used for a thin film transistor, wherein the oxide sintered body contains In and Zn as metal elements, and an element X as either La or Nd, and the contents of the above-mentioned In and the above-mentioned Zn in all metal elements are, In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, and has an In oxide crystal phase, a ZnIn oxide crystal phase and an XIn oxide crystal phase, and the composition of the above-mentioned ZnIn oxide crystal phase is Zn3In2O6 and / or Zn4In2O7.

[0047] This oxide sintered body can produce an oxide semiconductor film that can simultaneously improve the carrier mobility and stability of a thin film transistor with respect to ambient temperature.

[0048] [Details of Embodiments of the Invention]

[0049] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. In addition, regarding the numerical values ​​recorded in this specification, only one of the upper limit and the lower limit may be adopted, or the upper limit and the lower limit may be arbitrarily combined. In this specification, the numerical range from the upper limit to the lower limit that can be combined is all described as an appropriate range.

[0050] [Oxide semiconductor film]

[0051] The oxide semiconductor film is used for a thin film transistor. The oxide semiconductor film contains In (indium) and Zn (zinc) as metal elements, and an element X that is either La (lanthanum) or Nd (neodymium). In the oxide semiconductor film, the contents of the above-mentioned In, the above-mentioned Zn, and the above-mentioned X in all the metal elements are: In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, and X: 0.0001 atm% or more and 2 atm% or less.

[0052] The oxide semiconductor film can be used for any type of top-gate and bottom-gate thin film transistors, but is preferably used for, for example, a top-gate thin film transistor, which has an oxide semiconductor film, a gate insulating film, and a gate electrode in order on one side of a substrate. More specifically, the oxide semiconductor film is directly stacked on the above-mentioned substrate, or is indirectly stacked on the above-mentioned substrate via a buffer layer, etc. In addition, a gate electrode is arranged on the oxide semiconductor film via a gate insulating film. In addition, a conductive region (S / D region) is provided on the oxide semiconductor film, and a protective film and a source-drain electrode are arranged in the S / D region.

[0053] (In)

[0054] In is an element that helps to improve electrical conductivity (conductivity). The greater the content of In, the more the conductivity of the oxide semiconductor film is improved, and the more the carrier density and carrier mobility are improved. As the lower limit of the In content in all metal elements, as described above, it is 30atm%, preferably 50atm%, and more preferably 55atm%. On the other hand, as the upper limit of the In content in all metal elements, as described above, it is 90atm%, preferably 80atm%, and more preferably 78atm%. If the content of In is lower than the above lower limit, the carrier mobility may not be fully obtained. On the contrary, if the content of In is higher than the above upper limit, the device characteristics become unstable, the threshold voltage may show a large negative value, or the heat resistance may be insufficient.

[0055] (Zn)

[0056] Zn is an element that affects the processing characteristics of the oxide semiconductor film. As the lower limit of the Zn content in all metal elements, as mentioned above, it is 9atm%, preferably 10atm%, and more preferably 20atm%. On the other hand, as the upper limit of the Zn content in all metal elements, as mentioned above, it is 70atm%, preferably 65atm%, and more preferably 50atm%. If the Zn content is lower than the above lower limit, the In content is relatively large, the device characteristics become unstable, the threshold voltage may show a large negative value, or the heat resistance may be insufficient. On the contrary, if the Zn content is higher than the above upper limit, partial crystallization occurs, and it may be difficult to ensure the uniformity of the oxide semiconductor film.

[0057] (X)

[0058] As mentioned above, the oxide semiconductor film contains any one of La and Nd as element X. The inventors of the present invention have found that as an element X for improving stability to ambient temperature, it is preferred to contain any one of La and Nd. In particular, it has been found that by containing any one of La and Nd at a ratio of less than 2 atm%, it is possible to take into account both the improvement of carrier mobility and the stability to ambient temperature. As the lower limit of the X content in all metal elements, it is 0.0001 atm%, preferably 0.1 atm%, as mentioned above. On the other hand, as the upper limit of the X content in all metal elements, it is 2 atm%, preferably 1.6 atm%. If the content of X is lower than the above lower limit, the stability to ambient temperature may not be fully improved. On the contrary, if the content of X is higher than the above upper limit, the carrier density is insufficient, and it may be difficult to achieve high mobility as a thin film transistor.

[0059] The oxide semiconductor film may contain only one of La and Nd as the element X, or may contain both La and Nd. When the oxide semiconductor film contains both La and Nd as the element X, La and Nd may be contained in the above ranges respectively, or only one of La and Nd may be contained in the above range. In addition, when both La and Nd are contained as the element X, it is particularly preferred that the total content of La and Nd is within the above range.

[0060] (Y)

[0061] In the oxide semiconductor film, in addition to In, Zn and X, as a metal element, it may also contain an element Y as any one of Sn (tin) and Ge (germanium). The oxide semiconductor film can increase the optical band gap by containing element Y. As a result, it is possible to stabilize the characteristics of a high-mobility material with a high carrier density, optimize the threshold voltage of a thin film transistor, and improve the stability to ambient temperature. As the lower limit of the Y content in all metal elements, it is preferably 0.0001atm%, more preferably 0.1atm%, and further preferably higher than 1atm%. On the other hand, as the upper limit of the Y content in all metal elements, it is preferably 4atm%, more preferably 2atm%. If the content of Y is lower than the above lower limit, the optical band gap may not be fully increased. On the contrary, if the content of Y is higher than the above upper limit, the carrier density is insufficient, and it may be difficult to achieve a high mobility as a thin film transistor.

[0062] The oxide semiconductor film may contain only one of Sn and Ge or both of them as the element Y. When the oxide semiconductor film contains both of Sn and Ge as the element Y, Sn and Ge may be contained in the above ranges respectively, or only one of them may be contained in the above range. In addition, when both of Sn and Ge are contained as the element Y, it is particularly preferred that the total content of Sn and Ge is within the above range.

[0063] In the oxide semiconductor film, the elements other than the above are O (oxygen) and inevitable impurities. Inevitable impurities may be contained due to raw materials, materials, manufacturing equipment, etc. As such inevitable impurities, Al, Pb, Si, Fe, Ni, Ti, Mg, Cr and Zr can be listed, for example. The content of inevitable impurities in the oxide semiconductor film is preferably less than 1% by mass of each element, and more preferably less than 500 ppm by mass. In addition, in such a structure, the content of the above-mentioned In, the above-mentioned Zn, the above-mentioned X and the above-mentioned Y in the oxide semiconductor film can also refer to the proportion of all elements excluding O.

[0064] The average thickness of the oxide semiconductor film can be determined based on the conditions under which the leakage current can be turned off when used as a switching element. The lower limit of the average thickness of the oxide semiconductor film is preferably 10 nm, and more preferably 15 nm. On the other hand, the upper limit of the above average thickness is preferably 60 nm, and more preferably 50 nm. In addition, the so-called "average thickness" in this specification means the average value of the thickness of any five points.

[0065] The oxide semiconductor film is preferably an amorphous structure, or an amorphous structure that is at least partially crystallized. That is, the oxide forming the oxide semiconductor film is preferably amorphous, or at least partially crystallized amorphous. When the oxide semiconductor film has such a structure, it is also possible to fully improve the carrier mobility compared to general amorphous silicon. In addition, by having such a structure, the optical band gap can be easily and reliably increased.

[0066] The oxide semiconductor film can obtain the above-mentioned amorphous structure by, for example, controlling the gas pressure within a range of 1 mTorr to 5 mTorr and performing surface treatment with plasma or reducing gas after film formation. In addition, the so-called "amorphous" means that there is no clear diffraction peak from the crystal, which can be measured using an X-ray diffraction device or the like.

[0067] The upper limit of the thin film resistance of the oxide semiconductor film (the thin film resistance of the S / D region after surface treatment after film formation) is preferably 1.0 kΩ / □, and more preferably 0.5 kΩ / □. In the thin film transistor, the region (S / D region) between the source and drain electrodes and the channel portion in the oxide semiconductor film is made conductive. The oxide semiconductor film can easily and reliably realize the conductive nature of the S / D region by making the above-mentioned thin film resistance after surface treatment below the above-mentioned upper limit. In addition, the thin film resistance of general IGZO oxide semiconductor films is mostly higher than 1.0 kΩ / □. In such existing oxide semiconductor films, if a thermal process is applied in the manufacturing process of the thin film transistor, the tendency of increased thin film resistance is significantly manifested. This is because oxide semiconductor films are usually conductive due to the deficiency of constituent elements. For example, when the amount of oxygen is reduced due to surface treatment and conductive, if the oxygen is filled from the surrounding insulating layer by heat treatment, the defect is restored and the conductivity tends to be lost. Here, the above-mentioned thin film resistance can be a value measured by (a four-probe resistance measuring instrument).

[0068] <Advantages>

[0069] In the above-mentioned Patent Document 2, it is described that in a field effect transistor having a semiconductor layer composed of a composite oxide, by controlling the addition amount of X to a certain amount or less, it is possible to suppress the decrease in mobility while improving thermal stability and heat resistance, wherein the composite oxide includes In and Zn, and one or more elements X selected from the group consisting of Zr, Hf, Ge, Si, Ti, Mn, W, Mo, V, Cu, Ni, Co, Fe, Cr, Nb, Al, B, Sc, Y and lanthanide elements (La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu). On the other hand, the inventors of the present invention have made a discovery during their intensive research that the environmental temperature resistance varies depending on the type of X. On this basis, the inventors of the present invention have found that the elements X that can take into account both the improvement of carrier mobility and the environmental temperature resistance are La and Nd. According to the knowledge of the present inventors, the oxide semiconductor film can improve both the carrier mobility and the stability to the ambient temperature of the thin film transistor by controlling the contents of the above-mentioned In and Zn and the element X which is either La or Nd within the above-mentioned range.

[0070] [Thin Film Transistor]

[0071] Figure 1 In the figure, as an example of a thin film transistor having the above-mentioned oxide semiconductor film, a top-gate thin film transistor 10 (hereinafter referred to as "thin film transistor 10") is shown. The thin film transistor 10 has the oxide semiconductor film 1 having the above-mentioned structure. In more detail, the thin film transistor 10 includes: a substrate 2; a buffer layer 3 stacked on the substrate 2; the oxide semiconductor film 1 stacked on the buffer layer 3; a gate insulating film 4 stacked on the oxide semiconductor film 1; a gate electrode 5 stacked on the gate insulating film 4; a source-drain electrode 6 and a protective film 7 stacked on the conductive S / D region of the oxide semiconductor film 1. The thin film transistor 10 is configured in a display such as an organic EL display.

[0072] (Substrate)

[0073] The substrate 2 is not particularly limited, but a glass substrate and a silicon substrate can be cited. Examples of glass used for the glass substrate include alkali-free glass, high strain point glass, soda-lime glass, etc. In addition, as the substrate 2, a metal substrate such as a stainless steel film, a resin substrate such as a polyethylene terephthalate (PET) film, etc. can also be used.

[0074] The average thickness of the substrate 2 is preferably 0.001 mm or more and 10 mm or less from the viewpoint of processability. The size and shape of the substrate 2 can be set according to the size of the display and the like.

[0075] (Buffer layer)

[0076] As the buffer layer 3, for example, a silicon oxide film can be cited. The buffer layer 3 can be formed by a CVD (Chemical Vapor Deposition) method or a PECVD (Plasma Enhanced Chemical Vapor Deposition) method. In addition, since the buffer layer 3 is provided to improve the adhesion between the substrate 2 and the oxide semiconductor film 1 and to suppress the diffusion of impurities from the substrate 2 to the oxide semiconductor film 1, it is not a layer required for operation and can be omitted.

[0077] (Oxide semiconductor film)

[0078] The oxide semiconductor film 1 can be formed, for example, by a sputtering method using a sputtering target. The sputtering target used to form the oxide semiconductor film 1 is itself an embodiment of the present invention. In addition, the sputtering target itself can be formed using an oxide sintered body as an embodiment of the present invention. The oxide semiconductor film 1 is patterned by photolithography or the like after film formation. In addition, after this patterning, it is preferably subjected to heat treatment (pre-annealing treatment) in order to improve the film quality. The oxide sintered body and the sputtering target are described below.

[0079] 〔Oxide sintered body〕

[0080] An oxide sintered body according to one embodiment of the present invention contains In and Zn as metal elements, and an element X as either La or Nd, wherein the contents of the above-mentioned In, the above-mentioned Zn, and the above-mentioned X in the total metal elements are: In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, and X: 0.0001 atm% or more and 2 atm% or less. In addition, an oxide sintered body according to another embodiment of the present invention contains In and Zn as metal elements, and an element X as either La or Nd, wherein the contents of the above-mentioned In and the above-mentioned Zn in the total metal elements are: In: 30 atm% or more and 90 atm% or less, and Zn: 9 atm% or more and 70 atm% or less, and has an In oxide crystal phase, a ZnIn oxide crystal phase, and an XIn oxide crystal phase, wherein the composition of the above-mentioned ZnIn oxide crystal phase is Zn3In2O6 and / or Zn4In2O7.

[0081] In the oxide sintered body, the ZnIn oxide crystal phase has Zn3In2O6 crystal phase and / or Zn4In2O7 crystal phase as main components. The ZnIn oxide crystal phase may have both Zn3In2O6 crystal phase and Zn4In2O7 crystal phase, or may have only one of them. As the composition of the In oxide crystal phase, for example, In2O3 can be listed. As the composition of the XIn oxide crystal phase, for example, XInO3 can be listed. In the ZnIn oxide crystal phase, a lamellar pattern (striped pattern or dotted pattern) can also be formed.

[0082] The oxide sintered body may further contain an element Y which is either Sn or Ge as a metal element. The elements other than the above elements in the oxide sintered body (In, Zn, X, and elements other than Y contained as required) are O and inevitable impurities. The content of each element in the oxide sintered body may be the same as the range described in connection with the oxide semiconductor film 1.

[0083] The oxide sintered body can be Figure 2 That is, the method for manufacturing the oxide sintered body comprises the following steps: a step of weighing raw material powder (weighing step S1); a step of mixing the raw material powder weighed in the weighing step S1 (mixing step S2); a step of drying and granulating the mixture obtained in the mixing step S2 (drying and granulating step S3); a step of molding the granulated powder obtained in the drying and granulating step S3 (molding step S4); a step of sintering the molded powder obtained in the molding step S4 (sintering step S5).

[0084] In the weighing step S1, metal oxides such as In2O3, ZnO and X2O3 are weighed in such a manner as to achieve a desired content [atm %]. In the mixing step S2, the raw material powder and water weighed in the weighing step S1, and the binder and dispersant added as needed, are added to a nylon container using zirconium oxide balls as a medium, and mixed and crushed with a ball mill to obtain a slurry. In the drying and granulation step S3, the slurry obtained in the mixing step S2 is dried, and the obtained dry powder is sieved to obtain a granulated powder. In addition, the drying and granulation step S3 can also be performed using a spray dryer. In the molding step S4, the granulated powder obtained in the drying and granulation step S3 is filled into a mold to obtain a molding powder. In the sintering step S5, an oxide sintered body is manufactured using, for example, a normal pressure sintering method or a hot pressing method.

[0085] 〔Sputtering target〕

[0086] A sputtering target according to one embodiment of the present invention contains In and Zn as metal elements, and an element X as either La or Nd, wherein the contents of the above-mentioned In, the above-mentioned Zn, and the above-mentioned X in the total metal elements are: In: 30 atm% to 90 atm%, Zn: 9 atm% to 70 atm%, and X: 0.0001 atm% to 2 atm%. In addition, a sputtering target according to another embodiment of the present invention contains In and Zn as metal elements, and an element X as either La or Nd, wherein the contents of the above-mentioned In and the above-mentioned Zn in the total metal elements are: In: 30 atm% to 90 atm%, and Zn: 9 atm% to 70 atm%, and has an In oxide crystal phase, a ZnIn oxide crystal phase, and an XIn oxide crystal phase, wherein the composition of the above-mentioned ZnIn oxide crystal phase is Zn3In2O6 and / or Zn4In2O7.

[0087] The sputtering target may further contain an element Y as either Sn or Ge as a metal element. The elements other than the above elements in the sputtering target (In, Zn, X, and elements other than Y contained as required) are O and inevitable impurities. The composition (crystal structure) and the content of each element of the sputtering target may be the same as those of the oxide sintered body.

[0088] The sputtering target is formed by Figure 3 The sputtering target is manufactured according to the above-mentioned procedure. That is, the manufacturing method of the sputtering target comprises the following steps: a step of weighing raw material powder (weighing step S1); a step of mixing the raw material powder weighed in the weighing step S1 (mixing step S2); a step of drying and granulating the mixture obtained in the mixing step S2 (drying and granulating step S3); a step of molding the granulated powder obtained in the drying and granulating step S3 (molding step S4); a step of sintering the molded powder obtained in the molding step S4 (sintering step S5); a step of processing the oxide sintered body obtained in the sintering step S5 into a desired size (processing step S6); a step of bonding the oxide sintered body (target) processed in the processing step S6 to a backing plate (bonding step S7). The weighing step S1, mixing step S2, drying and granulating step S3, molding step S4 and sintering step S5 in the manufacturing method of the sputtering target can be performed according to the above-mentioned procedure using the manufacturing method of the oxide sintered body. That is, the sputtering target can be formed using the above-mentioned oxide sintered body and can have the same composition as the above-mentioned oxide sintered body. In the processing step S6, the above-mentioned oxide sintered body is processed by, for example, machining. In the bonding step S7, the target material is bonded to a backing plate made of, for example, Cu.

[0089] (Gate insulation film)

[0090] The gate insulating film 4 is formed on the oxide semiconductor film 1 after the above-mentioned pre-annealing treatment. Examples of the gate insulating film 4 include silicon oxide films, silicon nitride films, silicon oxynitride films, metal oxide films such as Al2O3 and Y2O3, etc. The gate insulating film 4 can be formed using a CVD method or a PECVD method. The gate insulating film 4 can be a single layer or a multilayer of more than two layers. When the gate insulating film 4 is a multilayer of more than two layers, it is preferred that the first layer and the second and subsequent layers have different compositions.

[0091] The lower limit of the average thickness of the gate insulating film 4 is preferably 50 nm, and more preferably 100 nm. On the other hand, the upper limit of the average thickness of the gate insulating film 4 is preferably 300 nm, and more preferably 250 nm. If the above average thickness is lower than the above lower limit, the withstand voltage of the gate insulating film 4 may be insufficient. On the contrary, if the above average thickness is higher than the above upper limit, the capacity of the capacitor formed between the gate electrode 5 and the oxide semiconductor film 1 may be insufficient, and the leakage current is insufficient. In addition, when the gate insulating film 4 is multilayer, the so-called "average thickness of the gate insulating film" refers to the average thickness of the entire gate insulating film.

[0092] (Gate Electrode)

[0093] The gate electrode 5 has conductivity. The gate electrode 5 is formed, for example, by performing a heat treatment (annealing treatment) on the oxide semiconductor film 1 after forming the gate insulating film 4. The gate electrode 5 is not particularly limited, but metals such as Al and Cu with low resistivity, and high melting point metals such as Mo, Cr, and Ti with high heat resistance, or alloys thereof can be preferably used.

[0094] The lower limit of the average thickness of the gate electrode 5 is preferably 50 nm, and more preferably 80 nm. If the average thickness is less than the lower limit, the resistance of the gate electrode 5 increases, and there is a possibility that the power consumption due to the gate electrode 5 increases. On the other hand, the upper limit of the average thickness of the gate electrode 5 is preferably 500 nm, and more preferably 400 nm, from the viewpoint of processability.

[0095] The gate insulating film 4 and the gate electrode 5 are patterned by photolithography or the like after the gate electrode 5 is formed.

[0096] (Protective film)

[0097] The protective film 7 is formed after patterning the gate insulating film 4 and the gate electrode 5 and then performing surface treatment on the oxide semiconductor film 1. The surface treatment is performed to make the S / D regions of the oxide semiconductor film 1 conductive, and can be performed by, for example, ion implantation, element diffusion, reduction with a reducing gas, plasma treatment, etc.

[0098] Examples of the protective film 7 include silicon oxide films, silicon nitride films, silicon oxynitride films, metal oxide films such as Al2O3 and Y2O3, etc. The protective film 7 can be formed by CVD and PECVD methods. After the protective film 7 is formed, contact holes are formed by photolithography or the like.

[0099] (Source-Drain Electrode)

[0100] The source-drain electrode 6 has conductivity. The source-drain electrode 6 covers a portion of the protective film 7 and fills the contact hole. By so configuring, the source-drain electrode 6 is electrically connected to the oxide semiconductor film 1 at both ends of the channel of the thin film transistor 10 .

[0101] The source-drain electrode 6 is not particularly limited, but metals with low resistivity such as Al and Cu, high melting point metals with high heat resistance such as Mo, Cr, and Ti, or alloys thereof can be preferably used.

[0102] The lower limit of the average thickness of the source-drain electrode 6 is preferably 100 nm, and more preferably 150 nm. If the average thickness is lower than the lower limit, the resistance of the source-drain electrode 6 increases, and there is a possibility that the power consumption due to the source-drain electrode 6 increases. On the other hand, the upper limit of the average thickness of the source-drain electrode 6 is preferably greater than the total thickness of the gate insulating film 4 and the gate electrode 5, and is preferably 1000 μm, and more preferably 800 μm, for example.

[0103] After the source-drain electrode 6 is formed, it is patterned by photolithography or the like.

[0104] <Characteristics of Thin Film Transistors>

[0105] (Threshold voltage drift)

[0106] The upper limit of the threshold voltage drift (the absolute value of the difference between the threshold voltage at 23°C and the threshold voltage at 100°C) of the thin film transistor 10 is preferably 3.5V, more preferably 3.0V, further preferably 2.5V, and particularly preferably 1.5V. If the threshold voltage drift is higher than the upper limit, the stability to the ambient temperature may be insufficient. In addition, the lower limit of the threshold voltage drift of the thin film transistor 10 is not particularly limited and can be 0V. In addition, the so-called "threshold voltage" means that the leakage current of the transistor is 10 -9 A's gate voltage.

[0107] <Advantages>

[0108] Since the thin film transistor 10 includes the oxide semiconductor film 1 , the carrier mobility is high and the stability with respect to the ambient temperature is excellent.

[0109] This sputtering target is suitable for manufacturing the oxide semiconductor film 1 .

[0110] The oxide sintered body is suitable for manufacturing the oxide semiconductor film 1 .

[0111] [Other embodiments]

[0112] The above embodiments do not limit the configuration of the present invention. Therefore, the above embodiments may be omitted, replaced or added to the components of each part of the above embodiments based on the description of this specification and technical common sense, and these should be interpreted as all belonging to the scope of the present invention.

[0113] For example, the specific structure of the thin film transistor is not limited to Figure 1 For example, the protective layer may be a multilayer structure having a plurality of insulating layers stacked thereon. In addition, the thin film transistor may also be a bottom gate type.

[0114] Example

[0115] Hereinafter, the present invention will be described in detail based on Examples, but the present invention is not to be limitedly interpreted based on the description of these Examples.

[0116] <Test Example 1>

[0117] [Fabrication of top-gate thin film transistor]

[0118] According to the following procedures, make Figure 1 First, a 250nm thick SiO2 film was formed as a buffer layer by CVD on a glass substrate (Eagle 2000 manufactured by Eagle) having a diameter of 4 inches and a thickness of 0.7 mm under the following film forming conditions.

[0119] (Film Formation Conditions of Buffer Layer)

[0120] Carrier gas: a mixture of SiH4 and N2O

[0121] Film forming power density: 0.96W / cm 2

[0122] Film forming temperature: 320℃

[0123] Air pressure during film formation: 133Pa

[0124] Next, an In-Zn-X-O film or an In-Zn-X-Y-O film containing metal elements in the proportions described in Table 1 was formed by sputtering to form an oxide semiconductor film having a thickness of 40 nm. In addition, the content analysis of the metal elements in each oxide semiconductor film was performed by separately forming an oxide semiconductor film having a thickness of 100 nm on a glass substrate in the same manner as described above. The analysis was performed by ICP (Inductively Coupled Plasma) emission spectroscopy using "CIROS MarkII" manufactured by Rigaku Corporation.

[0125] Next, after the oxide semiconductor film is formed, the oxide semiconductor film is patterned by photolithography and wet etching. In addition, it can be confirmed that there is no residue caused by wet etching in all oxide semiconductor films No. 1 to No. 13, and it can be properly etched. After this patterning, in order to improve the film quality, the oxide semiconductor film is heat treated (pre-annealing treatment). The pre-annealing treatment is performed at 350° C. for 1 hour in an atmospheric atmosphere.

[0126] After this pre-annealing treatment, a gate insulating film is formed on the oxide semiconductor film by a CVD method under the following film formation conditions. In addition, in order to improve the film quality of the oxide semiconductor film, heat treatment (annealing treatment) is performed in the air at 350° C. for 1 hour.

[0127] (Film Formation Conditions of Gate Insulation Film)

[0128] Carrier gas: a mixture of SiH4 and N2O

[0129] Film forming power density: 0.96W / cm 2

[0130] Film forming temperature: 270℃

[0131] Air pressure during film formation: 133Pa

[0132] Next, a gate electrode composed of a Mo metal film with a thickness of 100 nm was formed and patterned by photolithography and wet etching. In addition, the gate insulating film was patterned by dry etching using the gate electrode as a mask. After that, the surface of the oxide semiconductor film was irradiated with hydrogen plasma for 15 seconds to make the S / D regions of the oxide semiconductor film conductive.

[0133] After the above plasma irradiation, a protective layer was formed by CVD method under the following film forming conditions. Thereafter, contact holes for detection for transistor characteristic evaluation were formed on the protective layer by photolithography and dry etching. In addition, source and drain electrodes were formed and patterned by photolithography and wet etching, and finally heat treated (post-annealing treatment) at 250°C in a nitrogen atmosphere for 30 minutes to obtain a thin film transistor.

[0134] (Film formation conditions of protective layer)

[0135] Carrier gas: a mixture of SiH4 and N2O

[0136] Film forming power density: 0.96W / cm 2

[0137] Film forming temperature: 250℃

[0138] Air pressure during film formation: 133Pa

[0139] [Evaluation of static characteristics]

[0140] For the thin film transistors No. 1 to No. 13, the drain current (Id)-gate voltage (Vg) characteristics (Id-Vg characteristics) were measured under the following conditions using a probe and a semiconductor parameter analyzer (“4200SCS” manufactured by Keithley).

[0141] Gate voltage: -30V~30V (step length 0.25V)

[0142] Source voltage: 0V

[0143] Drain voltage: 10V

[0144] Substrate temperature: room temperature (23°C)

[0145] <Carrier mobility>

[0146] Carrier mobility μ FE [cm 2 / Vs], in the saturation region of the above static characteristics (Vg>Vd-Vth), according to the following formula (1): FE Calculate, where the gate voltage is Vg[V], the threshold voltage is Vth[V], the drain current is Id[A], the channel length is L[m], the channel width is W[m], and the capacity of the gate insulating film is C ox [F]. The calculation results are shown in Table 1.

[0147] [Formula 1]

[0148]

[0149] <Threshold voltage>

[0150] The threshold voltage [V] is calculated based on the above static characteristics when the transistor leakage current is 10 -9 The value of the gate voltage of A. The calculation results are shown in Table 1.

[0151] <S value>

[0152] The S value [V / decade] is the minimum value of the gate voltage change required to increase the drain current by one order of magnitude calculated based on the above static characteristics. The calculation results are shown in Table 1.

[0153] <Threshold voltage drift>

[0154] The static characteristics were measured under the same conditions as above except that the substrate temperature was set to 100°C. The absolute value of the difference between the threshold voltage at 23°C and the threshold voltage at 100°C was calculated as the threshold voltage shift [V]. The results are shown in Table 1. The static characteristics measurement results of No. 4 are shown in Table 1. Figure 4 The static characteristics of No.13 are shown in Figure 5 In. Figure 5 As shown in Figure 13, the leakage current becomes too large at 100°C because the current is greater than 10% of the calculated threshold voltage. -9 AThe threshold voltage cannot be calculated, so the threshold voltage drift cannot be measured.

[0155]

Table 1

[0156]

[0157] [Evaluation results]

[0158] As shown in Table 1 and Figure 4 , Figure 5 As shown, No. 1 to No. 8 have an oxide semiconductor film containing In and Zn and an element X which is either La or Nd, and the contents of In, Zn and X in all metal elements are In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, and X: 0.0001 atm% or more and 2 atm% or less, so the carrier mobility is higher than 30 cm 2 / Vs, and the threshold voltage drift is less than 3.5 V. This threshold voltage drift can be used as an indicator of stability with respect to the ambient temperature.

[0159] On the other hand, No. 9 to No. 11 have insufficient carrier mobility because the content of X exceeds 2 atm %. Also, No. 12 and No. 13 do not contain any La or Nd as the element X, so the threshold voltage drift is large and the stability with respect to the ambient temperature is insufficient.

[0160] <Test Example 2>

[0161] [Preparation of oxide sintered body by pressureless sintering]

[0162] based on Figure 2The oxide sintered bodies No. 14 to No. 17 were produced by the pressureless sintering method according to the process. First, the metal oxides of In2O3, ZnO and Nd2O3 were weighed so that the content of metal elements in the obtained oxide sintered bodies was as shown in Table 2. Then, the weighed raw material powders, water, binder and dispersant were added to a nylon jar using zirconium oxide balls as a medium, and mixed and crushed with a ball mill for 3 hours. Then, the obtained slurry was dried with a hot plate, and sieved with a sieve to obtain granulated powders of In2O3, ZnO and Nd2O3. Then, the granulated powder was filled into a molding die, and a molded body was obtained by pressurizing with a cold isostatic press at a molding pressure of 294 MPa and a holding time of 3 minutes. Then, the molded body was sintered at 1500°C in the atmosphere for 2 hours to produce an oxide sintered body.

[0163]

Table 2

[0164]

[0165] 〔Crystal structure〕

[0166] SEM-EDX analysis and X-ray diffraction spectrum analysis were performed on the oxide sintered bodies of No. 14 to No. 17. Regarding No. 14, its SEM backscattered electron image shows Figure 6 In the X-ray diffraction spectrum analysis results are shown in Figure 7 In. Figure 6 and Figure 7 As shown, the oxide sintered body of No. 14 is composed of two crystal phases, In2O3 and Zn3In2O6.

[0167] Regarding No.15, its SEM backscattered electron image shows Figure 8 In the X-ray diffraction spectrum analysis results are shown in Fig.10 In addition, Figure 8 A partial enlargement of the SEM backscattered electron image is shown in Fig. 9 In. Figures 8 to 10 As shown, the oxide sintered body of No. 15 contains 0.7 atm% of Nd and has a crystal phase of NdInO3 in addition to In2O3 and Zn3In2O6. In addition, in No. 15, a lamellar pattern can be confirmed in the Zn3In2O6 crystal phase.

[0168] Regarding No.16, its SEM backscattered electron image shows Fig.11 In the X-ray diffraction spectrum analysis results are shown in Fig.12 In. Fig.11 and Fig.12As shown, the oxide sintered body of No. 16 contains 1.9 atm% Nd and has a NdInO3 crystal phase in addition to In2O3 and Zn3In2O6. In addition, the proportion of the NdInO3 crystal phase is larger in No. 16 than in No. 15. In addition, a lamellar pattern can be confirmed in the Zn3In2O6 crystal phase in No. 16.

[0169] Regarding No.17, its SEM backscattered electron image shows Fig.13 In the X-ray diffraction spectrum analysis results are shown in Fig.14 In. Fig.13 and Fig.14 As shown, the oxide sintered body of No. 17 contains 4.0 atm% Nd, and in addition to the crystal phases of In2O3, Zn3In2O6, and NdInO3, a fourth crystal phase (assumed to be Zn2In2O5) composed of an oxide having an equal ratio of Zn to In is formed. In addition, in No. 17, a lamellar pattern can be confirmed in the Zn3In2O6 crystal phase.

[0170] <Test Example 3>

[0171] [Production of oxide sintered body by hot pressing]

[0172] based on Figure 2 The process of hot pressing is used to produce oxide sintered bodies. In Test Example 3, the metal oxides of In2O3, ZnO and Nd2O3 are weighed so that the content of metal elements in the obtained oxide sintered bodies is as shown in Table 3. The raw material powders are mixed in the same procedure as in Test Example 2, and dried, granulated and molded. The granulated powder is hot-pressed at a pressure of 30 MPa, a sintering temperature of 880°C to 1120°C, and a sintering time of 3 to 5 hours to produce an oxide sintered body. The relationship between the relative density of the obtained oxide sintered body and the sintering temperature is shown in Fig.15 middle.

[0173]

Table 3

[0174]

[0175] like Fig.15 As shown in Figure 1, as the sintering temperature increases, the relative density of the oxide sintered body increases. However, if the sintering temperature is too high, the dissolution of the metal component increases, making it difficult to control the composition of the obtained oxide sintered body. From this point of view, an oxide sintered body obtained by hot pressing at a sintering temperature of 1000°C was obtained as the oxide sintered body No. 18. Regarding No. 18, its SEM backscattered electron image shows Fig.16 The X-ray diffraction spectrum analysis results show that Fig.17 In. Fig.16 and Fig.17 As shown, the oxide sintered body of No. 18 has crystal phases of In2O3, Zn4In2O7 and NdInO3.

[0176] 〔Production of sputtering targets〕

[0177] according to Figure 3 The oxide sintered body of No. 18 was machined into a diameter of 50.8 mm and a thickness of 5 mm by the process shown in the figure to make a target. The relative density of the obtained target was 90.3%. Next, the target was bonded to a backing plate made of Cu with In to make a sputtering target (InZnNd oxide sputtering target). The content of the metal elements in the sputtering target (more specifically, the above-mentioned target) was analyzed by ICP emission spectrometry. The results are shown in Table 4.

[0178]

Table 4

[0179]

[0180] As shown in Table 4, it was confirmed that the sputtering target could be produced within ±1.0 atm% relative to the prepared composition. In addition, when the adhesion rate of this sputtering target was measured by ultrasonic testing, the adhesion rate was 100%. In addition, the warpage of the target was 0.1 mm, and the position deviation of the target was 0.2 mm.

[0181] Industrial Applicability

[0182] As described above, the oxide semiconductor film of one embodiment of the present invention is suitable for improving both the carrier mobility and the stability with respect to the ambient temperature of a thin film transistor.

[0183] Explanation of symbols

[0184] 1 Oxide semiconductor film

[0185] 2 Substrate

[0186] 3 Buffer layer

[0187] 4 Gate insulation film

[0188] 5. Gate electrode

[0189] 6 Source and drain electrodes

[0190] 7. Protective film

[0191] 10 Top-gate thin film transistor

[0192] P In2O3 crystal phase

[0193] Q Zn3In2O6 crystal phase

[0194] R NdInO3 crystal phase

[0195] S fourth crystal phase

[0196] T Zn4In2O7 crystal phase

Claims

1. An oxide semiconductor film, which is an oxide semiconductor film used for a thin film transistor, wherein: As metal elements, it contains: In and Zn; The element X is either La or Nd, The contents of In, Zn and X in all metal elements are: In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, X: 0.0001 atm% or more and 2 atm% or less.

2. The oxide semiconductor film according to claim 1, wherein The content of the In and Zn in all metal elements is, In: 55 atm% or more and 80 atm% or less, Zn: 20 atm % or more and 50 atm % or less.

3. The oxide semiconductor film according to claim 1 or claim 2, wherein: As a metal element, Y, which is either Sn or Ge, is also contained. The content of Y in all metal elements is Y: 0.0001 atm % or more and 4 atm % or less.

4. The oxide semiconductor film according to claim 3, wherein The content of the element Y in all metal elements is: Y: higher than 1 atm % and less than 2 atm %. 5 . A thin film transistor comprising the oxide semiconductor film according to claim 1 . 6 . A thin film transistor comprising the oxide semiconductor film according to claim 2 . 7 . A thin film transistor comprising the oxide semiconductor film according to claim 3 . 8 . A thin film transistor comprising the oxide semiconductor film according to claim 4 .

9. A sputtering target for forming an oxide semiconductor film used in a thin film transistor, wherein: As metal elements, it contains: In and Zn; The element X is either La or Nd, The contents of In, Zn and X in all metal elements are: In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, X: 0.0001 atm% or more and 2 atm% or less.

10. A sputtering target for forming an oxide semiconductor film used in a thin film transistor, wherein: As metal elements, it contains: In and Zn; The element X is either La or Nd, The content of the In and Zn in all metal elements is, In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, And has In oxide crystal phase, ZnIn oxide crystal phase and XIn oxide crystal phase, The composition of the ZnIn oxide crystal phase is Zn3In2O6 and / or Zn4In2O7.

11. An oxide sintered body, which is an oxide sintered body used for forming an oxide semiconductor film used in a thin film transistor, wherein: As metal elements, it contains: In and Zn; The element X is either La or Nd, The content of the In and Zn in all metal elements is, In: 30 atm% or more and 90 atm% or less, Zn: 9 atm% or more and 70 atm% or less, And has In oxide crystal phase, ZnIn oxide crystal phase and XIn oxide crystal phase, The composition of the ZnIn oxide crystal phase is Zn3In2O6 and / or Zn4In2O7.