Preparation method of multi-element co-doped nano-zinc oxide antibacterial sol

Through the preparation method of multi-combined nano zinc oxide antibacterial sol, the application of nano zinc oxide in the field of photocatalysis is solved, and efficient antibacterial and multiple properties are achieved. It is suitable for a variety of fields and has safety and long-term safety Effectiveness.

CN118901730APending Publication Date: 2024-11-08EAST CHINA JIAOTONG UNIVERSITY +1

Patent Information

Application Number
CN202410952828.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The application of existing antibacterial sols in the field of photocatalysis is limited by the short life of nano zinc oxide and the inability to absorb visible light, and traditional doping methods have safety hazards and insufficient performance.

Method used

The preparation method of multi-combined nano zinc oxide antibacterial sol is adopted. By heating and stirring zinc, copper, cerium, and silver compounds with deionized water, the complexing agent is slowly dripped, combined with surfactant and pH adjuster, water is carried out Thermal reaction is made to prepare a multivariate co-doped nano zinc oxide antibacterial sol with nano-scale particles.

Benefits of technology

Improve the photocatalytic effect of nano zinc oxide, enhance the antibacterial ability, has excellent sterilization, anti-mold, anti-viral, mite removal, formaldehyde removal, and odor removal. It is safe and non-toxic, suitable for daily chemicals, coatings and Industrial production has long-term antibacterial properties and broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118901730A_ABST
    Figure CN118901730A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of multi-element co-doped nano zinc oxide antibacterial sol, which mainly comprises the following steps: adding a zinc-containing compound, a copper-containing compound, a cerium-containing compound, a silver-containing compound and deionized water into a reaction kettle, heating and stirring, slowly dripping a complexing agent in the stirring process, and carrying out heat preservation hydrothermal reaction to obtain precursor sol; and controlling the obtained precursor sol at a certain temperature, then adding a proper amount of a surfactant and a pH regulator, and carrying out a heat preservation hydrothermal reaction to obtain the multi-element co-doped nano-zinc oxide antibacterial sol. The preparation method provided by the invention is simple in process, the reaction process is easy to control, and the prepared antibacterial sol can be directly used for indoor environment purification, can form an antibacterial film after being sprayed on the surface of an object, has efficient and lasting multiple effects of sterilization, mildew prevention, virus resistance, acarus killing, formaldehyde removal, odor removal and the like, and is suitable for popularization and application. The use requirements of various fields such as daily chemicals, coatings, industrial production and the like can be met, and wide application prospects are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to a method for preparing an antibacterial sol, and in particular relates to a method for preparing a multi-element co-doped nano zinc oxide antibacterial sol. Background Art

[0002] Microorganisms include bacteria, viruses, fungi and other tiny organisms that exist on various surfaces, in the air and in liquids. Some microorganisms can cause infectious diseases and pose a threat to human health. In addition, the growth of microorganisms in food processing and sanitary facilities may also lead to food contamination and disease outbreaks.

[0003] The development of antimicrobial sol technology aims to effectively control the spread and growth of microorganisms, thereby reducing the risk of infection and food contamination. These sols usually contain antimicrobial agents such as chlorides, peroxides, alcohols, phenols or other chemicals, which have bactericidal, disinfecting and antibacterial effects. Sols can be released in the form of aerosols, sprays or vapors, and spread to target surfaces through airborne particles or droplets.

[0004] Antimicrobial sol technology has a wide range of applications. In the medical field, antimicrobial sols can be used to disinfect operating rooms, wards and equipment surfaces to reduce the risk of hospital-acquired infections. In the food processing industry, sols can be applied to food handling equipment, packaging lines and storage areas to prevent microbial contamination and food spoilage. In addition, antimicrobial sols can also be used in public places such as schools, offices, transportation and commercial buildings to keep the environment sanitary and safe.

[0005] Nano zinc oxide is an n-type semiconductor with strong oxidation ability and ultraviolet photocatalytic ability, which makes it have certain antibacterial properties, but its short photogenerated carrier lifetime and inability to absorb and utilize visible light limit the wide application of nano zinc oxide in the field of photocatalysis. At present, the main methods to improve the photocatalytic performance of zinc oxide are doping modification and heterojunction modification.

[0006] A patent document with publication number CN109395710A and publication date March 1, 2019 discloses a method for preparing cerium-carbon co-doped zinc oxide, wherein a certain amount of imidazole substance is dissolved in a certain amount of deionized water; a mixed solution containing zinc and cerium is added to the aqueous solution of the imidazole substance, while stirring, and allowed to stand for a certain period of time to obtain a light yellow solid substance, and cerium ions are introduced in situ into the ZnO lattice to obtain a better doping effect. However, the ligand imidazole substance in this technical solution is irritating to the eyes and skin, and is a flammable liquid that will burn when exposed to open flames or high temperatures. The storage and reaction conditions are harsh, and the production has many inconveniences.

[0007] A patent document with publication number CN118000200A and publication date May 10, 2024 discloses a method for preparing a polysaccharide-based antibacterial liquid, which uses chitosan solution and polyvinyl alcohol solution as the matrix and adds antibacterial agents such as citral. However, the antibacterial activity of biological antibacterial agents is also affected by various factors such as temperature, polysaccharide concentration, and molecular weight. There are generally problems such as poor heat resistance, low bactericidal rate, and inability to be used for a broad spectrum and long period of time.

[0008] A patent document with publication number CN115724466A and publication date March 3, 2023 discloses a method for preparing a zinc oxide composite material, wherein zinc nitrate and bismuth nitrate are dissolved in water, stirred thoroughly and moved to a reactor for 22 hours at 140°C, washed and dried, and then calcined at 600°C to obtain bismuth-doped zinc oxide. After calcination, the material obtained by this method grows and crystallizes the zinc oxide particles, has a small specific surface area, and cannot be effectively utilized. The 24-hour formaldehyde degradation rate is as high as 98.76%. Summary of the invention

[0009] In view of the above-mentioned prior art, the present invention provides a method for preparing a multi-component co-doped nano zinc oxide antibacterial sol. The prepared antibacterial sol has excellent bactericidal, mildew-proof, antiviral, mite-removing, formaldehyde-removing and odor-removing effects, can meet the use requirements of various fields such as daily chemicals, coatings and industrial production, and has broad application prospects.

[0010] In order to solve the above technical problems, the present invention proposes a method for preparing a multi-element co-doped nano zinc oxide antibacterial sol, which mainly comprises: step 1, adding a zinc-containing compound, a copper-containing compound, a cerium-containing compound, a silver-containing compound and deionized water into a reaction kettle, heating and stirring, slowly dripping a complexing agent during the stirring process, and obtaining a precursor sol after a heat preservation hydrothermal reaction; step 2, controlling the precursor sol obtained in step 1 at a certain temperature, then adding an appropriate amount of a surfactant and a pH regulator, and obtaining a multi-element co-doped nano zinc oxide antibacterial sol after a heat preservation hydrothermal reaction.

[0011] Furthermore, the preparation method of the present invention, wherein:

[0012] In the reaction system of step 1, the molar concentration of the zinc-containing compound is 0.3 mol / L, the molar ratio of the copper-containing compound to the zinc-containing compound is 1%-5%, the molar ratio of the cerium-containing compound to the zinc-containing compound is 1%-5%, and the molar ratio of the silver-containing compound to the zinc-containing compound is 0.1%-0.3%.

[0013] In step 1, the zinc-containing compound is a water-soluble zinc salt, and one or more of zinc acetate, zinc nitrate, and zinc sulfate are selected; the copper-containing compound is a water-soluble copper salt, and one or more of copper sulfate, copper nitrate, and copper acetate are selected; the cerium-containing compound is a water-soluble cerium salt, and one or both of cerium nitrate and cerium sulfate are selected; the silver-containing compound is a water-soluble silver salt, and one or both of silver nitrate and silver acetate are selected.

[0014] In step 1, the complexing agent is ammonia water, and the speed of slowly dripping the complexing agent is 1 to 5 mL / min.

[0015] In step 1, the temperature of heating and stirring is 70-90° C., the temperature of the hydrothermal reaction is the same as the temperature of heating and stirring, and the time of the hydrothermal reaction is 100-150 min; the pH value of the precursor sol is 8-9.

[0016] In step 2, the surfactant is selected from one or more of polyvinyl pyrrolidone (PVP), sodium dodecyl sulfate (SDS), polyethylene glycol (PEG) and cetyltrimethylammonium bromide (CTAB); the pH adjuster is one or more of citric acid, acetic acid, hydrochloric acid and sulfuric acid.

[0017] In step 2, the mass volume ratio of the surfactant to the precursor sol is 5-10 g / L; the amount of the pH adjuster added is measured so that the pH of the reaction system reaches 6.5-7.5.

[0018] In step 2, the temperature of the precursor sol is 40° C. to 60° C., the temperature of the hydrothermal reaction is the same as the temperature of the precursor sol, and the time of the hydrothermal reaction is 30-60 min.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The use of copper, cerium, silver and other metal elements and zinc doping, through their synergistic effect, reduces the optical band gap of nano zinc oxide, enhances the photocatalytic effect of nano zinc oxide, and improves its antibacterial ability; at the same time, the prepared sol has excellent bactericidal, mildew-proof, antiviral, mite-removing, formaldehyde-removing, odor-removing and other properties, which can meet the disinfection needs of daily life scenes and industrial production, and can also be used as an air freshener in enclosed spaces such as cars and indoors.

[0021] (2) In the preparation method of the present invention, ammonia is preferably used as a complexing agent to form a stable silver-ammine complex through the complexation of ammonia and silver ions, so that the prepared sol has a more durable and stable antibacterial property than the silver solution, that is, it has a long-lasting antibacterial property.

[0022] (3) Nanoparticles are microscopic particles with at least one dimension less than 100 nanometers. Nano-sized materials have more excellent properties than conventional materials, such as surface effects, small size effects, quantum tunneling effects, etc., and also give materials physical properties such as light, heat, electricity, and magnetism. Nanotechnology has shown good application prospects in industrial fields such as daily cosmetics, food, industrial catalysis, and antibacterial. The outstanding feature of the multi-element co-doped nano-scale zinc oxide antibacterial sol prepared by the present invention is that the product particles are nano-scale and have the dual characteristics of nanomaterials and traditional zinc oxide. Compared with traditional zinc oxide products, it has a large specific surface area and high chemical activity. The product fineness, chemical purity and particle shape can be adjusted as needed, and it has photochemical effects and good ultraviolet shielding performance; at the same time, it also has a series of unique properties such as antibacterial, antibacterial, deodorizing and mildew-proofing.

[0023] (4) The multi-element co-doped nano zinc oxide antibacterial sol prepared by the present invention is safe and non-toxic, and is expected to be used for the preservation of vegetables and fruits, the antiseptic properties of various daily necessities, and the prevention and treatment of plant pathogens.

[0024] (5) The multi-element co-doped nano zinc oxide antibacterial sol prepared by the present invention has a transparent texture and can be used in scenarios where the antibacterial liquid has a transmittance requirement, such as being suitable for decoration after molding and mildew and antibacterial properties of glass.

[0025] (6) The preparation method of the present invention has a simple process and abundant raw material sources, and has excellent application prospects in various fields such as daily chemicals, coatings and industrial production.

[0026] (7) The present invention is easy to use and can be added to a base material such as a coating and stirred evenly to produce the product according to the original production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a flow chart of the preparation method of the multifunctional inorganic antibacterial liquid.

[0028] Figure 2 This is the SEM image of Example 1 at a scale of 200 nm. The nanoparticles are in the form of flakes with a thickness of 20 nm and a length of 200 nm.

[0029] Figure 3 This is the SEM image of Example 1 at a scale of 500 nm, showing a uniform flake shape with no obvious difference between the flake layers.

[0030] Figure 4 This is the SEM image of Example 1 at a scale of 1 μm, showing overlapping petal-like flakes. DETAILED DESCRIPTION

[0031] The invention proposes a multi-element co-doped nano zinc oxide antibacterial sol design idea, using copper, cerium, silver and other elements and zinc doping, to prepare a multi-element co-doped nano zinc oxide antibacterial sol, the preparation process is simple, such as Figure 1 As shown, the preparation method mainly includes: adding an appropriate amount of zinc salt, copper salt, cerium salt, and silver salt to deionized water, heating and stirring, slowly dripping a precipitant, and obtaining a precursor sol after heat preservation reaction; cooling the precursor sol to a certain temperature and then keeping it warm, stirring and dripping an appropriate amount of surfactant to improve its dispersibility and polybasic organic acid to adjust the pH, and obtaining a polybasic co-doped nano zinc oxide antibacterial sol. The preparation method provided by the present invention is not only simple in process, but also easy to control the reaction process. The obtained antibacterial sol can be directly used for indoor environmental purification, and can form an antibacterial film when sprayed on the surface of an object, and has excellent sterilization, mildew prevention, antiviral, mite removal, formaldehyde removal, and odor removal effects, and has good safety, heat resistance, durability, and high catalytic degradation efficiency under visible light. It can meet the use requirements of various fields such as daily chemicals, coatings, and industrial production, and has broad application prospects.

[0032] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but the following embodiments are by no means intended to limit the present invention in any way.

[0033] Example 1

[0034] A method for preparing a multi-element co-doped nano zinc oxide antibacterial sol comprises the following steps:

[0035] 1) Add 50g zinc sulfate (0.3mol), 0.57g copper sulfate (0.003mol), 1.7g cerium sulfate (0.003mol), 0.05g (0.0003mol) silver acetate and 1L deionized water into a reactor, heat to 70°C and stir to fully dissolve the solutes therein; at the same time, add ammonia water at a rate of 1mL / min to make the solution pH 8, and then hydrothermally react at 70°C for 150min to obtain a multi-element co-doped nano zinc oxide antibacterial precursor sol;

[0036] 2) The precursor sol obtained above was cooled to 40° C. and began to stir. During the stirring process, 5 g of CTAB was added and an appropriate amount of citric acid solution was added dropwise to adjust the pH value of the reaction system to 7.5. The reaction was then kept warm for 60 minutes. After the reaction was completed, a multi-element co-doped nano zinc oxide antibacterial sol was obtained, which was recorded as sample 1.

[0037] Figure 2 , Figure 3 and Figure 4The SEM images of the sample 1 prepared in Example 1 under different scales are shown respectively. It can be concluded that the nanoparticles in the sample 1 are in the form of flakes, with a thickness of 20nm and a length of 200nm. There is no significant difference between the layers, and the flakes are in the form of overlapping petals. The flower-like structure assembled by this flake structure can make the structure more stable. At the same time, the flake structure has a larger surface area exposure, more active sites, and can produce more active oxygen, which can effectively improve the degradation effect of formaldehyde. And the increase in active oxygen can effectively destroy bacterial DNA and protein, greatly improving the efficiency of antibacterial, anti-mildew and mite removal.

[0038] Example 2

[0039] A method for preparing a multi-element co-doped nano zinc oxide antibacterial sol comprises the following steps:

[0040] 1) Add 55 g zinc acetate (0.3 mol), 1.90 g copper acetate (0.01 mol), 3.30 g cerium nitrate (0.01 mol), 0.1 g (0.0006 mol) silver acetate and 1 L deionized water into a reactor, heat to 80 ° C and stir, and add ammonia water at a rate of 3 mL / min to make the solution pH 8.5, and then hydrothermally react at 80 ° C for 125 min to obtain a multi-co-doped nano zinc oxide antibacterial precursor sol;

[0041] 2) The precursor sol obtained above was cooled to 50° C. and began to stir. During the stirring process, 7.5 g of SDS was added and an appropriate amount of acetic acid solution was added dropwise to adjust the pH value of the reaction system to 7. The reaction was then kept warm for 45 minutes. After the reaction was completed, a multi-element co-doped nano zinc oxide antibacterial sol was obtained, which was recorded as sample 2.

[0042] Example 3

[0043] A method for preparing a multi-element co-doped nano zinc oxide antibacterial sol comprises the following steps:

[0044] 1) Add 60g zinc nitrate (0.3mol), 2.84g (0.015mol) copper nitrate, 4.89g cerium nitrate (0.015mol), 0.15g silver nitrate (0.0009mol) and 1L deionized water into a reactor, heat to 90°C and stir, and add ammonia water at a rate of 5mL / Min to make the solution pH 9, and then hydrothermally react at 90°C for 100min to obtain a multi-element co-doped nano zinc oxide antibacterial precursor sol;

[0045] 2) The precursor sol obtained above was cooled to 60°C and started to stir. During the stirring process, 10 g of PVP was added and an appropriate amount of hydrochloric acid solution was added dropwise to adjust the pH value of the reaction system to 6.5. The reaction was then kept warm for 30 minutes. After the reaction was completed, a multi-element co-doped nano zinc oxide antibacterial sol was obtained, which was recorded as sample 3.

[0046] Comparative Example 1

[0047] A method for preparing a multi-element co-doped nano zinc oxide antibacterial sol is disclosed. Compared with Example 1, the only difference is that copper sulfate is not added in step 1). The multi-element co-doped nano zinc oxide antibacterial sol finally prepared is recorded as comparative sample 1.

[0048] Comparative Example 2

[0049] A method for preparing a multi-component co-doped nano zinc oxide antibacterial sol is disclosed. Compared with Example 1, the only difference is that no cerium sulfate is added in step 1). The multi-component co-doped nano zinc oxide antibacterial sol finally prepared is recorded as Comparative Sample 2.

[0050] Comparative Example 3

[0051] A method for preparing a multi-element co-doped nano zinc oxide antibacterial sol is disclosed. Compared with Example 1, the only difference is that silver acetate is not added in step 1). The multi-element co-doped nano zinc oxide antibacterial sol finally prepared is recorded as comparative sample 3.

[0052] Comparative Example 4

[0053] A method for preparing a multi-element co-doped nano zinc oxide antibacterial sol is disclosed. Compared with Example 1, the only difference is that the surfactant CTAB is not added in step 2). The multi-element co-doped nano zinc oxide antibacterial sol finally prepared is recorded as comparative sample 4.

[0054] The test cases include the testing of antibacterial performance, anti-mildew performance, anti-mite performance and formaldehyde removal performance.

[0055] 1. Antibacterial performance test

[0056] The antibacterial sol samples used in the test experiments include samples 1, 2, and 3 prepared in Examples 1-3, comparative samples 1, 2, 3, and 4 prepared in Comparative Examples 1-4, and similar products available on the market (specifically, the sample used is Wesley disinfectant spray).

[0057] The antibacterial performance test experiment of the above antibacterial sol samples was carried out with reference to GB-T 21510-2008 "Test Method for Antibacterial Performance of Nano-inorganic Materials". The test process is: take an antibacterial sol sample as an example, and sterilize it with the ultraviolet sterilization lamp in the clean bench for 40 minutes. Dilute the bacterial solution cultured for 8 hours by 3 orders of magnitude, add 100μL of the antibacterial sol sample after disinfection, and place it in a shaker at a temperature of 37°C and a speed of 100rpm for 4 hours. Take 50μL of the shaken bacterial solution, inoculate it on the culture dish, and place it in a constant temperature and humidity incubator at a temperature of 37°C and a relative humidity of 90% for 24 hours to count the live bacteria. The results are shown in Table 1.

[0058] Table 1

[0059] Antibacterial sol samples Escherichia coli antibacterial rate (%) Antibacterial rate of Staphylococcus aureus (%) Sample 1 100.00 100.00 Sample 2 100.00 100.00 Sample 3 100.00 100.00 Comparison sample 1 99.21 99.89 Comparison sample 2 99.54 99.81 Comparison sample 3 96.74 98.10 Comparison sample 4 99.78 99.77 Wesley Disinfectant Spray 90.15 91.21

[0060] It can be seen from Table 1 that the multi-element co-doped nano zinc oxide antibacterial sol (sample 1, sample 2 and sample 3) of the present invention has excellent antibacterial properties, and the sterilization rates against Escherichia coli and Staphylococcus aureus can reach 100%.

[0061] 2. Anti-mildew performance test

[0062] The antibacterial sol samples used in the test experiments include samples 1, 2, and 3 prepared in Examples 1-3 and comparative samples 1, 2, 3, and 4 prepared in Comparative Examples 1-4.

[0063] The antibacterial performance test experiment of the above antibacterial sol sample was carried out with reference to GB / T 21866-2008 "Determination of antibacterial properties and antibacterial effects of antibacterial coatings (paint films)". The test process is: taking an antibacterial sol sample as an example, weigh 10g of the antibacterial sol sample and 990g of white paint, and disinfect them with an ultraviolet sterilization lamp in a clean bench for 40min. Mix the antibacterial sol sample with 990g of white paint and stir them thoroughly to obtain a paint with an antibacterial sol sample content of 1%, and evenly brush it on a 10*10cm PVC sheet. Place the PVC sheet in a cool and ventilated place for 48 hours. After the paint on the surface of the PVC sheet is completely solidified, place the PVC sheet in an environment with a temperature of 37°C and a relative humidity of 90% for 60d, and observe the growth of mold on the surface. The antibacterial test results are shown in Table 2.

[0064] Table 2

[0065] Antibacterial sol samples Mildew resistance level Sample 1 Level 0 Sample 2 Level 0 Sample 3 Level 0 Comparison sample 1 Level 1 Comparison sample 2 Level 1 Comparison sample 3 Level 0 Comparison sample 4 Level 1

[0066] It can be seen from Table 2 that the multi-element co-doped nano zinc oxide antibacterial sol (sample 1, sample 2 and sample 3) of the present invention has excellent anti-mildew performance.

[0067] 3. Mite killing performance test experiment

[0068] The antibacterial sol samples used in the test experiments include samples 1, 2, and 3 prepared in Examples 1-3 and comparative samples 1, 2, 3, and 4 prepared in Comparative Examples 1-4.

[0069] Refer to T / CIAA 017-2022 "Test Method for Anti-mite and Mite Removal Performance of Household Cleaning Products" to conduct a mite removal performance test experiment on the antibacterial sol sample. The test process is: taking an antibacterial sol sample as an example, draw 5mL of the antibacterial sol sample and drip it into the culture dish, evenly apply the white oil vaseline mixture on the upper edge of the inner wall of the culture dish, and then fix the culture dish on the sticky board. Put the culture dish and the sticky board together in a container covered with a sponge, and inject an appropriate amount of saturated salt water (the height of the water just submerges the sponge). Put 200 test insects in the center of the culture dish, and put 0.05g of mite feed in the center of the culture dish after 30 minutes. Place the container in a constant temperature and humidity incubator at a temperature of 25±2℃ and a humidity of 70±5% for 48 hours, and observe and record the data with a stereo microscope. The results of the mite removal experiment are shown in Table 3.

[0070] Table 3

[0071]

[0072]

[0073] 4. Formaldehyde removal performance test experiment

[0074] The antibacterial sol samples used in the test experiments include samples 1, 2, and 3 prepared in Examples 1-3 and comparative samples 1, 2, 3, and 4 prepared in Comparative Examples 1-4.

[0075] The formaldehyde removal performance of the above antibacterial sol samples was tested with reference to JC / T 1074-2008 "Purification Performance of Indoor Air Purification Functional Coating Materials". The testing process is: taking an antibacterial sol sample as an example, 1L of the antibacterial sol sample is added to a photocatalytic device (volume is 1L, light source is 40W fluorescent lamp) to degrade formaldehyde to evaluate the photocatalytic activity of the sample, and formaldehyde gas (initial mass concentration is controlled at 0.1mg / L) is used as a simulated pollutant. After 100 minutes of reaction, the formaldehyde concentration after the reaction is detected at a wavelength of 450nm to evaluate the photocatalytic activity of the sample under visible light irradiation. The results are shown in Table 4.

[0076] Table 4

[0077] Antibacterial sol samples Formaldehyde degradation rate (%) Sample 1 99.81 Sample 2 99.62 Sample 3 99.33 Comparison sample 1 92.71 Comparison sample 2 94.46 Comparison sample 3 96.72 Comparison sample 4 96.29

[0078] In summary, the multi-element co-doped nano zinc oxide antibacterial sol prepared by the present invention has good antibacterial properties, and the multi-element doping and nano-scale lamellar flower-like structure make its antibacterial properties better than traditional zinc oxide and unit doping and binary doping zinc oxide, and is suitable as an antibacterial material. The introduction of surfactants greatly improves its dispersibility, so that the present invention can be stably present in the form of sol, and the sol is released in the form of aerosol, spray or steam to achieve a rapid sterilization effect.

[0079] Although the present invention has been described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can make many improvements and changes without departing from the purpose of the present invention, which are all within the protection of the present invention.

Claims

1. A method for preparing a multi-element co-doped nano zinc oxide antibacterial sol, characterized in that: The following steps are involved: Step 1, adding a zinc-containing compound, a copper-containing compound, a cerium-containing compound, a silver-containing compound and deionized water into a reaction kettle, heating and stirring, slowly dripping a complexing agent during the stirring process, and performing a hydrothermal reaction at a temperature of 100° to obtain a precursor sol; Step 2: Control the precursor sol obtained in step 1 at a certain temperature, then add an appropriate amount of surfactant and pH regulator, and perform a hydrothermal reaction at a temperature to obtain a multi-element co-doped nano zinc oxide antibacterial sol.

2. The preparation method according to claim 1, characterized in that: In the reaction system of step 1, the molar concentration of the zinc-containing compound is 0.3 mol / L, the molar ratio of the copper-containing compound to the zinc-containing compound is 1%-5%, the molar ratio of the cerium-containing compound to the zinc-containing compound is 1%-5%, and the molar ratio of the silver-containing compound to the zinc-containing compound is 0.1%-0.3%.

3. The preparation method according to claim 1 or 2, characterized in that: In step 1, the zinc-containing compound is a water-soluble zinc salt, and one or more of zinc acetate, zinc nitrate, and zinc sulfate are selected; the copper-containing compound is a water-soluble copper salt, and one or more of copper sulfate, copper nitrate, and copper acetate are selected; the cerium-containing compound is a water-soluble cerium salt, and one or both of cerium nitrate and cerium sulfate are selected; the silver-containing compound is a water-soluble silver salt, and one or both of silver nitrate and silver acetate are selected.

4. The preparation method according to claim 1, characterized in that: In step 1, the complexing agent is ammonia water, and the speed of slowly dripping the complexing agent is 1 to 5 mL / min.

5. The preparation method according to claim 1, characterized in that: In step 1, the temperature of heating and stirring is 70-90° C., the temperature of the hydrothermal reaction is the same as the temperature of heating and stirring, and the time of the hydrothermal reaction is 100-150 min; the pH value of the precursor sol is 8-9.

6. The preparation method according to claim 1, characterized in that: In step 2, the surfactant is selected from one or more of polyvinyl pyrrolidone, sodium lauryl sulfate, polyethylene glycol and hexadecyltrimethylammonium bromide; the pH adjuster is one or more of citric acid, acetic acid, hydrochloric acid and sulfuric acid.

7. The preparation method according to claim 1, characterized in that: In step 2, the mass volume ratio of the surfactant to the precursor sol is 5-10 g / L; the amount of the pH adjuster added is measured so that the pH of the reaction system reaches 6.5-7.

5.

8. The preparation method according to claim 1, characterized in that: In step 2, the temperature of the precursor sol is 40° C. to 60° C., the temperature of the hydrothermal reaction is the same as the temperature of the precursor sol, and the time of the hydrothermal reaction is 30-60 min.

Citation Information

Patent Citations

  • Preparation method of cerium and carbon co-doped zinc oxide

    CN109395710A

  • Zinc oxide composite material and preparation method and application thereof

    CN115724466A

  • Polysaccharide-based antibacterial liquid as well as preparation method and application thereof

    CN118000200A

Cited By

  • Preparation method of photocatalyst synergistic slow-release type deodorizing gel

    CN120285254A

  • Preparation method of photocatalyst synergistic slow-release deodorant gel

    CN120285254B

  • Antiviral coating capable of continuously releasing negative ions and preparation method thereof

    CN121555013A