Method for preparing topography for improving blood coagulation and / or cell attachment on object made of titanium or titanium alloy

The dual etching method forms a specific morphology on the dental implant, which solves the problem of dental implants causing inflammation and rejection in the human body, achieves rapid blood coagulation and cell attachment, promotes bone integration and tissue interaction, and simplifies Packaging and storage of implants.

CN118903538APending Publication Date: 2024-11-08STRAUMANN HOLDING AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958395.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2015-05-26
Filing Date
2016-05-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing dental implants are prone to inducing inflammation and rejection in the human body, leading to pain and replacement surgery, and it is difficult to achieve rapid and strong tissue interactions, affecting bone integration and soft tissue interactions.

Method used

Using the dual etching method, the surface of the object is first etched with a first etching solution containing inorganic acid, and then further etched with a second etching solution containing hydrofluoric acid to form specific microscopic and submicroscopic morphology, which improves blood coagulation and cell attachment. Selective.

Benefits of technology

Rapid blood clotting and cell attachment are achieved, bone integration and tissue interaction are promoted, and good bone integration properties can be obtained even under hydrophobic conditions, simplifying the packaging and storage of implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118903538A_ABST
    Figure CN118903538A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a topography for improving blood coagulation and / or cell attachment on an object made of titanium or a titanium alloy. The method comprises the following sequential steps: a) etching at least a portion of the surface of the object with a first etching solution comprising an inorganic acid, and b) etching the surface etched under a) with a second etching solution different from the first etching solution, the second etching solution comprising hydrofluoric acid.
Need to check novelty before this filing date? Find Prior Art

Description

This application is a divisional application of Chinese patent application 201680043760.8, filed on May 26, 2016, “Method for preparing a morphology for improving blood coagulation and / or cell attachment on an object made of titanium or titanium alloy”. Technical Field The present invention relates to a method for preparing a topography for improving blood coagulation and / or cell attachment on an object made of titanium or a titanium alloy, to the object obtained by this method, and to the use of the object for a dental implant or a dental implant abutment. Background Art Implants such as dental implants are well known in the art. They are usually made of materials that are biocompatible and additionally have favorable mechanical properties. Currently used dental implants are usually made of titanium or titanium alloys, which, in addition to biocompatibility, also exhibit excellent mechanical strength.

[0003] The body's acceptance of implants is determined by the implant surface. When detected as a foreign body and rejected by the immune system, implants can cause inflammation, which not only causes pain to the patient but also often necessitates a secondary surgery to remove or replace the implant.

[0004] In order to avoid rejection of the implant by the body, the implant surface must be designed in such a way that cells attach to it and natural body tissue, in particular bone tissue or soft tissue, starts to grow around the implant.

[0005] In the case of dental implants, for example, a direct structural and functional connection between the living jawbone and the implant surface needs to be achieved shortly after implantation. This is known in the art as "osteointegration" (or "osseointegration"): good osseointegration means that the implant ossifies safely within a short healing time, thereby obtaining a permanent connection between the implant and the bone.

[0006] In addition to the importance of osseointegrative properties, there is increasing evidence that a good interaction between dental implants and the surrounding supracrestal connective tissue (hereinafter referred to as "soft tissue") is also crucial for successful implantation. This is supported by the view that soft tissue plays a fundamental role in establishing an effective seal between the oral environment and the intraosseous portion of the dental implant and is therefore also a barrier for bacterial adhesion on the soft tissue contacting surfaces and bone tissue contacting surfaces of the implant.

[0007] Once the implant is in contact with blood, the attachment of cells of the surrounding soft or bone tissue is controlled by proteins attached (ie, adsorbed) to the surface. Proteins adsorbed to the implant surface are believed to influence the behavior (eg, differentiation) of the corresponding tissue cells.

[0008] In order to achieve a fast and strong interaction between dental implants and the corresponding tissue, the adhesion of these proteins to the surface is therefore crucial.

[0009] An important factor affecting protein adhesion is surface hydrophilicity.

[0010] Recently, it has been discovered that the presence of specific nanostructures may play an important role in the adhesion of proteins.

[0011] Specifically, WO 2013 / 056844 describes a method for providing a structure for improving the adhesion of proteins on the surface of an object, in particular an implant. The method comprises the step of storing an acid-etched alkaline object in an aqueous solution, thereby forming a nanostructure on the surface of the alkaline object. According to WO 2013 / 056844, the formation of the nanostructure thus occurs gradually, resulting in "growth" or "accumulation" over time.

[0012] Furthermore, RA Gittens et al. (Biomaterials 32 (2011) 3395-3403) reported a study focusing on graded combinations of both micro- and nano-roughness to promote bone integration on clinically relevant surfaces.

[0013] Although the method according to WO 2013 / 056844 achieves good results, there is still a need to provide an object which establishes a rapid and intensive interaction with the surrounding tissue after implantation. Summary of the invention Taking this into account, an object to be solved by the present invention is to provide a method for preparing topography on an object made of titanium or a titanium alloy in a way that allows improved interaction with surrounding tissue. In particular, a simple and reproducible method for modifying the surface of an object should be provided that allows relatively selective adhesion of at least one blood protein that mediates blood coagulation and / or cell attachment, thereby allowing interaction of tissue with the object.

[0015] The object of the invention is solved by a method according to claim 1. Preferred embodiments of the invention are defined in the dependent claims.

[0016] According to claim 1, the method of the present invention relates to a method for preparing a topography for improving blood coagulation and / or cell attachment on an object made of titanium or titanium alloys, ie the most common material for dental implants or dental implant abutments.

[0017] The method comprises the following steps in sequence: a) etching at least a portion of the surface with a first etching solution comprising an inorganic acid, and b) etching the surface etched under a) with a second etching solution different from the first etching solution, the second etching solution comprising hydrofluoric acid (HF).

[0018] It has been surprisingly found that, by combined etching according to the present invention, a surface that allows rapid blood coagulation and thus forms a fibrin network and / or a firm attachment of surrounding tissue cells is achieved. In particular, improved osseointegration of an object is achieved, which will be shown in detail by the specific working examples described below.

[0019] It has further been found that even in the case of relatively hydrophobic surfaces, improved tissue interaction, in particular osseointegration, can be achieved. This finding is most surprising in view of the established principle that a hydrophilic surface is an important requirement for achieving good osseointegration.

[0020] Without wishing to be bound by theory, it is believed that the improved blood coagulation and / or cell attachment is due to the specific morphology of the objects obtained by the method of the invention according to the following mechanism: When an object is implanted in tissue, especially bone tissue, it first comes into contact with water molecules from the surrounding blood. Next, ions and proteins will accumulate and adhere to the surface of the implant without actually penetrating the material. As mentioned above, this "protein adhesion" or "protein adsorption" is considered to be decisive for the subsequent cellular response.

[0021] By means of the specific topography obtainable by the present invention, a "protein retention structure" is provided on the surface of the object, ie a structure which allows an improved adhesion of specific proteins.

[0022] As shown by the attached working examples, the morphology obtained allows relatively selective adhesion of fibrinogen, which plays an important role in blood coagulation and thus in the formation of a fibrin network. In this context, the working examples also show that, compared with the comparative examples, a relatively thick fibrin network is formed on the object according to the present invention.

[0023] The term "etching" as used in the context of the present invention is to be understood broadly and includes the formation or modification of the topography of an object by dissolving and thus removing material from the surface of the object through an etching solution. Etching thus relates to a subtractive surface treatment, which is in contrast to any additive surface treatment, such as is the case with anodizing. According to a specific embodiment, the term "etching" does not relate to the pure removal of the native oxide layer of an object, since the removal of the native oxide is not accompanied by the formation or modification of the topography. Etching within the meaning of this embodiment is similarly in contrast to a "pickling" treatment used to remove surface impurities and intended to preferentially remove material uniformly.

[0024] Specifically, by etching the surface according to step a), a microscopic topographical formation is formed, and by etching the surface according to step b), a submicroscopic topographical formation is formed in the microscopic topographical formation. Thus, a topographical level different from that in step a) is formed in step b), resulting in a graded topography.

[0025] As will be discussed in further detail below, the subtractive processing step a) preferably corresponds to the well-known In particular, step a) therefore involves a pretreatment prior to etching, comprising a mechanical subtractive treatment, more particularly a sandblasting treatment.

[0026] Like step a), step b) is also a subtractive processing step, meaning that by this step, material is removed from the object. Therefore, the term "forming a submicroscopic topography in a microscopic topography" should be understood as "forming by further removing material from the intermediate object having a microscopic topography obtained after step a)".

[0027] The submicroscopic topographic structure obtained by the method of the invention is therefore made of material originally contained in the object and remaining on the surface of the object after step a) and step b). The way in which the submicroscopic topographic structure is formed is therefore different in all respects from the construction of nanostructures described in WO 2013 / 056844, which involves the growth or accumulation of structures over time and thus involves an additive process.

[0028] Since process step b) is subtractive, the material composition of the submicroscopic topography corresponds substantially to the material composition of the surface of the object before processing and to the material composition of the microscopic topography present after process step a). Since the object is made of titanium or a titanium alloy having a surface on which a corresponding oxide layer is formed spontaneously, the microscopic topography with the submicroscopic topography formed thereon is likewise made of titanium or a titanium alloy, respectively, on which an oxide layer is formed.

[0029] Since both step a) and step b) are etching steps, the method of the invention can be considered as a "double etching" method. It is therefore different in any respect from a method comprising only one single etching step, i.e. one single subtractive surface treatment step. In particular, it is clearly contrasted with a two-step process in which a single etching step is followed by an additive surface treatment step, such as an anodizing step, for chemically modifying the surface and / or for structuring its topography.

[0030] According to a preferred embodiment of the present invention, the microscopic topography is defined by at least one of the following surface parameters: i)S a is the arithmetic mean deviation of the surface in three dimensions and is in the range of 0.1 μm to 2.0 μm, preferably in the range of 0.4 μm to 1.8 μm, more preferably in the range of 0.8 μm to 1.7 μm, and most preferably 0.9 μm to 1.5 μm; ii) S t is the maximum peak-to-valley height of the profile in three dimensions and is in the range of 1.0 μm to 20.0 μm, preferably in the range of 3.0 μm to 18.0 μm, more preferably 4.5 μm to 13.0 μm, and most preferably 6.0 μm to 12.0 μm; and / or iii) S sk It is the skewness of the profile in three dimensions, and is in the range of -0.6 to 1.0, preferably -0.4 to 0.6, more preferably -0.3 to 0.5.

[0031] The surface parameters are known to a person skilled in the art and are respectively the parameters R defined in EN ISO 4287 for two dimensions. a , R t and R sk The above values ​​relate to similar parameters for three dimensions. Specifically, the above values ​​relate to, for example, those obtainable by WinSAM software (SAM (Surface Analysis Method) for Windows) known to those skilled in the art.

[0032] S a , S t and S sk The above values ​​of relate in particular to the bone contact surface of the object, i.e. the surface area on the object, in particular the implant, which comes into contact with the bone tissue after implantation. For the soft tissue contact surface of the object, the preferred value is smaller. Specifically, for the soft tissue contact surface, S a It is preferably in the range of 0.05 μm to 0.5 μm, more preferably 0.05 μm to 0.3 μm.

[0033] As mentioned above, the microstructure defined above is usually obtained by further comprising step a) of sandblasting prior to etching.

[0034] Regarding the microscopic morphology, if the etching according to a) in the above preferred embodiment is carried out according to or The surface parameters are preferably or within the range of the surface.

[0035] and The treatment of both is well known in the relevant fields and involves a breakthrough technology in the preparation of osteophilic implants. Involving sandblasting the implant surface, followed by treatment with an etching solution comprising a first inorganic acid, and Further comprising conditioning the "SLA" surface in nitrogen or in isotonic saline solution to maintain The high hydrophilicity of the surface would otherwise be lost during storage due to interaction with the atmosphere.

[0036] According to a preferred embodiment of the invention, the first etching solution thus comprises or consists essentially of a mixture of HCl and H2SO4. More particularly, a mixture of HCl and H2SO4 is used for step a) at a temperature above 80°C. Alternatively, any other solution of at least one inorganic acid can be used for process step a), in particular a solution comprising at least one inorganic acid selected from HCl, H2SO4, H3PO4 and mixtures thereof. If HF is contained in the first etching solution, the concentration of HF is lower than the HF concentration of the second etching solution. According to a particularly preferred embodiment, the first etching solution is at least substantially free of HF. In this regard, the present invention differs even more significantly from the technology described in EP 1 477 141, according to which HF is used in a first step to remove native oxides before etching the surface in a second step.

[0037] It is further preferred that, before step a), the surface is provided with a macroscopic topography (more preferably by sandblasting). For example, corundum with a particle size of 250-500 μm can be used as a sandblasting material. In this embodiment, The sandblasting step of the conventional technique is also applied to the method of the present invention.

[0038] According to a particularly preferred embodiment, the present invention therefore relates to The same steps as the solution, but The etching step further comprises a step b).

[0039] Preferably, the method is carried out in such a way that the microscopic morphology formed in step a) is defined by the submicroscopic morphology formed in step b) and is selected from S a , S t and S sk At least one surface parameter of the substrate changes by at most 50%, preferably by at most 20%, more preferably by at most 10%, and most preferably remains essentially unchanged.

[0040] Therefore, by process step b) according to The macroscopic and microscopic topography established by the art has not changed or has changed only to a negligible extent. This is further illustrated by the accompanying drawings, which show almost the same picture focusing on the macroscopic and microscopic topography of the surface at a certain magnification, but show a completely different picture of the surface focusing on the submicroscopic topography at a certain magnification.

[0041] In particular, the submicroscopic topography achievable by the present invention comprises or consists essentially of a submicroscopic structure extending up to 1000 nm in at least two dimensions. Preferably, the submicroscopic structure extends from 20 nm to 1000 nm in at least two dimensions, preferably from 30 nm to 500 nm, more preferably from 40 nm to 300 nm, even more preferably from 50 nm to 250 nm, and most preferably from 100 nm to 200 nm.

[0042] Depending on the specific material of the object and the process parameters, different submicrostructures can be obtained. In particular, the submicrostructure has a shape with at least one straight edge, and more particularly sharp-edged and / or jagged, which will also be illustrated by the accompanying drawings. Alternatively or additionally, the submicrostructures can be arranged in a stepped or cascaded manner relative to each other. More specifically, the submicrostructure can be in the form of sharp-edged cliffs or pillars with cracks formed between them.

[0043] Preferably, the concentration of hydrofluoric acid in the second etching solution is 0.01 vol% to 4 vol%, preferably 0.05 vol% to 2 vol%, more preferably 0.1 vol% to 1 vol%. Most preferably, the concentration of hydrofluoric acid in the second etching solution is in the range of 0.2 vol% to 0.5 vol%.

[0044] According to a further preferred embodiment, the etching under step b) is carried out for a duration ranging from 0.1 min to 30 min, preferably from 0.5 min to 20 min, more preferably from 0.5 min to 10 min, most preferably from 1 min to 5 min.

[0045] By keeping the hydrofluoric acid concentration and duration of the treatment according to step b) within the preferred ranges given above, the desired submicroscopic topography can be achieved while keeping the features of both the macroscopic and microscopic topography intact. In particular, the surface parameter S defining the microscopic topography a , S t and S sk At least one of remains substantially unchanged, which is preferred as described above.

[0046] The relatively short duration of etching further emphasizes the difference between the method of the present invention and the growth of nanostructures over a much longer period of time mentioned in WO 2013 / 056844.

[0047] It is further preferred that the etching in step b) is carried out at a temperature of 10°C to 90°C, preferably 10°C to 60°C, more preferably 15°C to 40°C, even more preferably 15°C to 30°C, most preferably room temperature (20°C).

[0048] According to a further preferred embodiment, the object is made of a titanium-zirconium alloy, since for this material a particularly relevant surface morphology can be achieved by the method according to the invention. More preferably, the object is made of a bimetallic titanium-zirconium alloy containing 13-17% zirconium. A particularly preferred titanium-zirconium alloy is available under the trade name (Institut Straumann AG, Switzerland), the properties of which are known to the person skilled in the art. Depending on the objectives to be achieved, the objects can also be made of titanium, since it has been found that for objects made of titanium, in particular titanium implants, morphologies for improving blood coagulation and / or cell adhesion can also be achieved by the method according to the invention.

[0049] As indicated above, the method of the invention relates in particular to dental implants or dental implant abutments in order to provide them with a surface that allows intensive interaction with surrounding tissue. According to a preferred embodiment, the object is a dental implant or a dental implant abutment and the topography is provided on at least a portion of the surface of the object that is intended to be in contact with bone tissue or soft tissue, respectively, when in use.

[0050] As also described above and as shown in more detail by the working examples, improved osseointegration can be achieved by the topography provided according to the invention even in case of a relatively hydrophobic surface. Thus, the surface also provides good osseointegration properties after the dental implant has been stored in air, so that there is no need to store the dental implant in a protective environment. Ultimately, this allows for a very simple packaging of the dental implant.

[0051] The terms "hydrophobic" or "hydrophobicity" are used in contrast to the terms "hydrophilic" or "hydrophilicity". The terms "hydrophilic" or "hydrophilicity" used in the context of the present invention refer to a surface having a contact angle of less than 90°, more preferably less than 30°, and most preferably less than 10° when in contact with water.

[0052] According to a specific embodiment of the invention, the surface of the object is hydrophobic. In the context of the present invention, the term "hydrophobic" or "hydrophobicity" specifically relates to a surface having a contact angle higher than 90° when in contact with water. As described, the specific morphology achievable by the present invention enables excellent osseointegration properties to be obtained even at relatively high contact angles. Thus, very simple implant packaging and storage devices can be selected, which still have excellent osseointegration properties even after long storage periods.

[0053] According to another specific embodiment, the surface of the object is hydrophilic, with a contact angle of less than 90°, more specifically superhydrophilic, with a contact angle of less than 30°, most particularly less than 10°, when in contact with water. The hydrophilicity or superhydrophilicity of the surface leads to immediate wetting of the implant by blood and thus to rapid contact of water molecules and ions contained therein, followed by accumulation and adhesion of blood coagulation and / or cell attachment mediating proteins to the surface. Thus, an even further improved interaction of the surface with the surrounding tissue can be obtained.

[0054] In addition to the above-described method, the present invention also relates to an object obtainable by said method.

[0055] In particular, the present invention relates to an object whose surface is defined by microscopic topography and by submicroscopic topography formed within the microscopic topography.

[0056] As mentioned above, the microscopic topography is defined by at least one of the following surface parameters: i)S a is the arithmetic mean deviation of the surface in three dimensions and is in the range of 0.1 μm to 2.0 μm, preferably in the range of 0.4 μm to 1.8 μm, more preferably 0.8 μm to 1.7 μm, and most preferably 0.9 μm to 1.5 μm; ii) S t is the maximum peak-to-valley height of the profile in three dimensions and is in the range of 1.0 μm to 20.0 μm, preferably in the range of 3.0 μm to 18.0 μm, more preferably 4.5 μm to 13.0 μm, and most preferably 6.0 μm to 12.0 μm; and / or iii) S sk It is the skewness of the profile in three dimensions, and is in the range of -0.6 to 1.0, preferably -0.4 to 0.6, more preferably -0.3 to 0.5.

[0057] Specifically, the above-mentioned values ​​relate to values ​​which can be obtained, for example, by WinSAM software (SAM (Surface Analysis Method) for Windows) known to a person skilled in the art as described above.

[0058] As also described, the submicroscopic topography comprises or consists essentially of a submicroscopic structure extending up to 1000 nm in at least two dimensions.

[0059] Furthermore and in accordance with the above method, at least some of the submicroscopic structures have a shape with at least one straight edge, and more particularly are sharp-edged and / or jagged.Alternatively or additionally, the submicroscopic structures may be arranged in a stepped or cascaded manner relative to each other.

[0060] It will be appreciated that all features described above as preferred features for the method of the invention are also preferred features for the object of the invention and vice versa.

[0061] According to a further aspect, the invention also relates to the use of an object according to any of the preceding claims for a dental implant or a dental implant abutment. In this regard, the object may be used as a dental implant or a dental implant abutment, or as a part of a dental implant or a dental implant abutment. It should be understood that when the object is used as a part of a dental implant or a dental implant abutment, at least a part of the remaining part may be made of a material other than titanium or a titanium alloy, respectively.

[0062] If the object is used as a dental implant abutment, S a , S t and S sk The values ​​of S are preferably lower than those mentioned above, especially in relation to the bone contacting surface of the object. Specifically, in the case where the object is a dental implant abutment, S a Preferably it is in the range of 0.05 μm to 0.5 μm, more preferably in the range of 0.05 μm to 0.3 μm. This allows to obtain a particularly strong interaction of the dental implant abutment and the surrounding soft tissue. DETAILED DESCRIPTION The present invention also relates to the following embodiments: 1. A method for preparing a topography for improving blood coagulation and / or cell attachment on an object made of titanium or a titanium alloy, The method comprises the following steps in sequence: a) etching at least a portion of the surface of the object with a first etching solution comprising an inorganic acid, and b) etching the surface etched under a) with a second etching solution different from the first etching solution, the second etching solution comprising hydrofluoric acid. 2. The method according to embodiment 1, wherein a microscopic topography is formed by etching the surface according to step a), and a submicroscopic topography is formed in the microscopic topography by etching the surface according to step b). 3. The method according to embodiment 2, wherein the microscopic topography is defined by at least one of the following surface parameters: i) S a is the arithmetic mean deviation of the surface in three dimensions and is in the range of 0.1 μm to 2.0 μm, preferably in the range of 0.4 μm to 1.8 μm, more preferably 0.8 μm to 1.7 μm, and most preferably 0.9 μm to 1.5 μm; ii) S t is the maximum peak-to-valley height of the profile in three dimensions and is in the range of 1.0 μm to 20.0 μm, preferably in the range of 3.0 μm to 18.0 μm, more preferably 4.5 μm to 13.0 μm, and most preferably 6.0 μm to 12.0 μm; and / or iii) S sk It is the skewness of the profile in three dimensions, and is in the range of -0.6 to 1.0, preferably -0.4 to 0.6, more preferably -0.3 to 0.5. 4. The method according to embodiments 2 and 3, wherein the microscopic morphology formed in step a) is defined by the submicroscopic morphology formed in step b) and is selected from S a , S t and S sk At least one surface parameter of the substrate changes by at most 50%, preferably by at most 20%, more preferably by at most 10%, and most preferably remains essentially unchanged. 5. The method according to any one of embodiments 2 to 4, wherein the submicroscopic topography comprises or consists essentially of a submicroscopic structure, wherein the submicroscopic structure extends up to 1000 nm in at least two dimensions. 6. The method according to any of the preceding embodiments, further comprising the step of providing the surface with a macroscopic topography, in particular by sandblasting, before step a). 7. The method according to any of the preceding embodiments, wherein the object is made of a titanium-zirconium alloy, preferably a bimetallic titanium-zirconium alloy comprising 13-17% zirconium. 8. The method according to any one of the preceding embodiments, wherein the concentration of hydrofluoric acid in the second etching solution is in the range of 0.01 vol% to 4 vol%, preferably 0.05 vol% to 2 vol%, more preferably 0.1 vol% to 1 vol%. 9. The method according to any of the preceding embodiments, wherein the treatment under step b) is carried out for a duration ranging from 0.1 minutes to 30 minutes, preferably from 0.5 minutes to 20 minutes, more preferably from 0.5 minutes to 10 minutes, most preferably from 1 minute to 5 minutes. 10. The method according to any of the preceding embodiments, wherein the treatment under step b) is carried out in a temperature range of 10°C to 90°C, preferably 10°C to 60°C, more preferably 15°C to 40°C, even more preferably 15°C to 30°C and most preferably at room temperature. 11. The method according to any of the preceding embodiments, wherein the first etching solution comprises or consists essentially of a mixture of HCl and H2SO4. 12. The method according to any of the preceding embodiments, wherein the object is a dental implant or a dental implant abutment and the topography is provided on at least a portion of a surface of the object intended to come into contact with bone tissue or soft tissue, respectively, in use. 13. An object obtained by a method according to any one of the preceding embodiments. 14. An object according to embodiment 13, whose surface is defined by microscopic topography and by submicroscopic topography formed in the microscopic topography. 15. The object according to embodiment 14, wherein the microtopography is defined by at least one of the following surface parameters: i)S a is the arithmetic mean deviation of the surface in three dimensions and is in the range of 0.1 μm to 2.0 μm, preferably in the range of 0.4 μm to 1.8 μm, more preferably 0.8 μm to 1.7 μm, and most preferably 0.9 μm to 1.5 μm; ii) S t is the maximum peak-to-valley height of the profile in three dimensions and is in the range of 1.0 μm to 20.0 μm, preferably in the range of 3.0 μm to 18.0 μm, more preferably 4.5 μm to 13.0 μm, and most preferably 6.0 μm to 12.0 μm; and / or iii) S sk It is the skewness of the profile in three dimensions, and is in the range of -0.6 to 1.0, preferably -0.4 to 0.6, more preferably -0.3 to 0.5. 16. An object according to embodiment 14 or 15, wherein the submicroscopic topography comprises or consists of a submicroscopic structure, wherein the submicroscopic structure extends up to 1000 nm in at least two dimensions. 17. An object according to embodiment 16, wherein at least some of said submicroscopic structures have a shape with at least one straight edge, and more particularly are sharp-edged and / or jagged. 18. Use of an article according to any of the preceding embodiments for a dental implant or a dental implant abutment. Example

[0063] 1. Examples related to in vitro analysis Materials and methods Materials Discs with a diameter of 5 mm and a thickness of 1 mm were prepared from bimetallic TiZr alloy rods (Roxolid (RXD); 13-17% Zr).

[0064] "SLA" processing First, according to the preparation Sample Protocol The samples were treated. Specifically, the samples were sandblasted using large grits (250-500 μm particle size) corundum, and then the sandblasted surface was etched in a boiling mixture of HCl and H2SO4.

[0065] Samples "RXD SLA HF" and "RXD SLActive HF" Then pass Treatment (related to step a) of the method of the invention) A first portion of the obtained sample was treated in an aqueous solution containing 0.2% hydrofluoric acid (for a volume of 100 ml: 0.5 ml 40% HF, 99.5 ml H2O) at room temperature for 2 minutes (corresponding to step b) of the method).

[0066] The sample was then rinsed in ultrapure water by placing the Teflon beaker containing the sample into 400 ml of ultrapure water and sonicating the sample three times (each time in about 20 ml of ultrapure water for 1 minute). The sample was then blown dry in an argon stream and stored dry in aluminum foil.

[0067] Thus, a sample "RXD SLA HF" according to the present invention was obtained.

[0068] Additionally, samples "RXD SLActive HF" were prepared, which will be discussed in the context of evaluating fibrin network construction. Specifically, these samples were prepared similarly to the "RXD SLA HF" described above, but differed in that instead of storing the dried samples in air, they were stored in a commercially available The implants were placed in a 0.9% NaCl solution (pH approximately 5) in a vial.

[0069] Sample "RXD SLActive" For comparison purposes, Program, through The second part of the sample obtained by the treatment was directly immersed in and stored in a 0.9% NaCl solution, thereby obtaining a comparative sample "RXD SLActive".

[0070] Storage and Sterilization All samples were stored for at least 2 months.

[0071] Both RXD SLA HF and RXD SLActive samples were gamma sterilized (25-42 kGy) before their surfaces were analyzed according to the evaluation methods described below. Comparative experiments performed on discs before and after sterilization did not indicate that gamma sterilization had an effect on the results obtained by the evaluation methods described below.

[0072] Evaluation Method Contact angle measurement Contact angle measurements were performed to determine the degree of hydrophilicity or hydrophobicity. For "RXD SLA HF" and "RXDSLActive", three sample discs were analyzed.

[0073] The contact angle was determined using a sessile drop test with ultrapure water (EasyDrop DSA20E, Krüss GmbH). A drop size of 0.3 μl (microliter) was chosen for the RXD SLA HF samples (i.e., samples stored dry) and 0.1 μl (microliter) for the RXD SLActive samples (i.e., samples stored in saline solution). Prior to the contact angle measurement, the RXD SLActive samples were blown dry in an argon stream. The RXD SLA HF samples were measured as received. The contact angle was calculated by fitting a circular segment function according to the droplet profile on the surface.

[0074] Table 1a gives the results of the contact angle measurements.

[0075] Table 1a: Contact angle (first set of results) As shown in Table 1a, all RXD SLA HF discs are hydrophobic, exhibiting a contact angle of about 135° when in contact with pure water, while the RXD SLActive discs are hydrophilic, exhibiting complete wetting by water.

[0076] In further experiments, the contact angle of the RXD SLActive HF sample was also evaluated, the results of which are shown in Table 1b.

[0077] Table 1b: Contact angle (second set of results) These results confirm the previous findings on the RXD SLA HF and RXD SLActive samples and further show complete wetting of the RXDSLActive HF sample, so that its surface can be considered superhydrophilic within the above definition, as is also the case with the surface of the RXD SLActive sample. Thus, the submicrostructures according to the invention do not have any negative impact on the hydrophilicity of the surface on which they are formed.

[0078] 1.2.2.SEM (Scanning Electron Microscope) Scanning electron microscopy (SEM) was used to evaluate the visual appearance and morphology of the nanostructures.

[0079] SEM measurements were performed on three disks for each type of surface. Measurements were performed using a Zeiss Supra 55 scanning electron microscope. Overview SEM images were acquired using an Everhart-Thornley detector at an accelerating voltage of 20 kV, and high-resolution images were acquired using an in-lense detector at an accelerating voltage of 5 kV.

[0080] The SEM images of the samples are given in the attached figure. Figure 1 SEM image of the surface of the sample RXD SLA HF at a magnification of about 1000 times, with a scale bar corresponding to 10 microns given in the lower left corner of the image; Figure 2 SEM image of the surface of the sample RXD SLActive HF at a magnification of about 1000 times, with a scale bar corresponding to 10 microns given in the lower left corner of the image; Figure 3 SEM image of the surface of the sample RXD SLActive at about 1000 times magnification, with a scale bar corresponding to 10 microns given in the lower left corner of the image; Figure 4 The SEM image of the surface of the sample RXD SLA HF is magnified about 20,000 times, and the scale bar corresponding to 200 nanometers is given in the lower left corner of the image; Figure 5 a SEM image of the surface of a sample RXD SLActive HF at a magnification of about 50,000 times, with a scale bar corresponding to 200 nanometers given in the lower left corner of the image; and Figure 6 SEM image of the surface of the sample RXD SLActive at a magnification of about 20,000 times, with a scale bar corresponding to 200 nanometers given in the lower left corner of the image.

[0081] from Figure 1-6 It can be seen that the samples show The macro- and micro-morphological structures obtained by treatment (i.e., by sandblasting and etching the samples in a boiling mixture of HCl and H2SO4).

[0082] However, there are clear differences in the appearance of the submicroscopic topographical structures. Specifically, the submicroscopic structures are formed by the subtractive process step b) (ie by etching using an etching solution comprising HF).

[0083] The submicroscopic structure has a shape with at least one straight edge, and more particularly a sharp edge or even a sawtooth shape, which can be specifically seen from Figure 4 Further experiments have shown that the submicroscopic morphology is maintained after storage of RXD SLA HF samples in NaCl or air.

[0084] In addition, if or Surface as a starting point, we obtain a similar structure, such as Figure 4 and Figure 5 Shown (photographed at different magnifications).

[0085] The submicroscopic structures formed by the method of the invention comprising the subtractive process step b) are completely different in both size and shape from the nanostructures on the RXD SLActive sample formed according to the technique described in WO 2013 / 056844 and thus formed by gradual "growth" or "accumulation" over time.

[0086] 1.2.3. Determination of roughness parameters Roughness images were obtained using a confocal microscope (μsurf explorer, NanoFocus AG, Oberhausen, Germany) equipped with a 20x lens. Three measurements were performed for each sample disc, and three discs were measured for each type of surface. Roughness parameters were calculated using the WinSAM software described above. The 3D roughness parameters were calculated using a complete roughness image with a size of 798 μm (micrometers) × 798 μm (micrometers).

[0087] The value of the microtopography (roughness) was determined using a moving average Gaussian filter with a cutoff wavelength of 30 μm (x=31 μm, y=30 μm, 20 x 19 pixels). The roughness value was then calculated by KFL analysis using limits from the amplitude density.

[0088] Specifically, S a (arithmetic mean deviation of the three-dimensional surface), S t (maximum peak-to-valley height of the profile in three dimensions) and S sk(skewness) is similar to the corresponding parameter R in two dimensions. a , R t and R sk For parameters in three dimensions, further reference is made to ISO 25178, where the symbol S z The maximum peak-to-valley height of the profile (instead of the symbol S used in the context of the present invention) t ).

[0089] Table 2a shows the average micro-roughness values ​​of the two samples. This table shows that both RXD SLActive and RXD SLAHF have at least S a and S t The value falls on The same range is usually observed for implants. Specifically, the S a and S t The values ​​deviate from the corresponding values ​​of the RXD SLActive sample by less than 15%.

[0090] Table 2a: Values ​​of microstructure (first set of results) In further experiments, the microstructures formed thereon of the RXD SLActive HF sample were also evaluated, and the results thereof (in addition to the results of RXD SLA HF and RXD SLActive) are also shown in Table 2b.

[0091] Table 2b. Values ​​of microstructure (second set of results) These results confirm previous findings on the RXD SLA HF and RXD SLActive samples and further indicate that the topographic parameters determined for the RXD SLActive HF sample deviate only slightly from those determined for the RXD SLActive. Specifically, the S a and S t The deviation of the values ​​is less than 15%.

[0092] 1.2.4. Protein adsorption measurements Albumin (from bovine serum (BSA), Alexa Fluor 647 conjugate, Invitrogen, USA), fibrinogen (from human plasma; HPF, Alexa Fluor 546 conjugate, Invitrogen, USA) and fibronectin (Rhodamine Fibronectin from bovine plasma; BSF, Cytoskeleton, Inc., USA) were used as model proteins to study their adsorption (or "adhesion") behavior on different surfaces by fluorescence microscopy using a fluorescence scanner.

[0093] Stock solutions of 0.5 mg / ml albumin and 0.5 mg / ml fibrinogen were prepared according to the product manual. For storage, these stock solutions were divided into 0.5 ml aliquots and frozen at -20°C. Fibronectin solution was prepared directly from the 20 μg vial without preparing a stock solution.

[0094] All protein adsorption solutions were prepared with HEPES2 buffer, which was prepared with 10 mM 4-(2-hydroxyethyl)-piperazine-1-ethanesulfonic acid (HEPES) and 150 mM NaCl, pH 7.4. Prior to use, the HEPES2 buffer was filtered (Whatman FP 30 / 0.2CA-S, size 0.2 μm, maximum pressure 7 bar).

[0095] For low protein concentration experiments, protein solutions consisted of filtered HEPES2 and fluorescently labeled proteins of defined concentrations (see Table 3 below). For high concentration experiments, unlabeled proteins were additionally added to simulate the true protein concentration in human blood (Table 3). In order to improve the solubility of unlabeled proteins, HEPES2 was heated to 37°C (water bath, INCO 2 / 108, Memmert GmbH & Co, Germany) before preparing the solution. Different proteins were tested respectively; therefore, the protein solutions prepared always only included one type of protein. It was believed that the labeled proteins performed identically to the unlabeled proteins.

[0096] To reduce possible uncertainty in the results due to the instability of the fluorescent markers, fresh protein solutions were prepared just before the adsorption experiments.

[0097] The applied method is based on the use of fluorescently labeled proteins and intensity measurements and comparison of fluorescence scanned images.

[0098] For albumin and fibrinogen experiments, samples were usually immersed in 2 ml of protein solution for 10 minutes. The adsorption process was performed in 24-well plates. The fibronectin experiment was performed in 96-well plates with 0.3 ml of protein solution, and the adsorption time was also 10 minutes. All adsorption experiments were performed at room temperature.

[0099] The protein that is not adsorbed on the surface is removed by immersing the sample in 2ml pure HEPES2 for 10 seconds. Then, they are rotated in 5ml HEPES2 for 5 seconds, and then the rinsing step is carried out with the same 5ml HEPES2. In addition, the sample is rinsed with ultrapure water for 3 seconds, dried in a nitrogen stream (pressure of about 1 bar) and stored in a 24-well plate at room temperature. In order to avoid the bleaching of the fluorescent label of the adsorbed protein, the well plate is covered with aluminum foil.

[0100] The experimental conditions are given in Table 3 below: Table 3: Experimental conditions for protein adsorption experiments Unlabeled protein uses microarray fluorescence scanner (Axon Genepix 4200A, Molecular Devices, USA) to qualitatively measure the amount of protein attached to the surface. For intensity measurement, the resolution is set to 100 μm / pixel, and each line is scanned only once. For imaging, the resolution is set to 5 μm / pixel, and each line is scanned three times. In order to read out albumin adsorption, a laser with a wavelength of 635nm is used, while the scanning of fibrinogen and fibronectin adsorption surfaces is carried out using a 532nm laser. Each sample determines the optimal focus position individually.

[0101] The photomultiplier tube (PMT) of the fluorescence scanner is specified to be linear between gains of 350-600. For this reason, all scans are performed within this PMT range. In order to maintain the grayscale limit of the fluorescence signal of the sample, the gain is adapted to each combination of surface, protein and concentration. Table 4 lists all selected gains.

[0102] Table 4: Gains selected for each batch of samples to determine protein adsorption To assess the uniformity of protein adsorption, high-resolution images were compared to each other by visual inspection.

[0103] The fluorescence intensity data obtained by fluorescence scanning are given in the following figures: Figure 7 shows a graph regarding the fluorescence intensity of albumin, fibrinogen and fibronectin measured on the surface of RXD SLA HF at low protein concentrations defined above; and Figure 8Shown are graphs for the fluorescence intensity of albumin, fibrinogen and fibronectin measured on the RXD SLA HF surface at high protein concentrations as defined above.

[0104] Figure 7 and Figure 8 All values ​​given in The corresponding intensities measured for titanium objects treated with the protocol (Ti SLActive) were normalized as a baseline. Error bars indicate standard deviation.

[0105] according to Figure 7 , at low protein concentrations, much lower adsorption of all proteins on the hydrophobic RXD SLA HF surface was determined compared to the hydrophilic Ti SLActive and RXD SLActive surfaces.

[0106] like Figure 8 As shown, at high protein concentrations, a very selective adsorption of fibrinogen was determined for the RXD SLA HF according to the invention, with an intensity comparable to that of fibrinogen adsorbed on the established Ti SLActive. At both low and high protein concentrations, the non-specific adsorption of albumin by the RXD SLA HF was much lower than that of the comparative Ti SLActive and RXD SLActive.

[0107] 1.2.5. Evaluation of fibrin network formation after incubation with whole human blood RXDSLActive HF samples were incubated with whole human blood, and the fibrin network formation was analyzed by SEM and CLSM (confocal laser scanning microscopy) imaging.

[0108] Specifically, whole human blood obtained from healthy volunteers was directly partially heparinized with 3 IU / ml sodium heparin (final concentration 0.5 IU heparin / ml blood) and used for experiments within 1 hour of withdrawal.

[0109] The samples were placed in a sample holder and freshly drawn blood was added until all samples were covered with a 4 mm thick layer of blood. To prevent further contact with air, the sample holder was closed with a lid and sealed with a Parafilm film and then incubated at room temperature on a tumbling shaker rotating at 10 rpm.

[0110] The incubation time was determined for each experiment separately. For this purpose, whole blood was spiked with labeled fibrinogen (Alexa488), which allowed real-time monitoring of blood coagulation of the samples using a fluorescence microscope. As a reference, the samples RXD SLActive (and RXD SLA) were used and two time points were selected (t1: presence of a thin fibrin network on the reference sample, t2: presence of a thick fibrin network on the reference sample).

[0111] After incubation, blood was removed and samples were washed three times by adding pre-warmed PBS to the sample holder and then incubated for 1 minute on a shaker rotating at 10 rpm for each washing step. Afterwards, samples were transferred to new 96-well plates for further processing.

[0112] For SEM imaging, the sample was fixed at room temperature (RT) for 1 hour in a modified Karnovsky solution, and then washed twice in PBS. Afterwards, the sample was dehydrated by immersing it in a gradient series of ethanol solutions (50, 70, 80, 90 and 100%), and then incubated in hexamethyldisilazane (HMDS) for 30 minutes. Finally, the sample was placed in a new 96-well plate and dried overnight at room temperature. The next day, the sample was sputtered with gold / palladium (high vacuum coater Leica EMACE 600, Switzerland). Hitachi S-4800 (Hitachi High-Technologies, Canada) was used to perform SEM imaging at an accelerating voltage of 2kV and a current of 10μA.

[0113] For CLSM analysis, the sample was incubated in PBS containing 5% goat serum and 1% FCS for 30 minutes, and then the platelets were stained with phalloidin (phalloidin) labeled with Alexa546- for 1 hour at room temperature. Platelets and fibrin networks (visible due to the addition of Alexa488-labeled fibrinogen in blood) were imaged with CLSM (magnification 10 times, 40 times). According to the coverage and thickness of the fibrin network seen by SEM imaging, only one time point (t1 or t2) was imaged. On the sample that was completely covered with fibrin on the surface, the thickness of the fibrin network was measured from the z-to-stacked image. In order to evaluate the thickness of the fibrin network, 4 z-to-stacked images (2 images for each sample, 4 to 6 measurements for each image) of 2 samples were analyzed using the measurement function of Zeiss ZEN software to measure the distance from the sample surface to the top surface of the fibrin network. CLSM analysis was carried out with three independent experiments.

[0114] Semi-quantitative analysis of SEM imaging revealed a trend toward higher fibrin network thickness and greater sample coverage for the RXD SLActive HF sample compared to the RXD SLActive sample.

[0115] This is demonstrated by the following figure, in which Fig. 9 SEM image of the surface of the sample RXD SLActive HF after 14 minutes of incubation at a magnification of about 800 times, with a scale bar corresponding to 50 micrometers given in the lower right corner of the image; Fig.10 SEM image of the surface of the sample RXD SLActive after 14 minutes of incubation at a magnification of about 800 times, with a scale bar corresponding to 50 micrometers given in the lower right corner of the image.

[0116] To evaluate the presence, distribution and thickness of the fibrin network, the semi-quantitative analysis of the SEM images is summarized in Table 5, showing, for four different experiments, in each case for two samples and for the two different incubation times given in the table, values ​​on a quantitative scale from 0 to 4, ranging from blood cell plaques with only very few visible fibrin fibers (0) to a thick fibrin network completely covering the sample surface (4).

[0117] Table 5: Semi-quantitative analysis of SEM images of four different experiments performed on RXD SLActive HF and RXD SLActive samples The thickness of fibrin formed on samples incubated with whole blood (partially heparinized, 0.5 IU / ml) for 15 and 17 minutes was evaluated as described above and the results are given in Table 6.

[0118] Table 6. Analysis of fibrin layer thickness of RXD SLActive HF and RXD SLActive samples Therefore, it was determined that the sample according to the present invention had a higher fibrin thickness than the comparative sample.

[0119] 2. Examples related to in vivo analysis Biomechanical studies in rabbits were performed to investigate the effect of surface topography on osseointegration. The connection between bone and implant was directly assessed by a pull-out test.

[0120] Materials and methods In addition, biomechanical studies in rabbits were performed to investigate the osseointegration of titanium implant discs in vivo. For these additional studies, discs were prepared as described for the in vitro experiments, but using Roxolid discs with a diameter of 6.2 mm and a thickness of 2 mm. The corresponding samples are referred to below as "RXD SLA HF II".

[0121] 2.2. Characterization of sample surface The samples were analyzed using the procedures described above for contact angle measurements and roughness parameter determination.

[0122] Regarding the contact angle measurement, the average value of "RXD SLA HF II" was found to be 123.2°.

[0123] The roughness parameter determination produced the results given in Table 7.

[0124] Table 7: Roughness values ​​of microstructures of RXD SLA HF II samples studied in vivo The results given in Table 7 confirm the findings obtained above, namely, that at least S a and S t The values ​​are in agreement with the commonly observed Moreover, with regard to the in vivo study samples, S was only insubstantially altered by process step b), i.e. the formation of the submicroscopic topography. a , S t and S sk .

[0125] 2.3. Biomechanical pull-out assay As described above, extraction studies were performed with rabbits. For this purpose, the rabbits were sedated and, during a standard surgical procedure, received two disc implants per tibia, i.e. a total of four implants per rabbit.

[0126] The implant is provided with a Teflon cap to protect against bone overgrowth and stabilized with a preformed titanium band and fixed in the cortical bone with two titanium screws. After the implantation procedure, the soft tissue layers are repositioned and the wound is closed with absorbable sutures.

[0127] The bone-implant connection was tested 4 weeks after implantation.

[0128] Detailed information on the surgical procedure and description of the pullout trial has been provided by and Ellingsen (Biomaterials 23 (2002) 2201) and Monjo et al. (Monjo et al., Biomaterials 29 (2008) 3771) elsewhere.

[0129] Table 8 gives the pull-out forces [N] measured 4 weeks after implantation.

[0130] Table 8: Pull-out force 4 weeks after implantation Average extraction force [N] Standard value Median RXD SLA HF II 50.3 23.32 50.9 As can be clearly seen from Table 8, a very high pull-out force was determined for the RXD SLA HF prepared according to the present invention. This result is most surprising considering the relatively high hydrophobicity of the RXD SLA HF surface and it emphasizes the relevance of the submicroscopic topographical configuration obtained in the subtractive process step b) of the present invention.

Claims

1. A method for preparing a topography for improving blood coagulation and / or cell attachment on an object made of titanium or a titanium alloy, The method comprises the following steps in sequence: a) etching at least a portion of the surface of the object with a first etching solution comprising an inorganic acid, b) etching the surface etched under a) with a second etching solution different from the first etching solution, the second etching solution being an aqueous solution of hydrofluoric acid, and c) storing the object obtained under b) in a NaCl solution, The object is made of a titanium-zirconium alloy.

2. The method according to claim 1, wherein by etching the surface according to step a), a microscopic topography is formed, and by etching the surface according to step b), a submicroscopic topography is formed in the microscopic topography.

3. The method according to claim 2, wherein the micro-topography is defined by at least one of the following surface parameters: i)S a is the arithmetic mean deviation of the surface in three dimensions and is in the range of 0.1 μm to 2.0 μm; ii) S t is the maximum peak-to-valley height of the profile in three dimensions and is in the range of 1.0 μm to 20.0 μm; and / or iii) S sk is the skewness of the profile in three dimensions and is in the range of -0.6 to 1.

0.

4. The method according to claim 3, wherein said S a In the range of 0.4μm to 1.8μm.

5. The method according to claim 3, wherein said S a In the range of 0.8μm to 1.7μm.

6. The method according to claim 3, wherein said S a In the range of 0.9μm to 1.5μm.

7. The method according to claim 3, wherein said S t In the range of 3.0μm to 18.0μm.

8. The method according to claim 3, wherein said S t In the range of 4.5μm to 13.0μm.

9. The method according to claim 3, wherein said S t In the range of 6.0μm to 12.0μm.

10. The method according to claim 3, wherein said S sk In the range of -0.4 to 0.6.