Preparation method and application of intelligent piezoelectric hard bone scaffold

By mixing barium titanate with calcium phosphate and using 3D printing technology to prepare intelligent piezoelectric hard bone stents, the problem of simple structure of traditional bone stents leads to limited growth of bone tissue is solved, and rapid growth and recovery of bone tissue is achieved. It is close to the microscopic characteristics and good biological performance of the human skeleton structure.

CN118903542AInactive Publication Date: 2024-11-08BEIJING INST OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411005492.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional calcium phosphate bone stents cannot perform their maximum therapeutic effects, and their simple blocky structure limits the growth of bone tissue and cannot effectively promote the healing of bone deficiencies.

Method used

By mixing barium titanate with calcium phosphate, adding ethyl 2,4,6-trimethylbenzoylphenylphosphonate and dispersant, a slurry suitable for photocuring 3D printing was prepared, and 3D printing technology was used to prepare The intelligent piezoelectric hard bone stent with complex structure simulates the microstructure of human bones and combines ultrasound to promote bone tissue growth.

Benefits of technology

It achieves rapid growth and recovery of bone tissue, provides microstructure close to the true bone morphology of the human body and good biological osteogenic performance, significantly improving the therapeutic effect and treatment speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118903542A_ABST
    Figure CN118903542A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of an intelligent piezoelectric hard bone scaffold, and belongs to the technical field of medical materials. Barium titanate and calcium phosphate are mixed and added into a solution composed of 2, 4, 6-trimethylbenzoyl phenyl ethyl phosphonate TPO, a dispersing agent KOS163 and photosensitive resin, slurry suitable for photocuring 3D printing is formed, the intelligent piezoelectric hard bone scaffold prepared from the slurry has a microstructure close to the real bone form of a human body, the interior of the intelligent piezoelectric hard bone scaffold is communicated and smooth, and the stability of the intelligent piezoelectric hard bone scaffold is improved. The method is suitable for bone tissue growth. The preparation method is simple, meanwhile, photocuring 3D printing preparation can be carried out on various complex structures, meanwhile, the material has good biological osteogenesis performance and mechanical performance close to the strength of real cancellous bones, and bone tissue growth can be promoted more rapidly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of medical materials, and in particular to a preparation method and application of an intelligent piezoelectric hard bone scaffold. Background Art

[0002] Repairing bone loss caused by trauma, bone tumors, etc. has always been a focus of urgent concern in the field of medical technology. Traditional medical bone scaffolds are mainly made of main components of human bones such as calcium phosphate and hydroxyapatite. In particular, calcium phosphate scaffolds are a widely used degradable hard ceramic bone scaffold. However, traditional calcium phosphate scaffolds are mainly composed of a single calcium phosphate. After implantation into the human body, they are passively absorbed by the human body and cannot exert the maximum therapeutic effect. Therefore, how to increase the healing rate of bone loss, optimize the treatment effect, and shorten the treatment time has always been a focus of urgent concern in the field of medical technology. Piezoelectric materials can release electrical signals (charges) without the need to implant a power supply or connect an external power supply. The charge can directly act on the tissues in the biological microenvironment, stimulating or inhibiting tissue growth and healing through electrical signals.

[0003] Barium titanate, as a lead-free piezoelectric ceramic, has good piezoelectric function and biocompatibility. It can be mixed with calcium phosphate to prepare a piezoelectric hard bone scaffold, and combined with external ultrasound, it can effectively promote the growth of bone tissue. However, bone cell growth often requires the bone scaffold structure to have good porosity and a smooth morphology close to bone connectivity, while the current barium titanate-calcium phosphate bone scaffolds are mostly simple block structures and simple pore structures, which limit their efficient promotion of bone tissue growth. Therefore, there is an urgent need to provide a material and preparation method for preparing an intelligent piezoelectric hard bone scaffold with a complex structure, and to carry out structural design and biological applications. Summary of the invention

[0004] In order to overcome the problem that it is impossible to prepare piezoelectric hard bone scaffolds with complex structures in the prior art, the present invention provides an intelligent piezoelectric hard bone scaffold material, obtains the optimal ratio of barium titanate to calcium phosphate through biological experiments, and provides a material that can be used to prepare intelligent piezoelectric hard bone scaffolds through 3D printing technology, and the prepared scaffold has good biocompatibility.

[0005] The method for preparing the intelligent piezoelectric hard bone scaffold material of the present invention comprises the following steps:

[0006] SS11: Mixing barium titanate and calcium phosphate to obtain a mixed solid A;

[0007] SS12: adding 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester (TPO) to a photosensitive resin and mixing to obtain a resin matrix B;

[0008] SS13: adding a dispersant to the resin matrix B, and then adding the mixed solid A prepared in step S1 to the resin matrix B to obtain a mixture C;

[0009] SS14: Add an equal mass of ball milling beads to mixture C, and then use a ball mill to mix for 24 hours to obtain a slurry, which is the smart piezoelectric hard bone scaffold material.

[0010] Preferably, the mass ratio of barium titanate to calcium phosphate in step SS11 is 5-9:1-5; the diameter of the calcium phosphate particles is 1-4 μm; the diameter of the barium titanate particles is 1-4 μm; and the piezoelectric constant of the barium titanate is 80 pC / N to 120 pC / N.

[0011] Preferably, the photosensitive resin in step SS12 has a viscosity of 200 to 300 mPa·s and a density of 1.08 to 1.1 g / cm 3 The addition amount of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester is 1.5%-2.5% of the mass of the photosensitive resin.

[0012] Preferably, the amount of the dispersant added in step SS13 is 5% of the mixed solid A; the ratio of the mixed solid A to the resin matrix B is 30-40 vol%:60-70 vol%.

[0013] More preferably, the photosensitive resin is 1,6-hexanediol diacrylate (HDDA); and the dispersant is KOS163 dispersant.

[0014] Another object of the present invention is to provide an intelligent piezoelectric hard bone scaffold, comprising the following steps:

[0015] SS21: Use 3D modeling technology to model the porous interconnected structure designed to simulate cancellous bone;

[0016] SS22: Print the intelligent piezoelectric hard bone scaffold material using 3D printing technology, and wash it with alcohol after printing to obtain a 3D printed scaffold;

[0017] SS23: Sintering the 3D printed scaffold to obtain the intelligent piezoelectric hard bone scaffold.

[0018] Preferably, the diameter range of the model hole size modeled in step SS21 is 100 μm-800 μm.

[0019] Preferably, the parameters of the 3D printing technology in step SS22 are set to: the ultraviolet light intensity is 0.9-2 mW / cm 2 , the slice thickness is 50 μm, and the exposure time is 6 s. In the specific experiment, the parameters are adjusted according to the different proportions of raw materials, and the purpose is only to shape the material.

[0020] Preferably, the specific steps of sintering in step SS23 are: first, the temperature is raised to 550-600°C at 1°C / min, and the binder is debonded at 550-600°C for 2 hours; then the temperature is raised to 1250-1300°C at 2°C / min, and then kept warm for 3 hours; finally, the temperature is naturally lowered to room temperature.

[0021] Another object of the present invention is to provide an application of an intelligent piezoelectric hard bone scaffold, wherein the intelligent piezoelectric hard bone scaffold is used for biological osteogenesis experiments.

[0022] The present invention provides a preparation method and application of an intelligent piezoelectric hard bone scaffold. Compared with the prior art, the present invention has the following beneficial effects: the present invention forms a slurry suitable for photocuring 3D printing by mixing barium titanate with calcium phosphate and adding the mixture to a solution composed of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester TPO, dispersant KOS163, and photosensitive resin. The intelligent piezoelectric hard bone scaffold prepared by the slurry has a microstructure close to the real bone morphology of the human body, and the internal connection is smooth and suitable for bone tissue growth. The preparation method adopted by the present invention is simple, and photocuring 3D printing preparation can also be performed for various complex structures. At the same time, the material has good bio-osteogenic properties and mechanical properties close to the real cancellous bone strength, which can promote bone tissue growth more quickly. Compared with traditional calcium phosphate scaffolds, the intelligent piezoelectric hard bone scaffold composed of piezoelectric material and calcium phosphate can obviously promote the speed of tissue recovery, and combined with advanced 3D printing technology, it can be flexibly designed for different biological application requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Diagram of a model for modeling a porous interconnected structure designed to mimic cancellous bone;

[0024] Figure 2 The relationship between the ratio of different barium titanate and calcium phosphate and the cell survival rate in Examples 1 to 5;

[0025] Figure 3 These are the results of mechanical testing of the intelligent piezoelectric hard bone scaffolds prepared with different ratios of barium titanate and calcium phosphate in Examples 1 to 5. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with the embodiments.

[0027] Example 1

[0028] Step 1: Preparation of a smart piezoelectric hard bone scaffold material

[0029] A method for preparing an intelligent piezoelectric hard bone scaffold material, wherein the volume ratio of barium titanate to calcium phosphate is 5:5, and the solid-liquid ratio (the ratio of the mixed solid A and the resin matrix B) is 3:7, and the specific steps are as follows:

[0030] SS11: 13.245 ml of barium titanate (density 6.08 g / ml, 80.5296 g) and 13.245 ml (3.16 g / ml, 41.8542 g) of calcium phosphate were mixed to obtain mixed solid A;

[0031] SS12: 70g of photosensitive resin (HDDA, density 1.08g / cm 3 , volume 61.81 ml) was added to a ball mill bottle, 1.296 g of ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO, 2% of the mass of the photosensitive resin) was added thereto, and the mixture was mixed to obtain a resin matrix B;

[0032] SS13: 6.119 g of dispersant (5% of the mass of KOS163 mixed solid A) was added to the resin matrix B, and then the mixed solid A prepared in step S1 was added to the resin matrix B to obtain a mixture C;

[0033] SS14: Add an equal amount of ball milling beads to mixed material C, seal the mixture and place it in a ball mill. After ball milling at 400 rpm for 24 hours, mix well to obtain a slurry, which is the smart piezoelectric hard bone scaffold material.

[0034] Step 2:

[0035] A method for preparing an intelligent piezoelectric hard bone scaffold, the specific steps are as follows:

[0036] SS21: Using 3D modeling technology, a porous interconnected structure designed to simulate cancellous bone is modeled. The pore size of the model ranges from 100μm to 800μm. Figure 1 ;

[0037] SS22: Using the intelligent piezoelectric hard bone scaffold material as raw material, under the ultraviolet light intensity of 0.9mW / cm 2 , the slice thickness is 50μm, the exposure time is 6s, and the 3D printing technology is used to print layer by layer. After printing, it is cleaned with alcohol to obtain a 3D printed bracket;

[0038] SS23: Sintering the 3D printed bracket, the specific method is as follows:

[0039] First, the temperature was raised to 550°C at 1°C / min, and the binder was removed at 550°C for 2 hours; then the temperature was raised to 1250°C at 2°C / min, and the temperature was kept for 3 hours; finally, the temperature was naturally lowered to room temperature to obtain the intelligent piezoelectric hard bone scaffold.

[0040] Example 2

[0041] first step:

[0042] According to the method of Example 1, an intelligent piezoelectric hard bone scaffold material is prepared, except that the volume ratio of barium titanate to calcium phosphate in the mixed solid A used in Example 2 is 6:4.

[0043] Step 2:

[0044] Printing was carried out according to the design model of Example 1, and the ultraviolet light intensity was 1.13 mW / cm 2 , the slice thickness is 50μm, the exposure time is 5s, and the 3D printing technology is used to print layer by layer. After printing, it is cleaned with alcohol to obtain a 3D printed bracket;

[0045] Then, sintering is performed according to the sintering method of Example 1 to finally obtain an intelligent piezoelectric hard bone scaffold.

[0046] Example 3

[0047] first step:

[0048] An intelligent piezoelectric hard bone scaffold was prepared according to the method of Example 1, except that the volume ratio of barium titanate to calcium phosphate in the mixed solid A used in Example 3 was 7:3.

[0049] Step 2:

[0050] Printing was carried out according to the design model of Example 1, and the ultraviolet light intensity was 1.27 mW / cm 2 , the slice thickness is 50μm, the exposure time is 6s, and the 3D printing technology is used to print layer by layer. After printing, it is cleaned with alcohol to obtain a 3D printed bracket;

[0051] Then, sintering is performed according to the sintering method of Example 1 to finally obtain an intelligent piezoelectric hard bone scaffold.

[0052] Example 4

[0053] first step:

[0054] Step 1: Prepare an intelligent piezoelectric hard bone scaffold according to the method of Example 1, except that the volume ratio of barium titanate to calcium phosphate in the mixed solid A used in Example 4 is 8:2.

[0055] Step 2:

[0056] Printing was carried out according to the design model of Example 1, and the ultraviolet light intensity was 1.33 mW / cm 2, the slice thickness is 50μm, the exposure time is 5s, and the 3D printing technology is used to print layer by layer. After printing, it is cleaned with alcohol to obtain a 3D printed bracket;

[0057] Then, sintering is performed according to the sintering method of Example 1 to finally obtain an intelligent piezoelectric hard bone scaffold.

[0058] Example 5

[0059] first step:

[0060] An intelligent piezoelectric hard bone scaffold was prepared according to the method of Example 1, except that the volume ratio of barium titanate to calcium phosphate in the mixed solid A used in Example 5 was 9:1.

[0061] Step 2:

[0062] Printing was carried out according to the design model of Example 1, and the ultraviolet light intensity was 1.51 mW / cm 2 , the slice thickness is 50μm, the exposure time is 5s, and the 3D printing technology is used to print layer by layer. After printing, it is cleaned with alcohol to obtain a 3D printed bracket;

[0063] Then, sintering is performed according to the sintering method of Example 1 to finally obtain an intelligent piezoelectric hard bone scaffold.

[0064] Mechanical property experiments and biological osteogenesis experiments were carried out on the intelligent piezoelectric hard bone scaffolds prepared in Examples 1 to 5.

[0065] Experiment 1: Combined with ultrasound (ultrasound intensity of 1.6W / cm 2 , duty cycle 60%, frequency 1MHz), using mouse osteoblast cell line (MC3T3-E1, national identification cell culture system, China) as experimental material, to study its biocompatibility, and obtain the relationship between the ratio of barium titanate and calcium phosphate and cell survival rate, such as Figure 2 As shown, the survival rate of mouse osteoblasts was greater than 90%, proving that the scaffold had good cell compatibility.

[0066] Experiment 2: Mechanical tensile test was carried out according to the national standard GBT 528-2009ISO372005. The intelligent piezoelectric hard bone scaffold prepared in Example 1 was subjected to mechanical test. The test results under different ratios of barium titanate to calcium phosphate are shown in FIG. Figure 3 As shown, with the increase of the proportion of barium titanate in the scaffold, the compressive strength of the intelligent piezoelectric hard bone scaffold gradually decreases, but is close to the strength of human cancellous bone (the strength of human cancellous bone is about 2Mpa).

[0067] Comparative Example 1

[0068] Step 1: Preparation of a hard bone scaffold material, the steps are as follows:

[0069] SS11: 26.496 ml of calcium phosphate (3.16 g / ml, 83.73 g) as solid phase;

[0070] SS12: 70g photosensitive resin (density 1.08g / cm 3 , volume 61.81 ml) was added to a ball mill bottle, 1.296 g of ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO, 2% of the mass of the photosensitive resin) was added thereto, and the mixture was mixed to obtain a resin matrix B;

[0071] SS13: 4.186 g of dispersant (5% of the mass of calcium phosphate) is added to the resin matrix B, and then the calcium phosphate prepared in step S11 is added to the resin matrix B to obtain a mixture C;

[0072] SS14: Add an equal amount of ball milling beads to mixed material C, seal the mixture and place it in a ball mill. After ball milling at 400 rpm for 24 hours, mix well to obtain a slurry, which is a calcium phosphate hard bone scaffold material.

[0073] Step 2: A method for preparing a calcium phosphate hard bone scaffold, the specific steps are as follows:

[0074] SS21: Using 3D modeling technology, a porous interconnected structure designed to simulate cancellous bone is modeled. The pore size of the model ranges from 100μm to 800μm. Figure 1 ;

[0075] SS22: Using the calcium phosphate hard bone scaffold material as raw material, under the ultraviolet light intensity of 0.83mW / cm 2 , the slice thickness is 50μm, the exposure time is 6s, and the 3D printing technology is used to print layer by layer. After printing, it is cleaned with alcohol to obtain a 3D printed bracket;

[0076] SS23: Sintering the 3D printed bracket, the specific method is as follows:

[0077] First, the temperature was raised to 550°C at 1°C / min, and the binder was removed at 550°C for 2 hours; then the temperature was raised to 1250°C at 2°C / min, and the temperature was kept for 3 hours; finally, the temperature was naturally lowered to room temperature to obtain a calcium phosphate hard bone scaffold.

[0078] The calcium phosphate hard bone scaffold prepared in Comparative Example 1 was subjected to a mouse osteoblast compatibility test, and the mouse osteoblast survival rate was only 78%, which was significantly lower than that of the intelligent piezoelectric hard bone scaffolds of Examples 1-5.

[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an intelligent piezoelectric hard bone scaffold material, It is characterized in that The following steps are involved: SS11: Mixing barium titanate and calcium phosphate to obtain a mixed solid A; SS12: adding ethyl 2,4,6-trimethylbenzoylphenylphosphonate to a photosensitive resin and mixing to obtain a resin matrix B; SS13: adding a dispersant to the resin matrix B, and then adding the mixed solid A prepared in step S1 to the resin matrix B to obtain a mixture C; SS14: Add an equal mass of ball milling beads to mixture C, and then use a ball mill to mix for 24 hours to obtain a slurry, which is the smart piezoelectric hard bone scaffold material.

2. The method for preparing the intelligent piezoelectric hard bone scaffold material according to claim 1, It is characterized in that The mass ratio of barium titanate to calcium phosphate in step SS11 is 5-9:1-5; the diameter of the calcium phosphate particles is 1-4 μm; the diameter of the barium titanate particles is 1-4 μm; the piezoelectric constant of the barium titanate is 80 pC / N to 120 pC / N.

3. The method for preparing the intelligent piezoelectric hard bone scaffold material according to claim 1, It is characterized in that The photosensitive resin in step SS12 has a viscosity of 200-300 mPa·s and a density of 1.08-1.1 g / cm 3 ; The added amount of 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester is 1.5%-2.5% of the mass of the photosensitive resin.

4. The method for preparing the intelligent piezoelectric hard bone scaffold material according to claim 1, It is characterized in that The amount of the dispersant added in step SS13 is 5% of the mixed solid A; the ratio of the mixed solid A to the resin matrix B is 30-40 vol%: 60-70 vol%.

5. The method for preparing the intelligent piezoelectric hard bone scaffold material according to claim 1, It is characterized in that The photosensitive resin is 1,6-hexanediol diacrylate; and the dispersant is KOS163 dispersant.

6. A method for preparing an intelligent piezoelectric hard bone scaffold, It is characterized in that The following steps are involved: SS21: Use 3D modeling technology to model the porous interconnected structure designed to simulate cancellous bone; SS22: Using 3D printing technology, the intelligent piezoelectric hard bone scaffold material of claim 1 is printed, and after printing, it is cleaned with alcohol to obtain a 3D printed scaffold; SS23: Sintering the 3D printed scaffold to obtain the intelligent piezoelectric hard bone scaffold.

7. The method for preparing the intelligent piezoelectric hard bone scaffold according to claim 6, It is characterized in that The diameter range of the model hole size modeled in step SS21 is 100 μm-800 μm.

8. The method for preparing the intelligent piezoelectric hard bone scaffold according to claim 6, It is characterized in that The specific steps of sintering in step SS23 are: first, the temperature is raised to 550-600°C at 1°C / min, and the binder is removed at 550-600°C for 2 hours; then the temperature is raised to 1250-1300°C at 2°C / min, and then kept warm for 3 hours; finally, the temperature is naturally lowered to room temperature.

9. Application of the intelligent piezoelectric hard bone scaffold prepared by the method according to claims 6 to 8, It is characterized in that The intelligent piezoelectric hard bone scaffold material is used in biological osteogenesis experiments.

Citation Information

Patent Citations

  • Piezoelectric calcium phosphate cement composite material

    CN102423504A

  • Preparation method of piezoelectric ceramic / bone cement biological piezoelectric composite material

    CN108042852A

  • Calcium phosphate bone induction biological ceramic stent based on photocuring 3D printing technology and preparation method thereof

    CN109650909A

  • Photocuring 3D printing minimum curved surface artificial bone scaffold and preparation method thereof

    CN117122732A

  • 3D printing strontium-doped hydroxyapatite composite scaffold and preparation method thereof

    CN117180499A