Mechanically active hydrogel for treating intestinal fistula and preparation method thereof

The treatment of intermediate intestinal fistula is solved by using mechanically active hydrogels composed of N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid and polylysine. The problem of insufficient injectability and adhesion properties of the glue has achieved effective sealing and healing of intestinal fistulas, with good biocompatibility and antibacterial properties.

CN118903553APending Publication Date: 2024-11-08NANJING GENERAL HOSPITAL NANJING MILLITARY COMMAND P L A

Patent Information

Application Number
CN202410996176.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing treatment methods for intestinal fistula, mechanically active hydrogel lacks injectability and adhesion properties, resulting in limited effect in intestinal fistula sealing treatment, and is easily squeezed out due to excessive intestinal peristalsis pressure, resulting in treatment failure. .

Method used

Mechanical active hydrogel consisting of N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid and polylysine, is quickly formed by ultraviolet light irradiation and has a volume at body temperature. The properties of shrinkage and enhanced adhesion are suitable for intestinal fistula blocking treatment.

Benefits of technology

It realizes effective sealing and healing of intestinal fistula, has good biocompatibility and antibacterial properties, can shrink the fistula at body temperature, provides epithelial cell migration scaffolds, significantly improve inflammation and collagen deposition, and is simple to operate and inexpensive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118903553A_ABST
    Figure CN118903553A_ABST
Patent Text Reader

Abstract

The invention discloses mechanically active hydrogel for treating intestinal fistula and a preparation method of the mechanically active hydrogel. The mechanically active hydrogel is temperature-sensitive hydrogel which is obtained by carrying out addition reaction on N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid and polylysine. The mechanically active hydrogel disclosed by the invention combines injectability, temperature-sensitive shrinkage performance, proper degradability, tissue adhesion and antibacterial activity. According to the present invention, through the physical and chemical cross-linking and the firm adhesion with the tissue interface, the orificium fistulae can be effectively blocked, the orificium fistulae can be shrunk under the body temperature stimulation, and the stent is provided for the migration of the intestinal mucosa epithelial cells so as to accelerate the intestinal fistula healing; the novel mechanical active hydrogel is expected to be widely applied to other regenerative medicine fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomaterials, and in particular to a mechanically active hydrogel for treating intestinal fistula and a preparation method thereof. Background Art

[0002] Intestinal fistula is a difficult problem in abdominal surgery. Promoting the self-healing of intestinal fistula can significantly shorten the course of intestinal fistula and avoid the pain of reoperation. Some smaller intestinal fistulas can heal themselves after treatments such as negative pressure irrigation and drainage, endoscopic over-range clamps, and porcine fibrin glue. Intestinal contraction and re-epithelialization of intestinal fistulas play a key role in the healing of intestinal fistulas. However, due to the limited contraction ability of the intestine, mucosal epithelial cells cannot contact to form a cell barrier, resulting in the inability to heal intestinal fistulas. Therefore, in order to promote the healing of intestinal fistulas, appropriate plugging agents are needed to fill the fistulas. On the one hand, the mechanically active hydrogel plugging agent reduces the defect area of ​​the intestinal fistula by contraction; on the other hand, it provides a scaffold for epithelial cell crawling, which is conducive to the repair of the intestinal barrier and plays a role in promoting the healing of intestinal fistulas.

[0003] Chinese invention patent application 202210109358.2 discloses a biomimetic mechanically active hydrogel dressing, which dissolves N-isopropylacrylamide, sodium alginate, HKUST-1 nanoparticles, a cross-linking agent, an initiator, and a pro-initiator in deionized water, and reacts at low temperature to prepare a cross-linked interpenetrating network hydrogel as the main network of the hydrogel to achieve a temperature-sensitive volume phase transition effect. At the same time, chitosan-g-catechol with a branched catechol structure is prepared, and the chitosan-g-catechol solution is evenly coated on the surface of the hydrogel to improve the adhesion of the hydrogel in the form of a bridging polymer. Under the synergistic effect, the skin tissue around the wound is promoted to contract and wound healing is accelerated. However, the invention is not injectable and is not suitable for the occlusion of intestinal fistulas. At the same time, the adhesion performance of the main body is improved by the chitosan coating, and the interface between the coating and the main body is easily separated, resulting in the loss of adhesion of the hydrogel dressing.

[0004] Chinese invention patent application 201710467784.2 discloses an injectable hydrogel, which is obtained by etherifying alkaline chitosan with monochloroacetic acid to obtain carboxymethyl chitosan; at the same time, sodium periodate is used to prepare hydroformyl xanthan gum, and the hydroformyl xanthan gum is reacted with carboxymethyl chitosan to generate an injectable hydrogel, which is safe, non-toxic, low-cost, and has significant resistance to enzymolysis. However, due to the lack of mechanical activity, it can only block the fistula during the treatment of intestinal fistula, and the effect of promoting the healing of intestinal fistula is limited. At the same time, due to the low mechanical strength and insufficient adhesion, when this technology is applied to the blocking treatment of intestinal fistula, it may be squeezed out of the fistula due to excessive pressure during intestinal peristalsis, resulting in treatment failure. Summary of the invention

[0005] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention aims to provide a mechanically active hydrogel for treating intestinal fistula and a preparation method thereof.

[0006] The technical solution of the present invention is as follows:

[0007] The first aspect of the present invention provides a mechanically active hydrogel, which is composed of N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid, polylysine and a photoinitiator, and can quickly form a mechanically active hydrogel (GNGP) in situ by ultraviolet light irradiation. N-isopropylacrylamide (NIPAm) polymerizes to form poly-N-isopropylacrylamide, and the polymer gradually undergoes a phase change in an environment above 32°C, which manifests itself as a reduction in volume on a macroscopic scale. Gelatin is a product of the hydrolysis of animal skin collagen and has good biocompatibility and degradability. Methacrylic anhydride can form a covalent bond with the amino group in gelatin to form methacrylic anhydride grafted gelatin (GelMA), which enables it to undergo an addition reaction with N-isopropylacrylamide, thereby enhancing the mechanical strength of the mechanically active hydrogel, and enhancing the mechanical activity of the hydrogel by limiting the swelling of the mechanically active hydrogel.

[0008] Gallic acid is a natural polyphenolic compound with excellent antioxidant properties. By cross-linking the amino groups in gelatin with the carboxyl groups of gallic acid to form gelatin-g-gallic acid (GGA), pyrogallol groups can be introduced into the mechanically active hydrogel to enhance the adhesion properties of the hydrogel. At the same time, the rich hydrogen bonds of gelatin give the mechanically active hydrogel shear thinning properties under low temperature and topological adhesion effects under body temperature. Polylysine (ε-PL) is a natural antimicrobial peptide that can destroy the cell membrane of microorganisms and has excellent antibacterial effects. Polylysine is rich in cations, and through electrostatic interaction with the negative charges in the gelatin network, it is slowly released in the mechanically active hydrogel, giving the mechanically active hydrogel a broad-spectrum antibacterial activity. In vitro and in vivo studies have shown that the mechanically active hydrogel has good biocompatibility, blocks intestinal fistulas by in situ curing, and undergoes phase change under body temperature stimulation, which is manifested as a reduction in volume on a macro scale, and transmits contractile force through interfacial adhesion, effectively promoting the healing of intestinal fistulas. Therefore, the mechanically active hydrogel described in the present invention is an ideal medical product.

[0009] The purpose of the present invention can be achieved through the following technical solutions:

[0010] A method for preparing a mechanically active hydrogel comprises dissolving N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid and polylysine in a solution containing a photoinitiator, mixing them uniformly, and then rapidly curing them by ultraviolet light irradiation, thereby obtaining the mechanically active hydrogel.

[0011] In the method for preparing the mechanically active hydrogel, the mass ratio of N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid, polylysine and photoinitiator is 1-12: 0.1-8: 0.1-8: 01-10: 0.1-5;

[0012] Preferably, the mass ratio of N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid, polylysine and photoinitiator is 3-9: 0.5-5: 0.5-3: 1-3: 0.3-0.8.

[0013] In the method for preparing the mechanically active hydrogel, the intensity of the ultraviolet light is 1 to 20.0 W / cm 2 , the irradiation time is 1 to 60 seconds; preferably: the intensity of ultraviolet light is 1 to 10.0 W / cm 2 The irradiation time is 10 to 30 seconds.

[0014] In the preparation method of the mechanically active hydrogel, the preparation method of the methacrylic anhydride grafted gelatin is as follows: after dissolving the gelatin, adding methacrylic anhydride, reacting at 50 to 60° C. for 1 to 6 hours, terminating the reaction, dialyzing, filtering, and freeze-drying to obtain the methacrylic anhydride grafted gelatin;

[0015] The mass volume ratio of gelatin to methacrylic anhydride is (1-4) g:1 ml. The dialysis temperature is 20-60°C.

[0016] In the method for preparing the mechanically active hydrogel, the method for preparing gelatin-g-gallic acid comprises the following steps:

[0017] (1) dissolving gelatin in deionized water to obtain a gelatin solution;

[0018] (2) dissolving gallic acid in a mixed solution of N,N-dimethylformamide and deionized water to obtain a gallic acid solution; then adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide to the gallic acid solution to obtain a gallic acid mixed solution.

[0019] (3) Add the gallic acid mixture to the gelatin solution, stir overnight, dialyze, and freeze-dry to obtain gelatin-g-gallic acid.

[0020] In the preparation method of gelatin-g-gallic acid: the concentration of the gelatin solution is 30-50 g / L, and the mass concentration of the gallic acid solution is 1-5%;

[0021] The mass ratio of gallic acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide is 3-8:3-10:3-8;

[0022] In step (2), the mixing ratio of N,N-dimethylformamide to deionized water is 1-5:1-5;

[0023] The mass ratio of gelatin to gallic acid is 10-15:3-8.

[0024] In the preparation method of mechanically active hydrogel, the photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (CAS: 106797-53-9) or phenyl-2.4.6-trimethylbenzoyl lithium phosphite (CAS: 85073-19-4), and the concentration of the photoinitiator solution is 0.1-1wt%.

[0025] A mechanically active hydrogel is prepared by the method.

[0026] Furthermore, in an environment of 25° C., the pore size of the mechanically active hydrogel is 1-8 μm; in an environment of 37° C., the pore size of the mechanically active hydrogel is 0.2-2 μm.

[0027] The mechanically active hydrogel prepared by the above method is used in the treatment of intestinal fistula occlusion.

[0028] Beneficial effects of the present invention:

[0029] 1. The present invention is inspired by the fact that contraction promotes wound healing, and uses the recent application of hydrogels and tissue repair to design a hydrogel intestinal fistula plugging agent that is both mechanically active and injectable. The mechanically active hydrogel is composed of N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid and polylysine. The network structure formed after the polymerization of N-isopropylacrylamide can gradually undergo a phase change when the ambient temperature exceeds 32°C, thereby achieving a reduction in the volume of the hydrogel. The rich hydrogen bonds in gelatin give the mechanically active hydrogel excellent shear-thinning properties in low-temperature environments, as well as a unique topological adhesion effect at body temperature. These characteristics make the mechanically active hydrogel injectable, so it can be used for the occlusion treatment of intestinal fistulas.

[0030] 2. The present invention prepares methacrylic anhydride-grafted gelatin capable of undergoing addition reaction with N-isopropylacrylamide by chemically modifying gelatin, thereby strengthening the mechanical strength of the mechanically active hydrogel, and limiting the swelling of the mechanically active hydrogel through a covalent cross-linked network, thereby enhancing the mechanical activity of the hydrogel and optimizing the in vivo degradation ability of the hydrogel. The present invention also simulates the mussel adhesion structure and prepares gelatin-g-gallic acid, thereby strengthening the network structure of the hydrogel through physical bonds, and at the same time, the catechol group undergoes a covalent reaction with the tissue interface, thereby improving the wet adhesion ability of the mechanically active hydrogel. In addition, polylysine, as a cationic polypeptide with broad-spectrum antibacterial activity, is adsorbed in the gelatin network through electrostatic action, giving the mechanically active hydrogel excellent antibacterial properties and effectively inhibiting pathogenic bacteria around the fistula.

[0031] 3. Compared with the existing fibrin glue used for intestinal fistula occlusion treatment, mechanically active hydrogel has many significant advantages, including strong adhesion to the tissue interface through physical synergistic chemical cross-linking, the ability to shrink the fistula under body temperature stimulation, simple production method, easy to obtain raw materials, low cost, and can be mass-produced.

[0032] 4. The mechanically active hydrogel of the present invention can effectively block the rabbit intestinal fistula animal model and promote the healing process of intestinal fistula. The hydrogel has a strong tissue interface adhesion and can effectively block the fistula. At the same time, it shrinks the internal fistula and provides a scaffold for the migration of intestinal mucosal epithelial cells, further promoting the re-epithelialization of the internal fistula. In addition, the hydrogel can also significantly improve fistula inflammation and increase collagen deposition at the site of injury.

[0033] 5. The mechanically active hydrogel of the present invention is also widely used in other regenerative medicine fields, such as the repair of pancreatic fistula, anal fistula and body surface wounds. Therefore, this mechanically active hydrogel that is easy to prepare and store shows great potential and application value in the treatment of intestinal fistulas, providing a new treatment strategy for promoting the healing of intestinal fistulas. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is the structural formula of the chemically cross-linked network of methacrylic anhydride-grafted gelatin, gelatin-g-gallic acid and mechanically active hydrogel synthesized by the present invention, wherein x and y are both integers greater than 1;

[0035] Figure 2 1H-NMR diagram of the mechanically active hydrogel synthesized in Example 1;

[0036] Figure 3 is the FTIR image of the mechanically active hydrogel synthesized in Example 1;

[0037] Figure 4 This is a rheological test diagram of the mechanically active hydrogel precursor solution synthesized in Example 1;

[0038] Figure 5 The SEM images of the mechanically active hydrogel synthesized in Example 1 under different temperature environments;

[0039] Figure 6 This is a diagram showing the area shrinkage effect of the mechanically active hydrogel synthesized in Example 2 in a 37°C environment;

[0040] Figure 7 is a graph showing the adhesion strength of the mechanically active hydrogels synthesized in Examples 1 and 3 on pig skin;

[0041] Figure 8 The mechanically active hydrogel synthesized in Example 1 is a diagram showing the effect of contracting the abdominal wall of rats in an environment of 37°C before and after;

[0042] Fig. 9 The figures are the results of in vitro toxicity test of the mechanically active hydrogel synthesized in Example 1: (a) is a fluorescence optical microscope image of fibroblasts co-cultured with the mechanically active hydrogel extract, and (b) is the quantitative statistics of (a);

[0043] Fig.10 The antibacterial effect diagram of the mechanically active hydrogel synthesized in Examples 1 and 4;

[0044] Fig.11 is the degradation curve of the mechanically active hydrogel synthesized in Example 1 in rats;

[0045] Fig.12 The figures are of the healing of rabbit intestinal fistula after treatment with the hydrogel synthesized in Example 1 and Comparative Example 1: (a) is a representative figure of HE and Masson staining of the new tissue at the fistula, and (b) is the quantitative statistics of (a). DETAILED DESCRIPTION

[0046] The present invention provides a mechanically active hydrogel for the treatment of intestinal fistula and a preparation method thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the technical scheme in the embodiment of the present application will be clearly and completely described below in conjunction with the drawings in the embodiment of the present application. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. The reagents used in the embodiments of the present invention are all purchased from the market.

[0047] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0048] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0049] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be understood as each intermediate value between the upper and lower limits of the scope also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.

[0050] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs. Although the present application describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present application.

[0051] Example 1: Preparation of GNGP mechanically active hydrogel

[0052] 6.8 g of gallic acid was dissolved in a mixed solution of 150 mL of deionized water and 100 mL of N,N-dimethylformamide, and then 7.64 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 6.4 g of N-hydroxysuccinimide were added to the gallic acid solution and stirred at room temperature for 1 hour to activate the carboxyl group. The activated gallic acid solution was added to a 40 g / L gelatin aqueous solution (300 mL) dissolved at 40° C. for 2 hours, and the solution was stirred at 40° C. overnight. After the reaction was completed, the solution was dialyzed in deionized water for 1 week, with the deionized water replaced 3 times a day. Finally, the dialyzed solution was filtered and freeze-dried to obtain gelatin-g-gallic acid, which was sealed and stored at 4° C.

[0053] Dissolve 24 g of gelatin in 300 mL of phosphate buffered saline, stir at 55°C for 3 hours, add 8 ml of methacrylic anhydride at a rate of 0.3 mL / min, and react at 55°C for 3 hours. Add 300 mL of hot phosphate buffered saline to stop the reaction, dialyze with a dialysis membrane for 7 days, and replace deionized water every 8 hours. Finally, freeze-dry the dialysate to obtain methacrylic anhydride-grafted gelatin, which is sealed and stored at 4°C.

[0054] In this embodiment, the chemical reaction equation of the GNGP mechanically active hydrogel is as follows: Figure 1As shown, 7.5 g of N-isopropylacrylamide, 1.5 g of methacrylic anhydride grafted gelatin, and 1.2 g of gelatin-g-gallic acid were dissolved in 30 mL of 0.5% 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (I2959) solution, and 2 g of polylysine was dissolved in 10 mL of 0.5% I2959 solution. Subsequently, the four solutions were mixed evenly and illuminated by ultraviolet light (6.0 W / cm 2 ) for 20 seconds for rapid solidification, thereby obtaining the mechanically active hydrogel.

[0055] Example 2: Preparation of GNGP mechanically active hydrogels with different N-isopropylacrylamide concentrations

[0056] 3.4 g of gallic acid was dissolved in 75 mL of deionized water and 50 mL of N,N-dimethylformamide, and then 3.82 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide and 3.2 g of N-hydroxysuccinimide were added to the gallic acid solution and stirred at room temperature for 1 hour to activate the carboxyl group. The activated gallic acid solution was added to a 40 g / L gelatin solution (150 mL) dissolved at 40° C. for 2 hours, and the solution was stirred at 40° C. overnight. After the reaction was completed, the solution was dialyzed in deionized water for 1 week, with the deionized water replaced 3 times a day. Finally, the dialyzed solution was filtered and freeze-dried to obtain gelatin-g-gallic acid, which was sealed and stored at 4° C.

[0057] The preparation of methacrylic anhydride grafted gelatin is the same as in Example 1.

[0058] 0.75g, 1.5g, 3g or 4.5g of methacrylic anhydride grafted gelatin was dissolved in 30mL of 0.5% I2859 deionized water solution (the mass concentration of methacrylic anhydride grafted gelatin was 2.5%, 5%, 10% and 15%), 3g, 4.5g, 6g, 7.5g or 9g of N-isopropylacrylamide was dissolved in 30mL of 0.5% I2859 deionized water solution (the mass concentration of N-isopropylacrylamide was 10%, 15%, 20%, 25% and 30%), 1.2g of gelatin-g-gallic acid was dissolved in 30mL of 2 g of polylysine was dissolved in 10 mL of 0.5% I2859 deionized water solution. Then, the methacrylic anhydride grafted gelatin solution, gelatin-g-gallic acid solution, polylysine solution and N-isopropylacrylamide solution of different concentrations were fully mixed and stored at 4 °C. The mixture was then illuminated by ultraviolet light (6.0 W / cm 2 ) were irradiated for 20 seconds for rapid curing to synthesize GNGP mechanically active hydrogels with different methacrylic anhydride grafted gelatins and different N-isopropylacrylamide concentrations.

[0059] Example 3: Preparation of GNGP mechanically active hydrogels with different gelatin-g-gallic acid concentrations

[0060] The preparation of gelatin-g-gallic acid is the same as in Example 2.

[0061] The preparation of methacrylic anhydride grafted gelatin is the same as in Example 1.

[0062] 1.5 g of methacrylic anhydride grafted gelatin was dissolved in 30 mL of 0.5% I2859 deionized water solution, 7.5 g of N-isopropylacrylamide was dissolved in 30 mL of 0.5% I2859 deionized water solution, and 0.6 g, 1.2 g, 1.8 g, 2.4 g or 3 g of gelatin-g-gallic acid were dissolved in 30 mL of 0.5% I2859 deionized water solution (the corresponding target product numbers are GNG2P, GNG4P, GNG6P, GNG8P, GNG 10 P), 2 g polylysine was dissolved in 10 mL 0.5% I2859 deionized water solution, then N-isopropylacrylamide solution, methacrylic anhydride grafted gelatin solution, gelatin-g-gallic acid solution and polylysine solution were fully mixed and stored at 4 °C. 2 ) were irradiated for 20 seconds for rapid solidification, and GNGP mechanically active hydrogels with different poly-lysine concentrations were synthesized.

[0063] Or 7.5g N-isopropylacrylamide was dissolved in 30mL 0.5% I2859 deionized water solution, 1.5g methacrylic anhydride grafted gelatin was dissolved in 30mL 0.5% I2859 deionized water solution, 2g polylysine was dissolved in 10mL 0.5% I2859 deionized water solution, the three were fully mixed, stored at 4°C, and illuminated by ultraviolet light (6.0W / cm 2 ) was irradiated for 20 seconds for rapid solidification to synthesize GNGP mechanically active hydrogel, and the corresponding target product number was GNG0P.

[0064] Example 4: Preparation of GNGP mechanically active hydrogels with different polylysine concentrations

[0065] The preparation of gelatin-g-gallic acid is the same as in Example 2.

[0066] The preparation of methacrylic anhydride grafted gelatin is the same as in Example 1.

[0067] 1.5 g of methacrylic anhydride grafted gelatin was dissolved in 30 mL of 0.5% I2859 deionized water solution, 7.5 g of N-isopropylacrylamide was dissolved in 30 mL of 0.5% I2859 deionized water solution, 1.2 g of gelatin-g-gallic acid was dissolved in 30 mL of 0.5% I2859 deionized water solution, 1 g, 2 g or 3 g of polylysine was dissolved in 10 mL of 0.5% I2859 deionized water solution (the corresponding target product numbers are GNGP 10 GNGP 20 GNGP 30 ), then the N-isopropylacrylamide solution, the methacrylic anhydride grafted gelatin solution, the gelatin-g-gallic acid solution and the polylysine solution were fully mixed and stored at 4°C. 2 ) were irradiated for 20 seconds for rapid solidification, and GNGP mechanically active hydrogels with different poly-lysine concentrations were synthesized.

[0068] Or N-isopropylacrylamide was dissolved in 30mL of 0.5% I2859 deionized water solution, 1.5g of methacrylic anhydride grafted gelatin was dissolved in 30mL of 0.5% I2859 deionized water solution, 1.2g of gelatin-g-gallic acid was dissolved in 30mL of 0.5% I2859 deionized water solution, stored at 4°C, and illuminated by ultraviolet light (6.0W / cm 2 ) irradiated for 20 seconds for rapid curing, the corresponding target product number is GNGP0,

[0069] Or 1.5 g of methacrylic anhydride grafted gelatin was dissolved in 30 mL of 0.5% I2859 deionized water solution, 1.2 g of gelatin-g-gallic acid was dissolved in 30 mL of 0.5% I2859 deionized water solution, and 1 g of polylysine was dissolved in 10 mL of 0.5% I2859 deionized water solution. Subsequently, the methacrylic anhydride grafted gelatin solution, gelatin-g-gallic acid solution and polylysine solution were fully mixed (the corresponding target product number is GN0GP 10 ), stored at 4°C, and exposed to ultraviolet light (6.0 W / cm 2 ) Irradiate for 20 seconds for rapid curing.

[0070] Example 5: Characterization of Mechanically Active Hydrogels

[0071] The synthesis of methacrylic anhydride grafted gelatin, gelatin-g-gallic acid and GNGP mechanically active hydrogels was confirmed by nuclear magnetic resonance spectroscopy. 5 mg of freeze-dried methacrylic anhydride grafted gelatin, gelatin-g-gallic acid, GNGP mechanically active hydrogel and polylysine synthesized in Example 1 were placed in 5 mm nuclear magnetic sample tubes, and 0.6 ml of deuterium oxide was added. After full dissolution, the H spectrum was measured. The freeze-dried samples of methacrylic anhydride grafted gelatin, GNGP mechanically active hydrogel and N-isopropylacrylamide synthesized in Example 1 were fully ground into powder at room temperature, and the corresponding samples were pressed into tablets using the KBr tablet method and placed in a dry place. The detection wavelength range was set to 4000-500cm -1 , according to 4cm -1 The resolution was scanned. The injectability and photocuring properties of the hydrogel synthesized in Example 1 were tested by rheological time scanning with variable temperature and alternating ultraviolet light irradiation. The morphological structure of the mechanically active hydrogel synthesized in Example 1 at 25 and 37°C was observed by scanning electron microscopy. The mechanically active hydrogel was placed in a 37°C environment, and the thermal responsiveness of the hydrogel was reflected by the change in area. The adhesion of the hydrogel to pig skin was tested using a universal mechanical machine. After the rat abdominal wall blocked with the mechanically active hydrogel was placed in a 37°C environment for 20 minutes, the effect of the hydrogel on shrinking the defective tissue was verified in vitro.

[0072] Figure 2 This is the 1H-NMR graph of the mechanically active hydrogel. As shown in the figure, the peak of gelatin-g-gallic acid at 7.0 ppm in the NMR spectrum is the proton peak of pyrogallol of gallic acid, indicating that gallic acid has been successfully grafted onto gelatin. The proton peaks of methacrylic anhydride grafted gelatin at 5.5 and 5.7 ppm indicate the successful synthesis of methacrylic anhydride grafted gelatin.

[0073] Figure 3 This is the FTIR graph of the mechanically active hydrogel. It can be seen from the figure that the mechanically active hydrogel of GNGP is similar to that of N-isopropylacrylamide at 1366 cm -1 and 1385cm -1 The absorption peak at 3300 cm is the characteristic peak of isopropyl. -1 The absorption peak at is the stretching vibration of the olefin group. After photocrosslinking, the absorption peak of the GNGP mechanically active hydrogel here is significantly reduced, which means the occurrence of addition reaction and the synthesis of GNGP hydrogel.

[0074] Figure 4This is a rheological temperature rise and intermittent UV irradiation time scan of the mechanically active hydrogel precursor solution. As shown in the figure, the GNGP precursor solution is in a gel state under low temperature conditions, and gradually becomes a sol state as the temperature rises, with a critical temperature of 25°C. Through UV irradiation, the storage modulus of the GNGP precursor solution gradually increases and a sol-gel transition occurs at 7 seconds.

[0075] Figure 5 The following are SEM images of mechanically active hydrogels at different temperatures. It can be seen from the figure that the GNGP mechanically active hydrogel has a three-dimensional porous network structure. The pore size of the mechanically active hydrogel is 1-8μm in a 25°C environment; the pore size of the mechanically active hydrogel is 0.2-2μm in a 37°C environment. The pore size of the GNGP hydrogel at 37°C is only one-fourth of the pore size at 25°C.

[0076] Figure 6 This is a diagram of the area shrinkage effect of the mechanically active hydrogel in an environment of 37°C. From the figure, it can be seen that with the increase of the concentration of methacrylic anhydride grafted gelatin and the decrease of the concentration of N-isopropylacrylamide, the deformation ability of the GNGP hydrogel gradually weakens.

[0077] Figure 7 Figure 2 is a graph showing the adhesion strength of the mechanically active hydrogel on pig skin. As shown in the figure, as the amount of gelatin-g-gallic acid added increases, the shear adhesion strength of the mechanically active hydrogel gradually increases.

[0078] Figure 8 This is a picture of the mechanically active hydrogel contracting the abdominal wall of a rat before and after in a 37°C environment. As shown in the figure, the mechanically active hydrogel can shrink its volume and change color due to phase change in a 37°C environment, thereby achieving a pulling and contracting effect on both sides of the abdominal wall.

[0079] Example 6: Toxicity study of mechanically active hydrogels at the cellular level

[0080] The concentration was 0.5×10 5 L929 fibroblasts were seeded into 12-well plates at 10 cells / well. After culturing for 24 hours, 1 mL of 1640 culture medium extract of the mechanically active hydrogel synthesized in Example 1 was added to the hydrogel group, and 1 mL of 1640 culture medium was added to the control group, and the culture was continued for 24 and 48 hours. After staining the cells with calcein and propidium iodide, images were recorded using an inverted fluorescence microscope. The results are shown in Figure 2-9 .

[0081] Fig. 9 It is a graph showing the in vitro toxicity test results of the mechanically active hydrogel. Fig. 9(a) is a fluorescence optical microscopy image of fibroblasts co-cultured with the mechanically active hydrogel extract. Fig. 9 (b) is the quantitative statistics of the number of live / dead cells. The proportion of live cells treated with the mechanically active hydrogel extract is greater than 97%, indicating that the mechanically active hydrogel has good cell compatibility.

[0082] Example 7: Study on the antibacterial properties of mechanically active hydrogels

[0083] Escherichia coli, Staphylococcus aureus and highly virulent Klebsiella pneumoniae bacterial suspensions with a concentration of 0.5 McFarland units were uniformly inoculated on LB agar plates, and 200 μL of the hydrogel synthesized in Examples 1 and 5 was placed on the surface of the plate after being sterilized by ultraviolet light for 1 hour. After incubation in a 37°C 5% CO2 incubator for 24 hours, observation was performed. The results are shown in Figure 2-10 .

[0084] Fig.10 This is the antibacterial effect diagram of mechanically active hydrogels. As shown in the figure, the hydrogel without polylysine has almost no antibacterial effect. In other groups, as the concentration of ε-PL increases, its antibacterial distance gradually increases. At the same time, N-isopropylacrylamide strengthens the antibacterial ability of the hydrogel.

[0085] Example 8: Study on the degradation properties of mechanically active hydrogels

[0086] 200 μL of the mechanically active hydrogel synthesized in Example 1 was placed in a solution containing Cy5-NHS activated ester and incubated overnight at room temperature in the dark. The hydrogel was taken out and washed in PBS in the dark for 15 minutes × 3 times. It was implanted subcutaneously in the back of Sprague-Dawley rats to evaluate its biocompatibility and degradation ability in vivo. The degradation of the hydrogel was evaluated by a small animal fluorescence imaging system immediately after surgery, on the third day after surgery, and from one to eight weeks. The results are shown in Figure 2-11 .

[0087] Fig.11 This is the degradation curve of the mechanically active hydrogel in rats. It can be seen from the figure that after eight weeks, the degradation rate of the mechanically active hydrogel in rats is as high as 99%, which has good in vivo degradation performance.

[0088] Example 9: Study on the mechanically active hydrogel promoting the healing of intestinal fistula in rabbits

[0089] New Zealand white rabbits were fasted for 1 day and 8 hours before surgery. Isoflurane was used for induction and maintenance of anesthesia. After anesthesia, the rabbits were fixed on the operating table in a supine position, the abdominal hair was shaved, and the rabbits were disinfected with iodine and 75% alcohol. After laparotomy, a stent was placed at the end of the ileum. The stent was removed on the 10th day, and the hydrogel prepared in Example 1 and commercial fibrin glue were used for occlusion treatment. The control group was not treated. The rabbits were put back in the cage and continued to be raised. After 7 days, the rabbits were killed, and the fistula and surrounding tissues were taken for HE and Masson staining to evaluate the therapeutic effect of the mechanically active hydrogel on intestinal fistula. The results are shown in Figure 2-12 .

[0090] Fig.12 This is a picture of the healing of rabbit intestinal fistula after mechanically active hydrogel treatment. Fig. 9 (a) is a representative image of HE and Masson staining of the new tissue at the fistula. Fig. 9 (b) is the quantitative statistics of the distance between the fistula opening, the width of the sinus inflammation, and the volume fraction of collagen after intestinal fistula treatment. As shown in the figure, the intestinal fistula healed faster after treatment with the mechanically active hydrogel, and the intestinal tract at the fistula opening had basically achieved full-thickness healing. At the same time, the distance of the sinus inflammation was smaller and the volume fraction of collagen was higher. This shows that the mechanically active hydrogel effectively promoted the healing of rabbit intestinal fistula.

[0091] Comparative Example 1:

[0092] The preparation of gelatin-g-gallic acid is the same as in Example 2.

[0093] The preparation of methacrylic anhydride grafted gelatin is the same as in Example 1.

[0094] 1.5 g of methacrylic anhydride grafted gelatin was dissolved in 30 mL of 0.5% I2859 deionized water solution, 1.2 g of gelatin-g-gallic acid was dissolved in 30 mL of 0.5% I2859 deionized water solution, and 2 g of polylysine was dissolved in 10 mL of 0.5% I2859 deionized water solution. Subsequently, the methacrylic anhydride grafted gelatin solution, gelatin-g-gallic acid solution and polylysine solution were fully mixed (the corresponding experimental group was the hydrogel control group), stored in an environment of 4°C, and synthesized by ultraviolet light polymerization to synthesize a hydrogel with no mechanical activity.

[0095] Comparative Example 2

[0096] The preparation of gelatin-g-gallic acid is the same as in Example 2.

[0097] 7.5 g of N-isopropylacrylamide was dissolved in 30 mL of 0.5% I2859 deionized water solution, 1.2 g of gelatin-g-gallic acid was dissolved in 30 mL of 0.5% I2859 deionized water solution, and 2 g of polylysine was dissolved in 10 mL of 0.5% I2859 deionized water solution. Subsequently, the N-isopropylacrylamide solution, gelatin-g-gallic acid solution and polylysine solution were fully mixed and stored at 4°C. A milky white flocculent product was easily formed through ultraviolet light polymerization, so no relevant detection was performed.

Claims

1. A method for preparing a mechanically active hydrogel, characterized in that: The method comprises the following steps: dissolving N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid and polylysine in a solution containing a photoinitiator, uniformly mixing, and rapidly curing by ultraviolet light irradiation, thereby obtaining the mechanically active hydrogel.

2. The mechanically active hydrogel according to claim 1, characterized in that The mass ratio of N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid, polylysine and photoinitiator is 1-12: 0.1-8: 0.1-8: 01-10: 0.1-5; Preferably, the mass ratio of N-isopropylacrylamide, methacrylic anhydride grafted gelatin, gelatin-g-gallic acid, polylysine and photoinitiator is 3-9: 0.5-5: 0.5-3: 1-3: 0.3-0.

8.

3. The mechanically active hydrogel according to claim 1, characterized in that The intensity of ultraviolet light is 1~20.0W / cm 2 , the irradiation time is 1 to 60 seconds; preferably: the intensity of ultraviolet light is 1 to 10.0 W / cm 2 The irradiation time is 10 to 30 seconds.

4. The method for preparing the mechanically active hydrogel according to claim 1, characterized in that: The preparation method of methacrylic anhydride grafted gelatin is as follows: after dissolving gelatin, adding methacrylic anhydride, reacting at 50-60° C. for 1-6 hours, terminating the reaction, dialyzing, filtering, and freeze-drying to obtain methacrylic anhydride grafted gelatin; Wherein: the mass volume ratio of gelatin to methacrylic anhydride is (1-4) g:1 ml.

5. The method for preparing the mechanically active hydrogel according to claim 1, characterized in that: The preparation method of gelatin-g-gallic acid comprises the following steps: (1) dissolving gelatin in deionized water to obtain a gelatin solution; (2) dissolving gallic acid in a mixed solution of N,N-dimethylformamide and deionized water to obtain a gallic acid solution; then adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide to the gallic acid solution to obtain a gallic acid mixed solution. (3) Add the gallic acid mixture to the gelatin solution, stir overnight, dialyze, and freeze-dry to obtain gelatin-g-gallic acid.

6. The method for preparing the mechanically active hydrogel according to claim 5, characterized in that: The concentration of the gelatin solution is 30-50 g / L, and the mass concentration of the gallic acid solution is 1-5%; The mass ratio of gallic acid, 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide is 3-8:3-10:3-8; In step (2), the mixing ratio of N,N-dimethylformamide to deionized water is 1-5:1-5; The mass ratio of gelatin to gallic acid is 10-15:3-8.

7. The method for preparing the mechanically active hydrogel according to claim 1, characterized in that: The photoinitiator is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (CAS: 106797-53-9) or phenyl-2.4.6-trimethylbenzoyl lithium phosphite (CAS: 85073-19-4), and the concentration of the photoinitiator solution is 0.1-1wt%.

8. A mechanically active hydrogel, characterized in that: The hydrogel is prepared by the method according to any one of claims 1 to 6.

9. The mechanically active hydrogel according to claim 8, characterized in that: In an environment of 25° C., the pore size of the mechanically active hydrogel is 1-8 μm; in an environment of 37° C., the pore size of the mechanically active hydrogel is 0.2-2 μm.

10. Use of the mechanically active hydrogel prepared by the method of claim 1 in the treatment of intestinal fistula occlusion.

Citation Information

Patent Citations

  • Injectable hydrogel as well as preparation method and application thereof

    CN107417801A

  • Biomimetic mechanical active hydrogel adhesive and preparation method thereof

    CN114470313A

Cited By

  • High-strength high-storage-stability temperature-sensitive phase-change reversible hydrogel and preparation method thereof

    CN119241871A

  • High-strength high-storage-stability temperature-sensitive phase-change reversible hydrogel and preparation method thereof

    CN119241871B

  • Composite hydrogel precursor fluid, preparation method and application thereof, and preparation method of anti-swelling medical hydrogel

    CN119570065A