High-flux polytetrafluoroethylene filter membrane and preparation method thereof
By pretreatment and chemical modification of the PTFE filter membrane, cross-linked network-like polymer is formed, which solves the problem of low flux and easy contamination in the aqueous phase separation system, and achieves high Flux and long-life filter performance.
Patent Information
- Application Number
- CN202411088682.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure BDA0004985888300000031 
Figure BDA0004985888300000032 
Figure BDA0004985888300000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of membrane materials, and in particular relates to a high-flux polytetrafluoroethylene filter membrane and a preparation method thereof. Background Art
[0002] Polytetrafluoroethylene (PTFE) is an ideal choice for dust filtration due to its good chemical stability, resistance to heat, cold, flame retardancy, aging, chemical corrosion, low friction coefficient, excellent electrical insulation and high and low temperature adaptability. It is also widely used in chemical, electronic, pharmaceutical and cutting-edge technology fields.
[0003] However, the surface energy of polytetrafluoroethylene filter membrane is low and its hydrophobicity is extremely strong. When treating the aqueous phase separation system, the mass transfer driving force of the fluid through the membrane is high, the body resistance is large, the energy consumption is large, and the water flux is low. In addition, the hydrophobic membrane surface is very easy to adsorb organic matter and protein, etc., resulting in concentration polarization, causing the membrane to be contaminated, resulting in a sharp drop in flux, affecting the performance of the filter membrane, and greatly reducing the service life of the filter membrane. Therefore, unmodified polytetrafluoroethylene filter membranes can only be used in fields such as waterproof and breathable, limiting their application in industrial fields such as sewage treatment, medical treatment, and sanitation.
[0004] The hydrophilic modification methods of polytetrafluoroethylene filter membrane mainly include wet chemical method, plasma treatment, high-energy radiation treatment, surface coating, etc. The wet chemical method is highly corrosive and can destroy the CF bond, forming hydrophilic groups on the surface to achieve hydrophilic modification, but it will destroy the membrane structure and make waste liquid treatment difficult; plasma and high-energy radiation treatment both activate the membrane surface to form hydrophilic groups or peroxide groups, which can further react with hydrophilic monomers, but these methods are based on the modification of the membrane surface and cannot achieve modification of the membrane pores. In addition, high-energy radiation is harmful to the human body, and plasma treatment has disadvantages such as expensive equipment. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a high-throughput polytetrafluoroethylene filter membrane and a preparation method thereof.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The method for preparing a high-throughput polytetrafluoroethylene filter membrane comprises the following steps:
[0008] (1) soaking the polytetrafluoroethylene membrane after washing with anhydrous ethanol and drying in a 10-20 wt % surfactant ethanol solution for 3-9 hours to obtain a pretreated membrane;
[0009] (2) The monomer, the auxiliary agent and the deionized water are stirred and mixed to obtain a reaction solution; then the pretreated membrane obtained in step (1) is immersed in the reaction solution, and the initiator is added. After the addition is completed, it is purged with nitrogen for 10 minutes, and then reacted at 30-60° C. for 0.2-1 hour. After the reaction is completed, it is cooled to room temperature, and then washed with deionized water for 3-5 times, and finally vacuum dried at 50° C. for 12 hours to obtain a high-throughput polytetrafluoroethylene filter membrane.
[0010] Furthermore, the polytetrafluoroethylene membrane in step (1) is one of a polytetrafluoroethylene hollow fiber membrane and a polytetrafluoroethylene flat membrane.
[0011] Furthermore, in step (1), the pore size of the polytetrafluoroethylene membrane is less than 10 microns.
[0012] Furthermore, the surfactant in step (1) is a nonionic surfactant.
[0013] Furthermore, the nonionic surfactant is one or more of polyoxyethylene laurate, alkylphenol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether.
[0014] Furthermore, the auxiliary agent is prepared by the following steps:
[0015] S1. A dry three-necked flask was purged with nitrogen for 30 minutes to drive away the air in the flask, and then 2,3-dihydroxypropyl acrylate, DBU (1,8-diazobisspiro[5.4.0]undec-7-ene) and toluene were added to the flask, stirred evenly, and then diallylamine was slowly added under nitrogen protection. After the addition was completed, the temperature was raised to 60°C and reacted for 48 hours. After the reaction was completed, vacuum distillation was performed, column chromatography was used for purification (the eluent was a mixed solvent of chloroform and diethyl ether, and the volume ratio of chloroform and diethyl ether was 9:1), and vacuum distillation was performed to obtain intermediate 1; the amount ratio of 2,3-dihydroxypropyl acrylate, diallylamine, DBU and toluene was 0.085 mol:0.08 mol:2.4 mL:180 mL;
[0016] Under the catalytic action of DBU, 2,3-dihydroxypropyl acrylate and diallylamine undergo Michael addition reaction. The reaction process is as follows:
[0017]
[0018] S2. Add intermediate 1, pyridine and DMF (N, N-dimethylformamide) to a dry three-necked flask under nitrogen protection, stir evenly and slowly add tetradecane bromide, then heat to 80°C, keep warm for 4 hours, cool to room temperature after the reaction, distill under reduced pressure, purify by column chromatography (select a mixed solvent of benzene and ethyl acetate as the eluent, the volume ratio of benzene and ethyl acetate is 8:2), distill under reduced pressure to obtain an auxiliary agent. The dosage ratio of intermediate 1, tetradecane bromide, pyridine and DMF is 0.07 mol: 0.076 mol: 8.5 mL: 180 mL.
[0019] Pyridine is used as an acid-binding agent, and the tertiary amine group of intermediate 1 and the -Br of tetradecane bromide undergo a nucleophilic substitution reaction. The reaction process is as follows:
[0020]
[0021] The auxiliary agent of the present invention has a quaternary ammonium salt antibacterial structure containing a long carbon chain (14 carbons), and the quaternary ammonium salt has good surface activity, can be combined with the cell membrane surface of bacteria and adsorbed on its surface. The positive charge in the quaternary ammonium salt molecule can attract the negative charge substance in the bacterial cell membrane, thereby destroying the membrane structure of the bacterial cell, causing bacterial death; the quaternary ammonium salt can also disturb the enzyme system inside the bacteria, affecting the metabolism and growth of the bacteria; the quaternary ammonium salt changes the protein structure by combining with anions such as chloride, acetic acid and phosphoric acid in the protein, causing the denaturation and inactivation of proteins in the bacterial cells, destroying the metabolism and growth of bacteria, and finally causing bacterial death; in addition, the quaternary ammonium salt alkyl chain can insert and crack the cell membrane, so that materials such as intracellular proteins, DNA and RNA leak so that bacteria die, and when the carbon number in the quaternary ammonium salt alkyl chain is 14, the antibacterial performance of the quaternary ammonium salt is the strongest. Therefore, the auxiliary agent of the present invention has an excellent antibacterial effect.
[0022] In addition, the additive also contains two terminal carbon-carbon double bonds and hydrophilic hydroxyl groups, so the additive and monomer can penetrate through the membrane surface into the membrane pores, and then under the action of the initiator, the two produce a chemical reaction in the pores and surface of the polytetrafluoroethylene filter membrane to form a cross-linked network polymer coated polytetrafluoroethylene filter membrane, which not only makes the filter membrane have excellent and stable antibacterial and hydrophilic properties, greatly improving the flux, but also makes the additives in the cross-linked network not easy to migrate and escape, and can stably exist in the polytetrafluoroethylene filter membrane, so that the filter membrane has excellent antibacterial effect for a long time and is not easy to be contaminated, thereby maintaining the stability of the filter membrane flux and reducing the filtration resistance. At the same time, the filtration accuracy of the filter membrane is always maintained at 99.999%, and the service life is greatly improved.
[0023] Therefore, the polytetrafluoroethylene filter membrane of the present invention has excellent and stable antibacterial property, hydrophilicity and high flux.
[0024] Furthermore, the monomer in step (2) is one or more of diethylene glycol diacrylate, ethylene glycol dimethacrylate, and 1,6-hexanediol diacrylate.
[0025] Furthermore, the mass ratio of the monomer, the auxiliary agent and the initiator is 100:0.8-2:3-5.
[0026] Furthermore, the mass concentration of the monomer in step (2) is 10-15%.
[0027] Furthermore, the initiator is one or more of ammonium persulfate, potassium persulfate, and sodium persulfate.
[0028] The invention also discloses a high-flux polytetrafluoroethylene filter membrane, which is prepared according to the preparation method of the high-flux polytetrafluoroethylene filter membrane.
[0029] The invention has the beneficial effects that the auxiliary agent and monomer containing the quaternary ammonium salt antibacterial structure produce a chemical reaction in the pores of the polytetrafluoroethylene filter membrane and on the surface of the filter membrane under the action of an initiator, so as to form a cross-linked network polymer-coated polytetrafluoroethylene filter membrane, which not only enables the filter membrane to have excellent and stable antibacterial and hydrophilic properties, reduces resistance, and greatly improves flux, but also makes the auxiliary agent in the cross-linked network difficult to migrate and escape, and can stably exist in the filter membrane, thereby making the filter membrane have excellent antibacterial effect for a long time and not easy to be contaminated, the filtration accuracy of the filter membrane can always be maintained at 99.999%, and the service life is greatly improved. DETAILED DESCRIPTION
[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] Preparation of auxiliary agent, the specific steps are as follows:
[0033] S1. A 500 mL dry three-necked flask was purged with nitrogen for 30 min to drive away the air in the flask, and then 12.4 g of 2,3-dihydroxypropyl acrylate, 2.4 mL of DBU and 180 mL of toluene were added to the flask, stirred evenly, and then 9.9 mL of diallylamine was slowly added under nitrogen protection. After the addition was completed, the temperature was raised to 60° C. and reacted for 48 h. After the reaction was completed, the mixture was distilled under reduced pressure, purified by column chromatography (the eluent was a mixed solvent of chloroform and ether, and the volume ratio of chloroform and ether was 9:1), and distilled under reduced pressure to obtain intermediate 1;
[0034] S2. Under nitrogen protection, add 17 g of intermediate 1, 8.5 mL of pyridine and 180 mL of DMF into a 500 mL dry three-necked flask, stir evenly and then slowly add 22.6 mL of tetradecane bromide, then raise the temperature to 80°C and keep the reaction for 4 hours. After the reaction is completed, cool to room temperature, distill under reduced pressure, purify by column chromatography (a mixed solvent of benzene and ethyl acetate is selected as the eluent, and the volume ratio of benzene and ethyl acetate is 8:2), and distill under reduced pressure to obtain an auxiliary agent.
[0035] Example 2
[0036] Prepare the polytetrafluoroethylene filter membrane. The specific steps are as follows:
[0037] (1) soaking a polytetrafluoroethylene flat membrane with a pore size of less than 10 μm after cleaning with anhydrous ethanol for 1 hour and drying in an ethanol solution of 10 wt % fatty alcohol polyoxyethylene ether for 3 hours to obtain a pretreated membrane;
[0038] (2) 1,6-hexanediol diacrylate, the auxiliary agent prepared in Example 1 and deionized water were fully stirred and mixed uniformly, wherein the mass concentration of 1,6-hexanediol diacrylate was 10%, to obtain a reaction solution; then the pretreated membrane obtained in step (1) was immersed in the reaction solution, and sodium persulfate was added. After the addition was completed, nitrogen was purged for 10 minutes, and then reacted at 30° C. for 0.2 hours, wherein the mass ratio of 1,6-hexanediol diacrylate, the auxiliary agent prepared in Example 1 and sodium persulfate was 100:0.8:3. After the reaction was completed, it was cooled to room temperature, washed with deionized water for 3 times, and finally vacuum dried at 50° C. for 12 hours to obtain a polytetrafluoroethylene filter membrane.
[0039] Example 3
[0040] Prepare the polytetrafluoroethylene filter membrane. The specific steps are as follows:
[0041] (1) soaking a polytetrafluoroethylene hollow fiber membrane having a pore size of less than 10 μm after cleaning with anhydrous ethanol for 1 hour and drying in an ethanol solution containing 20 wt % alkylphenol polyoxyethylene ether for 9 hours to obtain a pretreated membrane;
[0042] (2) Ethylene glycol dimethacrylate, the auxiliary agent prepared in Example 1 and deionized water are fully stirred and mixed uniformly, wherein the mass concentration of ethylene glycol dimethacrylate is 15%, to obtain a reaction solution; then the pretreated membrane obtained in step (1) is immersed in the reaction solution, and potassium persulfate is added. After the addition is completed, nitrogen is purged for 10 minutes, and then the reaction is carried out at 40° C. for 1 hour, wherein the mass ratio of ethylene glycol dimethacrylate, the auxiliary agent prepared in Example 1 and potassium persulfate is 100:2:5. After the reaction is completed, the membrane is cooled to room temperature, washed with deionized water for 5 times, and finally vacuum dried at 50° C. for 12 hours to obtain a polytetrafluoroethylene filter membrane.
[0043] Example 4
[0044] Prepare the polytetrafluoroethylene filter membrane. The specific steps are as follows:
[0045] (1) soaking a polytetrafluoroethylene hollow fiber membrane having a pore size of less than 10 μm after cleaning with anhydrous ethanol for 1 hour and drying in an ethanol solution of 12 wt % polyoxyethylene laurate for 4 hours to obtain a pretreated membrane;
[0046] (2) diethylene glycol diacrylate, the auxiliary agent prepared in Example 1 and deionized water were fully stirred and mixed uniformly, wherein the mass concentration of diethylene glycol diacrylate was 11%, to obtain a reaction solution; then the pretreated membrane obtained in step (1) was immersed in the reaction solution, and ammonium persulfate was added. After the addition was completed, nitrogen was purged for 10 minutes, and then the reaction was carried out at 60° C. for 0.5 hours, wherein the mass ratio of diethylene glycol diacrylate, the auxiliary agent prepared in Example 1 and ammonium persulfate was 100:1:4. After the reaction was completed, the membrane was cooled to room temperature, washed with deionized water for 4 times, and finally dried in vacuum at 50° C. for 12 hours to obtain a polytetrafluoroethylene filter membrane.
[0047] Comparative Example 1
[0048] Prepare the polytetrafluoroethylene filter membrane. The specific steps are as follows:
[0049] The remaining steps remain unchanged, except that the polytetrafluoroethylene hollow fiber membrane with a membrane pore size of less than 10 μm is soaked and cleaned with anhydrous ethanol for 1 hour and vacuum dried at 50° C. for 12 hours to obtain a polytetrafluoroethylene filter membrane.
[0050] Comparative Example 2
[0051] The remaining steps remain unchanged, except for step (2) of Example 4, to obtain a polytetrafluoroethylene filter membrane.
[0052] Comparative Example 3
[0053] Prepare the polytetrafluoroethylene filter membrane. The specific steps are as follows:
[0054] The remaining steps remain unchanged, and the auxiliary agent in step (2) of Example 4 is removed to obtain a polytetrafluoroethylene filter membrane.
[0055] Comparative Example 4
[0056] Prepare the polytetrafluoroethylene filter membrane. The specific steps are as follows:
[0057] The remaining steps remain unchanged, and the auxiliary agent in step (2) of Example 4 is replaced by dodecyltrimethylammonium chloride to prepare a polytetrafluoroethylene filter membrane.
[0058] Performance Testing
[0059] The water contact angle, antibacterial property and pure water flux of the filter membranes of Examples 2-4 and Comparative Examples 1-3 were tested before and after washing for 30 days; the antibacterial property test was in accordance with GB / T31402-2015; the pure water flux test pressure was 0.1 MPa, pre-pressed for 30 minutes before the test, and the pure water flux F = V / (S×t), where V represents the volume of water obtained by filtration in a certain period of time, S represents the effective area of the membrane, and t represents the filtration time. The test results of all items are shown in the following table:
[0060]
[0061] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0062] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a high-throughput polytetrafluoroethylene filter membrane, characterized in that: The following steps are involved: (1) soaking a polytetrafluoroethylene membrane in an ethanol solution containing 10-20 wt % of a surfactant for 3-9 hours to obtain a pretreated membrane; (2) stirring the monomer, the additive and the deionized water to obtain a reaction solution; immersing the pretreated membrane in the reaction solution, adding an initiator, purging with nitrogen, reacting at 30-60° C. for 0.2-1 h, cooling, washing and drying to obtain a high-flux polytetrafluoroethylene filter membrane; Wherein, the auxiliary agent is prepared by the following steps: S1, after nitrogen blowing into the flask, add 2,3-dihydroxypropyl acrylate, DBU and toluene, stir, add diallylamine, react at 60°C for 48h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 1; S2. Under nitrogen protection, add intermediate 1, pyridine and DMF into a flask, stir and add tetradecane bromide, react at 80° C. for 4 h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain an auxiliary agent.
2. The method for preparing a high-throughput polytetrafluoroethylene filter membrane according to claim 1, characterized in that: The usage ratio of 2,3-dihydroxypropylacrylate, diallylamine, DBU and toluene in step S1 is 0.085 mol: 0.08 mol: 2.4 mL: 180 mL; the usage ratio of intermediate 1, tetradecane bromide, pyridine and DMF in step S2 is 0.07 mol: 0.076 mol: 8.5 mL: 180 mL.
3. The method for preparing a high-throughput polytetrafluoroethylene filter membrane according to claim 1, characterized in that: The polytetrafluoroethylene membrane in step (1) is one of a polytetrafluoroethylene hollow fiber membrane and a polytetrafluoroethylene flat membrane.
4. The method for preparing a high-throughput polytetrafluoroethylene filter membrane according to claim 1, characterized in that: The pore size of the polytetrafluoroethylene membrane in step (1) is less than 10 microns.
5. The method for preparing a high-throughput polytetrafluoroethylene filter membrane according to claim 1, characterized in that: The surfactant in step (1) is a nonionic surfactant.
6. The method for preparing a high-throughput polytetrafluoroethylene filter membrane according to claim 5, characterized in that: The nonionic surfactant is one or more of polyoxyethylene laurate, alkylphenol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether.
7. The method for preparing a high-throughput polytetrafluoroethylene filter membrane according to claim 1, characterized in that: The monomer in step (2) is one or more of diethylene glycol diacrylate, ethylene glycol dimethacrylate, and 1,6-hexanediol diacrylate.
8. The method for preparing a high-throughput polytetrafluoroethylene filter membrane according to claim 1, characterized in that: The mass ratio of the monomer, the auxiliary agent and the initiator is 100:0.8-2:3-5; the mass concentration of the monomer in step (2) is 10-15%.
9. The method for preparing a high-throughput polytetrafluoroethylene filter membrane according to claim 1, characterized in that: The initiator is one or more of ammonium persulfate, potassium persulfate and sodium persulfate.
10. High flux polytetrafluoroethylene filter membrane, characterized in that: The high-throughput polytetrafluoroethylene filter membrane is prepared according to the preparation method of any one of claims 1 to 9.
Citation Information
Cited By
Polyacrylonitrile / polyamide composite porous membrane as well as preparation method and application thereof
CN119746657A