Modified zeolite material for synchronously removing ammonia nitrogen and phosphate in wastewater and preparation method of modified zeolite material

By zircon and sodium modification of natural zeolites, Zr-Na-Z composite materials were prepared, which solved the problem of poor adsorption of natural zeolites on ammonia nitrogen and phosphate, achieved efficient wastewater treatment, and improved wastewater The removal capacity of ammonia nitrogen and phosphate is suitable for the treatment of lake sediment pollutants.

CN118904281AActive Publication Date: 2024-11-08HUAZHONG UNIV OF SCI & TECH

Patent Information

Application Number
CN202411262868.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-08
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove ammonia nitrogen and phosphate in wastewater, especially natural zeolites, and the regeneration capacity of modified zeolites is limited, which affects its economic and sustainability in practical applications.

Method used

By first modifying the natural zeolite and then modifying sodium, Zr-Na-Z composite material is prepared, and the principle of exchange between zirconium oxide and sodium ions is used to improve the adsorption capacity of ammonia nitrogen and phosphate.

Benefits of technology

It significantly improves the adsorption capacity of ammonia nitrogen and phosphate, especially in low-concentration water bodies, and shows efficient removal effect. It is suitable for batch construction of adsorbent materials, improving the economic and sustainable water treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904281A_ABST
    Figure CN118904281A_ABST
Patent Text Reader

Abstract

The invention discloses a modified zeolite material for synchronously removing ammonia nitrogen and phosphate in wastewater and a preparation method thereof.Natural zeolite is taken as a carrier, synchronous adsorption of ammonia nitrogen and phosphate is taken as a target, the zeolite is subjected to function regulation, the internal structure and surface physicochemical properties of the zeolite are modified and regulated in a targeted mode, and the modified zeolite is prepared. The Zr-Na-Z composite material capable of efficiently and synchronously removing low-concentration ammonia nitrogen and phosphate is successfully obtained, the Zr-Na-Z composite material has good application prospects in the field of nitrogen and phosphorus sewage treatment and the field of lake sediment pollutant passivation, the method is suitable for constructing adsorbing materials in batches, and the preparation process is simple and efficient; in an adsorption experiment for simulating a low-concentration water body with the concentration of 10 mg / l ammonia nitrogen and 2 mg / l phosphate, compared with the original zeolite, the modified zeolite material prepared by the invention has the advantages that the adsorption capacity of the ammonia nitrogen is increased from 2.92 mg / g to 3.52 mg / g and the adsorption capacity of the phosphate is increased from 0 mg / g to 0.94 mg / g, which are obviously increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment, and in particular to a modified zeolite material for simultaneously removing ammonia nitrogen and phosphate in wastewater and a preparation method thereof. Background Art

[0002] The discharge of domestic sewage and industrial wastewater has become an important source of water pollution worldwide, especially in my country, where the concentrations of nitrogen and phosphorus in lakes and rivers have increased significantly, leading to serious ecological and environmental problems. The intensification of water eutrophication has not only affected the water quality, but also had a profound impact on the aquatic ecosystem. Although my country has taken a series of measures to control water eutrophication in recent years, the state of lake eutrophication still exists, and ammonia nitrogen and phosphate are still the most common water pollutants in my country. The large amount of these two types of pollutants and their wide distribution have brought huge pollution pressure to the water environment and seriously affected the self-purification capacity and ecological balance of the water body. Therefore, effectively controlling the discharge of ammonia nitrogen and phosphorus in water bodies has become a major environmental protection issue that my country urgently needs to solve.

[0003] As an important mineral material, natural zeolite has good ion exchange capacity and adsorption performance. Natural zeolite is a type of hydrous alkali metal or alkaline earth metal aluminosilicate mineral. Due to its unique crystal structure, it can accommodate cations in the lattice cavities to achieve ion exchange. The rich pore structure of natural zeolite enables it to effectively adsorb pollutants in water during water treatment. Compared with synthetic zeolite, natural zeolite is not only cheap, but also abundant and easy to obtain.

[0004] In recent years, the research on the removal of ammonia nitrogen using natural zeolites has attracted extensive attention from researchers at home and abroad. Through simple modification methods such as salt, high temperature, and alkali treatment, researchers have successfully prepared some modified zeolites with good ammonia nitrogen removal performance. These modified zeolites perform well in removing ammonia nitrogen, but they still have the disadvantage of not being able to be regenerated multiple times, which limits their economy and sustainability in practical applications.

[0005] On the other hand, phosphorus mainly exists in the form of anions in water, which causes electrostatic repulsion between it and the negatively charged zeolite framework, resulting in poor adsorption of phosphorus by natural zeolites. In order to improve the phosphorus removal ability of natural zeolites, researchers are exploring a variety of modification methods, including surface modification and preparation of composite materials.

[0006] For example, Chinese patent document CN111530412A discloses a method for synthesizing a simultaneous denitrification and phosphorus removal adsorbent based on natural zeolite. By introducing lanthanum element in the process of synthesizing molecular sieve from natural zeolite, a lanthanum-modified molecular sieve adsorbent with simultaneous denitrification and phosphorus removal performance is prepared. The prepared adsorbent has a good adsorption effect on ammonium and phosphate ions, but the ability to remove ammonia nitrogen in wastewater still needs to be further improved. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a modified zeolite material and a preparation method thereof for simultaneously removing ammonia nitrogen and phosphate in wastewater. The goal of simultaneously removing ammonia nitrogen and phosphate in wastewater is achieved by first modifying natural zeolite with zirconium and then with sodium.

[0008] In order to achieve the above object, the present invention adopts the following technical scheme:

[0009] A method for preparing a modified zeolite material for simultaneously removing ammonia nitrogen and phosphate in wastewater comprises the following steps:

[0010] S1. Add natural zeolite and soluble zirconium salt into deionized water, mix well and shake, evaporate and remove deionized water after shaking, and then dry, wash and dry to obtain zirconium-modified natural zeolite;

[0011] S2. Add the zirconium-modified natural zeolite to the NaCl solution, mix evenly to obtain a solid-liquid mixture, and then put the solid-liquid mixture into a water bath oscillator for oscillation. After the oscillation is completed, take out the solid, wash it, and dry it to obtain a modified zeolite material.

[0012] Specifically, in step S1, the mass ratio of natural zeolite and soluble zirconium salt is 10:2-6. In some embodiments of the present invention, for example, 10:2, 10:3, 10:4, 10:5, 10:6 can be selected, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] Wherein, the natural zeolite is 40-80 mesh, and the soluble zirconium salt is selected from ZrOCl 2 8(H 2 O) or ZrO(NO 3 ) 2 ·2H 2 O.

[0014] Specifically, in step S1, the usage ratio of natural zeolite and deionized water is 1g:10-15mL. In some embodiments of the present invention, for example, 1g:10mL, 1g:11mL, 1g:12mL, 1g:13mL, 1g:14mL, 1g:15mL can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] Specifically, in step S1, the rotation speed of the shaker during the shaking process is 100-400r / min. In some embodiments of the present invention, for example, 100r / min, 200r / min, 300r / min, and 400r / min can be selected; the shaking time is 18-36h, for example, 18h, 24h, 30h, and 36h can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] Specifically, in step S2, the dosage ratio of zirconium-modified natural zeolite and NaCl solution is 1g:15-30mL. In some embodiments of the present invention, for example, 1g:15mL, 1g:20mL, 1g:25mL, 1g:30mL can be selected, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] The concentration of the NaCl solution is 0.1-1.5 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.4 mol / L, 0.5 mol / L, 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.5 mol / L can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] Specifically, in step S2, the rotation speed of the oscillator is 100-300 r / min, for example, 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min can be selected; the oscillation time is 4-8 h, for example, 4 h, 5 h, 6 h, 7 h, 8 h can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] The present invention provides a modified zeolite material prepared by the above preparation method.

[0020] The present invention also provides application of the modified zeolite material in wastewater treatment.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention uses natural zeolite as a carrier, aims at the simultaneous adsorption of ammonia nitrogen and phosphate, regulates the function of zeolite, specifically modifies and regulates the internal structure and surface physicochemical properties of zeolite, and successfully obtains a Zr-Na-Z composite material that can efficiently and simultaneously remove low concentrations of ammonia nitrogen and phosphate. It has good application prospects in the fields of nitrogen and phosphorus wastewater treatment and lake sediment pollutant passivation. This method is suitable for batch construction of adsorption materials, and the preparation process is simple and efficient.

[0023] (2) In the adsorption experiment simulating a low concentration of water with ammonia nitrogen of 10 mg / l and phosphate of 2 mg / l, the modified zeolite material prepared by the present invention has a significant improvement in the adsorption capacity of ammonia nitrogen from 2.92 mg / g to 3.52 mg / g and the adsorption capacity of phosphate from 0 mg / g to 0.94 mg / g compared with the original zeolite at this concentration.

[0024] (3) The applicant also found that the adsorption effect of the adsorbent material obtained by first modifying the natural zeolite with zirconium and then with sodium is better than that of the adsorbent material obtained by first modifying with sodium and then with zirconium. This may be because if the sodium modification is performed first, due to the principle of ion exchange adopted by the salt modification, when the high concentration of zirconium is regulated, some Na ions will be exchanged out, resulting in a decrease in its removal effect on ammonia nitrogen. However, the zirconium regulation modification is performed first, and the phosphate removal is based on the principle of surface zirconium oxide anion ligand exchange, and the generated zirconium oxide is more stable and attached to the surface of the zeolite. It is not easy to fall off during the next step of salt modification, and it can more efficiently improve its removal rate of ammonia nitrogen. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is the SEM image of the natural zeolite of Comparative Example 1;

[0026] Figure 2 is the EDS image of the natural zeolite of Comparative Example 1;

[0027] Figure 3 is a SEM image of the modified zeolite material prepared in Example 1;

[0028] Figure 4 This is the EDS graph of the modified zeolite material prepared in Example 1. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.

[0030] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.

[0031] The mesh number of the natural zeolite used in the present invention is 40-80 mesh.

[0032] Example 1

[0033] A method for preparing a modified zeolite material for simultaneously removing ammonia nitrogen and phosphate in wastewater comprises the following steps:

[0034] S1, 10g natural zeolite and 4g ZrOCl 2 8(H 2 O) was added into 100 mL of deionized water, mixed and shaken, the speed of the shaker was 200 r / min, the shaking time was 24 h, after the shaking was completed, it was placed in a 100 ° C water bath, the deionized water was evaporated and removed, the obtained material was moved to a 105 ° C oven, dried for 2 h, and the obtained product was washed 5 times with deionized water, and dried again in a 105 ° C oven for 2 h to obtain a zirconium-modified natural zeolite;

[0035] S2. Add 10 g of zirconium-modified natural zeolite to 200 mL of 1.0 mol / L NaCl solution, mix well to obtain a solid-liquid mixture, and then put the solid-liquid mixture into a water bath oscillator for oscillation treatment. The oscillator speed is 200 r / min, the water temperature is 25°C, and the oscillation time is 6 h. After the oscillation is completed, wash with deionized water 3 times, collect the solid and dry it in a 105°C forced air drying oven for 12 h to obtain a modified zeolite material.

[0036] Example 2

[0037] A method for preparing a modified zeolite material for simultaneously removing ammonia nitrogen and phosphate in wastewater comprises the following steps:

[0038] S1, 10g natural zeolite and 4g ZrOCl 2 8(H 2 O) was added into 100 mL of deionized water, mixed and shaken, the speed of the shaker was 200 r / min, the shaking time was 24 h, after the shaking was completed, it was placed in a 100 ° C water bath, the deionized water was evaporated and removed, the obtained material was moved to a 105 ° C oven, dried for 2 h, and the obtained product was washed 5 times with deionized water, and dried again in a 105 ° C oven for 2 h to obtain a zirconium-modified natural zeolite;

[0039] S2. Add 10 g of zirconium-modified natural zeolite to 200 mL of 0.1 mol / L NaCl solution, mix well to obtain a solid-liquid mixture, and then put the solid-liquid mixture into a water bath oscillator for oscillation treatment. The oscillator speed is 200 r / min, the water temperature is 25°C, and the oscillation time is 6 h. After the oscillation is completed, wash with deionized water 3 times, collect the solid and dry it in a 105°C forced air drying oven for 12 h to obtain a modified zeolite material.

[0040] Compared with Example 1, Example 2 is a method in which the concentration of the NaCl solution is replaced with 0.1 mol / L.

[0041] Example 3

[0042] A method for preparing a modified zeolite material for simultaneously removing ammonia nitrogen and phosphate in wastewater comprises the following steps:

[0043] S1, 10g natural zeolite and 4g ZrOCl 2 8(H 2 O) was added into 100 mL of deionized water, mixed and shaken, the speed of the shaker was 200 r / min, the shaking time was 24 h, after the shaking was completed, it was placed in a 100 ° C water bath, the deionized water was evaporated and removed, the obtained material was moved to a 105 ° C oven, dried for 2 h, and the obtained product was washed 5 times with deionized water, and dried again in a 105 ° C oven for 2 h to obtain a zirconium-modified natural zeolite;

[0044] S2. Add 10 g of zirconium-modified natural zeolite to 200 mL of 1.5 mol / L NaCl solution, mix well to obtain a solid-liquid mixture, and then put the solid-liquid mixture into a water bath oscillator for oscillation treatment. The oscillator speed is 200 r / min, the water temperature is 25°C, and the oscillation time is 6 h. After the oscillation is completed, wash with deionized water 3 times, collect the solid and dry it in a 105°C forced air drying oven for 12 h to obtain a modified zeolite material.

[0045] Compared with Example 1, Example 3 is a method in which the concentration of the NaCl solution is replaced with 1.5 mol / L.

[0046] Comparative Example 1

[0047] Natural zeolite is used as the adsorption material without modification.

[0048] Comparative Example 2

[0049] A method for preparing a modified zeolite material comprises the following steps:

[0050] 10g natural zeolite and 4g ZrOCl 2 8(H 2 O) was added into 100 mL of deionized water, mixed evenly and then shaken. During the shaking process, the speed of the shaker was 200 r / min and the shaking time was 24 h. After the shaking was completed, it was placed in a 100 ° C water bath to evaporate and remove the deionized water. The obtained material was moved to a 105 ° C oven and dried for 2 h. The obtained product was washed 5 times with deionized water and dried again in a 105 ° C oven for 2 h to obtain a modified zeolite material.

[0051] Compared with Example 1, Comparative Example 2 did not undergo sodium ion modification treatment.

[0052] Comparative Example 3

[0053] A method for preparing a modified zeolite material for simultaneously removing ammonia nitrogen and phosphate in wastewater comprises the following steps:

[0054] S1. Add 10 g of natural zeolite to 200 mL of 1.0 mol / L NaCl solution, mix well to obtain a solid-liquid mixture, and then put the solid-liquid mixture into a water bath oscillator for oscillation treatment. The oscillator speed is 200 r / min, the water temperature is 25 ° C, and the oscillation time is 6 h. After the oscillation is completed, wash with deionized water 3 times, collect the solid and dry it in a 105 ° C forced air drying oven for 12 h to obtain sodium modified zeolite;

[0055] S2, 10g sodium modified zeolite and 4g ZrOCl 2 8(H 2 O) was added into 100 mL of deionized water, mixed evenly and then shaken. During the shaking process, the speed of the shaker was 200 r / min and the shaking time was 24 h. After the shaking was completed, it was placed in a 100 ° C water bath to evaporate and remove the deionized water. The obtained material was moved to a 105 ° C oven and dried for 2 h. The obtained product was washed 5 times with deionized water and dried again in a 105 ° C oven for 2 h to obtain a modified zeolite material.

[0056] Compared with Example 1, in Comparative Example 3, the natural zeolite is firstly modified with sodium and then with zirconium.

[0057] The SEM of natural zeolite in Comparative Example 1 is as follows: Figure 1 As shown, the EDS of natural zeolite is Figure 2 As shown, the SEM of the modified zeolite material prepared in Example 1 is as follows Figure 3 As shown, the EDS of the modified zeolite material is Figure 4 As shown in the figure, it can be seen that compared with the original zeolite, the surface of the modified zeolite material has disappeared particle fragments, the surface has become looser, rough and uneven, and obvious grooves appear. After loading zirconium oxide, more granular substances appear on the surface, the previous grooves are partially filled, the particles are loosely arranged, and the dispersion is relatively uniform; compared with the original zeolite, the relative mass proportions of Zr and Na elements on the surface of the modified zeolite material are significantly improved, the relative mass of Na element increases from 0.8% to 1.4%, and the relative mass of Zr element increases from 0% to 10.7%.

[0058] The samples prepared in Examples 1-3 and Comparative Examples 1-3 were respectively put into simulated wastewater, where the concentrations of ammonia nitrogen (in terms of N) and phosphate (in terms of P) in the simulated wastewater were 10 mg / L and 2.0 mg / L, respectively, the solution pH was 7.0, the dosage was 2.0 g / L, the adsorption time was 6 h, the temperature was 25° C., and the speed of the water bath oscillator was 200 r / min, and the removal effects of ammonia nitrogen and phosphate were measured;

[0059] The test results are shown in the following table:

[0060] Ammonia nitrogen adsorption capacity (mg / g) Phosphate adsorption capacity (mg / g) Example 1 3.52 0.94 Example 2 2.87 0.97 Example 3 3.49 0.94 Comparative Example 1 2.92 0 Comparative Example 2 1.61 0.99 Comparative Example 3 3.05 0.88

[0061] In Comparative Example 2, no sodium ion modification was performed. The concentration of the NaCl solution in Example 2 was 0.1 mol / L, the concentration of the NaCl solution in Example 1 was 1 mol / L, and the concentration of the NaCl solution in Example 3 was 1.5 mol / L. As can be seen from the table above, the removal effect of the sample on phosphate slightly decreased with the increase of the NaCl modification concentration, and there was a slight antagonistic effect, while the removal effect on ammonia nitrogen increased with the increase of the NaCl modification concentration. After reaching 1.0 mol / L, the NaCl concentration continued to increase, and the effect of improving ammonia nitrogen remained basically unchanged. Considering the economic factor, it is best to select 1.0 mol / L NaCl solution for modification.

[0062] It can be seen from Example 1 and Comparative Example 3 that the adsorption effect of the adsorbent obtained by first modifying the natural zeolite with zirconium and then modifying it with sodium on ammonia nitrogen and phosphate is better than that of the adsorbent obtained by first modifying it with sodium and then modifying it with zirconium.

[0063] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.

Claims

1. A method for preparing a modified zeolite material for simultaneously removing ammonia nitrogen and phosphate from wastewater, characterized in that: The steps include: S1. Add natural zeolite and soluble zirconium salt into deionized water, mix well and shake, evaporate and remove deionized water after shaking, and then dry, wash and dry to obtain zirconium-modified natural zeolite; S2. Add the zirconium-modified natural zeolite to the NaCl solution, mix evenly to obtain a solid-liquid mixture, and then put the solid-liquid mixture into a water bath oscillator for oscillation. After the oscillation is completed, take out the solid, wash it, and dry it to obtain a modified zeolite material.

2. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of natural zeolite to soluble zirconium salt is 10:2-6.

3. The preparation method according to claim 1, characterized in that: In step S1, the soluble zirconium salt is selected from ZrOCl2·8(H2O) or ZrO(NO3)2·2H2O.

4. The preparation method according to claim 1, characterized in that: In step S1, the usage ratio of natural zeolite and deionized water is 1 g:10-15 mL.

5. The preparation method according to claim 1, characterized in that: In step S1, the rotation speed of the shaking table during the shaking process is 100-400 r / min, and the shaking time is 18-36 h.

6. The preparation method according to claim 1, characterized in that: In step S2, the usage ratio of zirconium-modified natural zeolite and NaCl solution is 1 g:15-30 mL.

7. The preparation method according to claim 1, characterized in that: In step S2, the concentration of the NaCl solution is 0.1-1.5 mol / L.

8. The preparation method according to claim 1, characterized in that: In step S2, the rotation speed of the oscillator is 100-300 r / min, and the oscillation time is 4-8 h.

9. The modified zeolite material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the modified zeolite material according to claim 9 in wastewater treatment.

Citation Information

Patent Citations

  • Modified zeolite adsorbent for removing ammonia nitrogen and phosphate in water, and preparation and regeneration method thereof

    CN105381782A

  • Natural water purifying agent as well as preparation method and application thereof

    CN114132977A

Cited By

  • Zinc modified montmorillonite material for synchronously removing ammonia nitrogen and phosphate in wastewater and preparation method of zinc modified montmorillonite material

    CN120550774A