Hydrophobic Cu / SiO2 catalyst and preparation and application thereof
By hydrophobic treatment of Cu/SiO2 catalyst, the acidic sites on the catalyst surface are reduced, the dehydration and hydrogenation reaction activity is reduced, the selectivity and yield of dioxycyclohexanone are improved, and the problem of low selectivity of existing catalysts is solved. , achieving efficient synthesis of dioxycyclohexanone.
Patent Information
- Application Number
- CN202411317529.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The existing catalysts have low selectivity in the dehydrolactization reaction of diethylene glycol, many side reactions, and are difficult to separate and purify, and lack the yield and selectivity of dioxycyclohexanone, mainly due to the dehydration and addition of raw materials. The by-product generation caused by hydrogen reaction.
By using a hydrophobic Cu/SiO2 catalyst, by mixing the Cu/SiO2 catalyst with a hydrophobic treatment agent and an organic solvent, oscillation and drying treatment, the acidic siloxane hydroxyl group on the catalyst surface is reduced, thereby reducing the dehydration and hydrogenation reaction activity, and a dehydration and hydrogenation reaction activity is prepared. A hydrophobic Cu/SiO2 catalyst with high selectivity and yield is used to improve catalytic performance by hydrogen reduction treatment in the dehydrolactification reaction of diethylene glycol.
It significantly reduces the formation of by-products 1,4-dioxane and ethanol, improves the selectivity and yield of dioxane, simplifies the catalyst preparation process, reduces production costs, and is suitable for industrial applications.
Smart Images

Figure SMS_1 
Figure HDA0005052643440000011
Abstract
Description
(I) Technical field
[0001] The present invention relates to a hydrophobic Cu / SiO 2 Catalyst, preparation thereof and application in dehydrogenation lactonization of diethylene glycol. (II) Background technology
[0002] Para-dioxanone (PDO) is an important organic chemical product with a wide range of uses. It can not only be used directly as a fragrance and food additive, but also as a synthetic monomer of polydioxanone (PPDO). Polydioxanone can be used to make housings for electronic components to protect circuit boards and electronic components and improve the high temperature resistance of products. In the construction industry, it can be used to make building materials such as heat insulation, sound insulation, fire resistance and waterproofing to improve the service life and quality of buildings. In the automotive industry, it can be used to make automotive parts such as hoods and doors to improve the durability and safety of cars. In the chemical industry, it can be used as a manufacturing material for chemical equipment such as corrosion-resistant containers, pipes and valves. In the medical industry, it can be used to make surgical sutures, drug sustained-release materials, orthopedic fixation materials and tissue repair materials.
[0003] There are three methods for synthesizing p-dioxanone: the first method is to use an organic synthesis method to synthesize p-dioxanone using ethylene glycol, metallic sodium and chloroacetic acid as raw materials. This method is cumbersome to operate, has a high production cost, and is not conducive to industrial production.
[0004] The second method is the catalytic carbonylation reaction: carbon monoxide, formaldehyde and 1,2-ethylene glycol or 1,3-dioxolane are used as raw materials for carbonyl addition to synthesize p-dioxanone. The catalysts used mainly include hydrogen fluoride, copper and silver carbonyl complexes.
[0005] The third method is the catalytic oxidative dehydrogenation cyclization method, which usually uses diethylene glycol as a reaction raw material for synthesis, and uses a transition metal such as copper, silver, platinum, zinc or a composite oxide catalyst of the above elements supported by an inert carrier such as alumina, activated carbon, and silicon dioxide. Diethylene glycol is first oxidatively dehydrogenated to convert into 2-(2-hydroxyethoxy)acetaldehyde, and its terminal aldehyde group then undergoes aldol condensation cyclization with the terminal hydroxyl group to generate 2-hydroxy-1,4-dioxane, and 2-hydroxy-1,4-dioxane is then dehydrogenated under the action of a catalyst to obtain p-dioxanone. For example, US Pat. 2,142,033 uses a copper-chromium composite oxygenate catalyst (chromium content ≤ 5wt%) to make diethylene glycol undergo gas phase dehydrogenation lactonization to obtain the target product, with a selectivity of 75.0%, but a yield of only 25%. US Pat.2,807,629 increases the selectivity of p-dioxanone to 94.0% and the yield to 84% by changing the chromium content in the copper-chromium catalyst. US Pat.3,119,840 also uses a copper-chromium catalyst. When the molar ratio of hydrogen to the raw material is 3 to 100, the yield of the target product p-dioxanone can reach up to 96%. Japanese Patent Laid-Open No. 58-99476 uses activated carbon, silicon dioxide or aluminum oxide to support platinum or palladium metal catalysts, and uses oxygen in the air as an oxidant to synthesize p-dioxanone through oxidative dehydrogenation self-condensation of diethylene glycol, but its selectivity can only reach up to 75%. Fetizon.M. et al. (Fetizon M, et al., Tetrahedron, 1975, 31, 171-176) used silver carbonate loaded on a diatomaceous earth carrier as a catalyst, refluxed diethylene glycol in benzene for 10 hours, and the yield of p-dioxanone could reach 95%. In CN 1739852A, Wang Yuzhong et al. used a coprecipitation method to load copper, zinc and other alkali metal or alkaline earth metal compounds on an inert carrier, and the mass percentage of the active component was 20-90%; the activity and selectivity of the catalyst were high, but the catalyst preparation process was relatively complicated, which was not conducive to industrial expansion of production. In short, the synthetic route of preparing p-dioxanone using diethylene glycol as a raw material has attracted much attention. Its main advantages are: the synthetic process is relatively simple, the reaction time is short, and the reaction conversion rate is high, but the disadvantages are also obvious: there are many side reactions (mainly dehydration reactions and over-hydrogenation reactions), which makes the selectivity of the target product poor and difficult to separate and purify.
[0006] It can be seen from the published literature that the main reasons for the low selectivity of dioxanone on the existing catalysts are: 1) the raw material diethylene glycol undergoes intramolecular dehydration reaction to generate 1,4-dioxane; 2) the raw material diethylene glycol undergoes hydrogenation and cracking to generate two by-products, ethanol and ethylene glycol. 2The catalyst is hydrophobically pretreated to eliminate the acidic silanol groups on the surface of the silica carrier, thereby significantly reducing the formation of 1,4-dioxane, a by-product of raw material dehydration, and at the same time reducing the hydrocracking activity of the catalyst, thereby reducing the selectivity of the by-products ethanol and ethylene glycol. (III) Summary of the invention
[0007] The first technical problem to be solved by the present invention is to provide a hydrophobic Cu / SiO 2 A method for preparing a catalyst.
[0008] The second technical problem to be solved by the present invention is to provide a hydrophobic Cu / SiO 2 catalyst.
[0009] The third technical problem of the present invention is to provide the hydrophobic Cu / SiO 2 Application of the catalyst in the dehydrogenation lactonization reaction of diethylene glycol.
[0010] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a hydrophobic Cu / SiO 2 A method for preparing a catalyst, comprising: 2 The catalyst is added to a mixed solution of a hydrophobic treatment agent and an organic solvent, and oscillated at 30-60°C for 1-12 hours. After the oscillation is completed, the mixture is filtered and washed with ethanol to remove excess hydrophobic treatment agent, and then dried in an oven at 40-200°C for 1-24 hours to obtain the hydrophobic Cu / SiO 2 Catalyst; the hydrophobic treatment agent is one or more of methoxytrimethylsilane, trimethylchlorosilane, dimethyldiacetoxysilane, and triisopropyloxysilane;
[0012] The Cu / SiO 2 The catalyst includes the following components in weight percentage:
[0013] Silica carrier 62.5%~99.5%
[0014] Copper oxide 0.5%~37.5%.
[0015] Preferably, the organic solvent is one or more of methanol, ethanol, isopropanol, acetylacetone, chloroform, tetrahydrofuran and N,N-dimethylformamide.
[0016] Preferably, the hydrophobic treatment agent and the organic solvent are mixed in a volume ratio of 1 to 99:100, more preferably in a volume ratio of 5 to 80:100.
[0017] Preferably, the Cu / SiO 2 The specific surface area of the catalyst is 150~700m 2 / g, the most probable pore diameter is 2-25nm, the pore volume is 0.2-1.5ml / g, the particle size is 4-40 mesh, and the particle strength: the average value is greater than 1Kg / particle.
[0018] The Cu / SiO 2 The catalyst may contain other ingredients which do not substantially affect its catalytic performance, such as small amounts of impurities introduced by using commercial silica supports, soluble copper salts, and the like.
[0019] The Cu / SiO 2 The catalyst is prepared by an impregnation method, that is, the metallic copper precursor is loaded onto the surface of the silica carrier by impregnation, and then the silica carrier loaded with the metallic copper precursor is calcined in air or an inert gas atmosphere to obtain Cu / SiO 2 Catalyst. The Cu / SiO 2 The specific steps for preparing the catalyst are as follows:
[0020] (1) immersing the silica support in a mixed solution of a copper precursor and a complexing agent, and shaking and immersing for 1 to 48 hours;
[0021] (2) drying the mixture obtained in step (1) so that the copper precursor is evenly loaded on the inner and outer surfaces of the silica carrier;
[0022] (3) placing the dried catalyst precursor obtained in step (2) into a muffle furnace and calcining it in air or inert gas atmosphere to obtain the Cu / SiO 2 catalyst.
[0023] In the above preparation method, the copper precursor can be a soluble copper salt such as copper nitrate, copper chloride, copper acetate, copper acetylacetonate, etc., the ligand is ammonia water, ethylenediamine, ethylenediaminetetraacetic acid or citric acid, and the molar ratio of the ligand to the copper precursor is 1 to 150:1, preferably 5 to 100:1. The drying treatment is carried out in a rotary evaporator and an oven, first drying for 1 to 24 hours at 10 to 60°C and 0.005 to 0.1 MPa in a rotary evaporator, and then drying for 1 to 48 hours at 50 to 150°C in an oven. The catalyst is calcined in a muffle furnace, heated to 150 to 800°C at a heating rate of 0.5 to 20°C / min and calcined for 1 to 10 hours, preferably heated to 300 to 600°C at a heating rate of 3 to 15°C / min and calcined for 2 to 6 hours.
[0024] In a second aspect, the present invention provides a hydrophobic Cu / SiO prepared according to the preparation method of the first aspect. 2catalyst.
[0025] In a third aspect, the present invention provides the hydrophobic Cu / SiO 2 Application of the catalyst in the dehydrogenation of diethylene glycol, the hydrophobic Cu / SiO 2 The catalyst is reduced with hydrogen before the dehydrolactonization reaction of diethylene glycol.
[0026] Preferably, the dehydrogenation lactonization reaction of diethylene glycol is continuously carried out in a fixed bed reactor. The hydrophobic catalyst is reduced by hydrogen-nitrogen mixed gas (1:1-9, v / v) before use, and the reduction conditions are: normal pressure, temperature 200-350°C, reduction time 1-12h, and the space velocity of hydrogen-nitrogen mixed gas is 200-1600h -1 .
[0027] The reaction conditions of the dehydrogenation lactonization reaction of diethylene glycol are as follows: temperature of 220-280°C, reaction pressure of 0.1-1 MPa, liquid space velocity of the raw material of 0.2-1.5 h -1 , carrier gas hydrogen space velocity is 100~800h -1 Under these conditions, the selectivity and yield of the dehydrogenation lactonization product of the catalyst for dioxanone are high, and the main by-products of the reaction, such as 1,4-dioxane, ethanol, and ethylene glycol, are 2 The catalysts showed a significant decrease after being treated with hydrophobicity.
[0028] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0029] (1) The byproducts of the dehydrogenation of diethylene glycol are mainly produced by the surface silanol acid sites on the catalyst support surface, and the hydrophobic reagent combines with the silanol to reduce the Cu / SiO 2 The number of silanol acid sites on the catalyst surface is increased to avoid the formation of dehydration by-products; at the same time, the removal of silanol on the catalyst surface also reduces the Cu / SiO 2 The hydrogenation capacity of the catalyst reduces the degree of hydrogenolysis of the feedstock, thereby further improving the selectivity / yield of the target product.
[0030] (2) The hydrophobic Cu / SiO 2 The preparation method of the catalyst is simple and reliable, and the production cost is low. At the same time, when it is applied to the dehydrogenation lactonization reaction of diethylene glycol, a fixed bed continuous reaction process is adopted, so it is suitable for industrial application. (IV) Description of the drawings
[0031] Figure 1This is a schematic diagram of the reaction device for the continuous catalytic synthesis of p-dioxanone by fixed-bed diethylene glycol: 1-hydrogen bottle, 2-nitrogen bottle, 3-raw material bottle, 4-high-pressure constant flow pump, 5-three-way valve, 6-pressure reducing valve, 7-stop valve, 8-mass flow meter, 9-check valve, 10-reaction tube, 11-reaction furnace, 12-condenser, 13 and 14-condensate inlet and outlet, 15-filter, 16-back pressure valve, 17-product collection tank, 18-catalyst bed. (V) Specific implementation methods
[0032] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto.
[0033] SiO used in the examples 2 The carrier is granular, with a particle diameter of 4 to 40 meshes and a specific surface area of 310 m 2 / g, average pore diameter 9.8nm, pore volume 1.0mL / g.
[0034] The normal temperature in the examples refers to 25°C.
[0035] Example 1
[0036] Weigh 0.9505 g of copper nitrate trihydrate, add it to 20 mL of ammonia solution and wait for it to completely dissolve, then add 2 g of silica carrier, and shake at room temperature for 2 h. Evaporate the solvent under reduced pressure at 60 ° C, dry the evaporated catalyst precursor in a forced air drying oven at 110 ° C for 4 h, and then calcine it in a muffle furnace at 500 ° C for 4 h to obtain Cu / SiO 2 The weight content of CuO in the catalyst is 15.6%, and the rest is silica gel carrier. 2 The catalyst was added to a mixed solution of 10 mL of ethanol and 2 mL of methoxytrimethylsilane, and shaken at room temperature for 2 h. After the shaking was completed, it was filtered and repeatedly washed with ethanol to remove excess methoxytrimethylsilane, and then baked in an oven at 110° C. for 4 h to obtain catalyst A.
[0037] Example 2
[0038] The preparation method of catalyst B is the same as that of Example 1, except that a mixed solution of 10 mL of ethanol and 2 mL of methoxytrimethylsilane is added and shaken at room temperature for 6 h. After the shaking is completed, it is filtered and repeatedly washed with ethanol to remove excess methoxytrimethylsilane, and then baked in an oven at 110° C. for 4 h to obtain catalyst B.
[0039] Example 3
[0040] The preparation method of catalyst C is the same as that of Example 1, except that a mixed solution of 10 ml of ethanol and 2 ml of methoxytrimethylsilane is added and shaken at room temperature for 12 h. After the shaking is completed, it is filtered and repeatedly washed with ethanol to remove excess methoxytrimethylsilane, and then baked in an oven at 110° C. for 4 h to obtain catalyst C.
[0041] Example 4
[0042] The preparation method of catalyst D is the same as that of Example 1, except that the mixture is added to a mixed solution of 10 ml of ethanol and 2 ml of methoxytrimethylsilane and shaken at 40°C for 6 h. After the shaking is completed, the mixture is filtered and repeatedly washed with ethanol to remove excess methoxytrimethylsilane, and then baked in an oven at 110°C for 4 h to obtain catalyst D.
[0043] Comparative Example 1
[0044] The preparation method of catalyst E is the same as that of Example 1, but the calcined catalyst is not subjected to hydrophobic treatment.
[0045] Comparative Example 2
[0046] Weigh 2g SiO 2 The carrier was placed in a mixed solution of 10 ml ethanol and 2 ml methoxytrimethylsilane, shaken at room temperature for 6 h, filtered after shaking, and repeatedly washed with ethanol to remove excess methoxytrimethylsilane, and then dried in an oven at 110 ° C for 4 h to obtain a hydrophobic SiO 2 Carrier. Weigh 0.9505g of copper nitrate trihydrate and add it to 20mL of ammonia solution until it is completely dissolved, then add 2g of hydrophobic SiO 2 The catalyst precursor was placed in a forced air drying oven at 110°C for 4 hours and then calcined in a muffle furnace at 500°C for 4 hours to obtain catalyst F, which had a CuO weight content of 15.6% and the rest was silica gel carrier.
[0047] Example 5
[0048] Reaction device such as Figure 1 As shown, the catalysts A, B, C, D, E and F prepared in the above examples and comparative examples were respectively loaded into the reaction tube of the fixed bed reactor, and the catalysts were first reduced under the following conditions: 320°C, normal pressure, hydrogen-nitrogen mixed gas (1:9, v / v) with a space velocity of 900 h -1 , the reduction time is 4h, and then the diethylene glycol dehydrogenation lactonization reaction is carried out. The reaction conditions are set as: 260℃, 0.1MPa, LHSV=0.5h -1 , carrier gas hydrogen space velocity is 480h -1 ; The results are shown in Table 1.
[0049] Table 1 Catalytic performance of different catalysts in the continuous catalytic synthesis of p-dioxanone in a fixed bed of diethylene glycol
[0050]
[0051] [a] DEG-diethylene glycol; [b] PDO - para-dioxanone; [c] Diox-1,4-dioxane; [d] ET-ethanol; [e] EG-ethylene glycol; [f] 2-(2-Hydroxyethoxy)acetaldehyde.
Claims
1. A method for preparing a hydrophobic Cu / SiO2 catalyst, characterized in that: The preparation method comprises: adding a Cu / SiO2 catalyst to a mixed solution of a hydrophobic treatment agent and an organic solvent, oscillating at 30-60°C for 1-12 hours, filtering after the oscillation is completed, washing with ethanol to remove excess hydrophobic treatment agent, and then drying in an oven at 40-200°C for 1-24 hours to obtain the hydrophobic Cu / SiO2 catalyst; the hydrophobic treatment agent is one or more of methoxytrimethylsilane, trimethylchlorosilane, dimethyldiacetoxysilane, and triisopropyloxysilane; The Cu / SiO2 catalyst comprises the following components in weight percentage: Silica carrier 62.5%~99.5% Copper oxide 0.5%~37.5%.
2. The preparation method according to claim 1, characterized in that: The organic solvent is one or more of methanol, ethanol, isopropanol, acetylacetone, chloroform, tetrahydrofuran and N,N-dimethylformamide.
3. The preparation method according to claim 1, characterized in that: The hydrophobic treatment agent and the organic solvent are mixed in a volume ratio of 1 to 99:100, preferably in a volume ratio of 5 to 80:
100.
4. The preparation method according to claim 1, characterized in that: The specific surface area of the Cu / SiO2 catalyst is 150 to 700 m 2 / g, the most probable pore diameter is 2-25nm, the pore volume is 0.2-1.5ml / g, the particle size is 4-40 mesh, and the particle strength: the average value is greater than 1Kg / particle.
5. The preparation method according to claim 1, characterized in that: The preparation steps of the Cu / SiO2 catalyst are as follows: (1) immersing the silica support in a mixed solution of a copper precursor and a complexing agent, and shaking and immersing for 1 to 48 hours; (2) drying the mixture obtained in step (1) so that the copper precursor is evenly loaded on the inner and outer surfaces of the silica carrier; (3) placing the dried catalyst precursor obtained in step (2) into a muffle furnace and calcining it in air or inert gas atmosphere to obtain the Cu / SiO2 catalyst.
6. The preparation method according to claim 5, characterized in that: The copper precursor is a soluble copper salt, the ligand is ammonia water, ethylenediamine, ethylenediaminetetraacetic acid or citric acid, and the molar ratio of the ligand to the copper precursor is 1 to 150:1; the drying treatment is carried out in a rotary evaporator and an oven, first drying for 1 to 24 hours at 10 to 60°C and 0.005 to 0.1 MPa in the rotary evaporator, and then drying for 1 to 48 hours at 50 to 150°C in the oven; the calcination is carried out in a muffle furnace, heating to 150 to 800°C at a heating rate of 0.5 to 20°C / min and calcining for 1 to 10 hours, preferably heating to 300 to 600°C at a heating rate of 3 to 15°C / min and calcining for 2 to 6 hours.
7. A hydrophobic Cu / SiO2 catalyst prepared according to the preparation method according to any one of claims 1 to 6.
8. Use of the hydrophobic Cu / SiO2 catalyst as claimed in claim 7 in the dehydrogenation lactonization reaction of diethylene glycol, wherein the hydrophobic Cu / SiO2 catalyst is first reduced with hydrogen before the dehydrogenation lactonization reaction of diethylene glycol.
9. The use according to claim 8, characterized in that: The diethylene glycol dehydrogenation lactonization reaction is continuously carried out in a fixed bed reactor.
10. The use according to claim 9, characterized in that: The hydrophobic Cu / SiO2 catalyst is reduced by hydrogen-nitrogen mixed gas before use. The reduction conditions are: normal pressure, temperature 200-350°C, reduction time 1-12h, and space velocity of hydrogen-nitrogen mixed gas 200-1600h -1 ; The reaction conditions of the dehydrogenation of diethylene glycol are as follows: temperature of 220-280°C, reaction pressure of 0.1-1 MPa, liquid space velocity of the raw material of 0.2-1.5 h -1 , carrier gas hydrogen space velocity is 100~800h -1 .
Citation Information
Patent Citations
Supported copper-based catalyst preparation method and applications of supported copper-based catalyst in synthesis of ethylene glycol
CN110694672A
Silanization modified copper-silicon catalyst and preparation method and application thereof
CN111389460A
Preparation method and application of supported catalyst for catalyzing hydrogenation of dimethyl oxalate
CN111774050A
Catalyst for preparing p-dioxanone and method for preparing p-dioxanone
CN112473675A
Hydrophobic catalyst for synthesizing methanol through carbon dioxide hydrogenation and preparation method and application of hydrophobic catalyst
CN112588320A